Environmentally friendly water-based paint with long-term formaldehyde removal and preparation method thereof

By using aqueous silicone modified acrylic resin, activated bentonite, yttrium manganese borate @Co/Bi-MOFs and other ingredients in the coating, a long-acting formaldehyde removal water-based coating with high impact resistance and excellent salt spray resistance is prepared. The problem of poor formaldehyde removal effect of existing paints has been solved, and the efficient and long-term formaldehyde removal effect has been achieved, which has significantly improved indoor air quality and human health and safety.

CN118772715BActive Publication Date: 2024-11-15GUANG DONG KA BAI LI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411281013.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

Most paints on the existing market have poor formaldehyde removal effect and are difficult to achieve long-term aldehyde removal, which cannot effectively improve indoor air quality and protect human health.

Method used

Using aqueous silicone modified acrylic resin, activated bentonite and yttrium manganese borate @Co/Bi-MOFs as main components, a long-term formaldehyde-removing environmentally friendly water-based coating was prepared through a specific preparation method, combining pigments and additives to form It is a coating with impact resistance, high surface hardness and excellent salt spray resistance, and improves the aldehyde removal effect through sintering treatment.

Benefits of technology

It has achieved efficient and long-term formaldehyde removal effect. The formaldehyde removal rate of the paint reaches 95.3% within 24 hours, and remains a high removal rate after 5 days, significantly improving indoor air quality and human health and safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of water-based coatings, and in particular to an environmentally friendly water-based coating for long-term formaldehyde removal and a preparation method thereof, wherein the environmentally friendly water-based coating components are calculated by weight, including: 75-95 parts of water-based organosilicon-modified acrylic resin, 11-22 parts of activated bentonite, 8-16 parts of aldehyde removal enhancers, 3.3-4.6 parts of pigments, 0.4-0.8 parts of wetting and dispersing aids, 0.5-1 parts of defoamers, 0.2-0.6 parts of leveling agents, 0.05-0.1 parts of film-forming aids and 26-42 parts of deionized water. The present invention prepares an environmentally friendly water-based coating, which uses water-based organosilicon-modified acrylic resin as the main raw material, activated bentonite as the main filler, and the aldehyde removal enhancer is used as a filler and a reinforcing agent at the same time, and pigments and auxiliary agents are also added in addition, and the prepared water-based coating is not only strong in impact resistance, large in surface hardness, and excellent in salt spray resistance, but also has the effect of long-term formaldehyde removal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of water-based coatings, and in particular to an environmentally friendly water-based coating with long-term formaldehyde removal and a preparation method thereof. Background Art

[0002] At present, architectural decorative paints, especially the decorative paints for the interior walls of houses, mainly play the role of beautifying indoor and outdoor, making people feel comfortable and warm, and the most commonly used interior decorative paint is latex paint, which is an emulsion paint with latex as a diluent. It is a kind of paint that is easy to apply, safe, washable, and breathable. It can be mixed with different colors according to different color schemes, which plays the role of beautification and wall protection. However, as people's requirements for environmental protection are getting higher and higher, the simple decorative effect can no longer meet people's needs, and the requirements for health are getting higher and higher.

[0003] Since formaldehyde-containing adhesives and coatings are used in the production process of furniture and building materials, a large amount of free formaldehyde will be generated during indoor use, causing a decline in indoor air quality and possibly affecting human health. Formaldehyde inhalation through the respiratory tract can cause dizziness, headaches, nausea and other symptoms, and has a certain irritating effect on the eyes and nose. In severe cases, it can cause asthma, confusion, vomiting and bronchitis. Therefore, it is very important to remove indoor formaldehyde. Compared with the traditional purchase of professional formaldehyde removal equipment, the use of formaldehyde-removing wall paint is cheaper and more economical. Therefore, the formaldehyde removal function of wall paint has become a popular method.

[0004] However, most of the paints on the market currently remove formaldehyde through physical adsorption, and the effect of removing formaldehyde is relatively poor, and it is also difficult to achieve a long-term formaldehyde removal effect. Therefore, it is more important to have a water-based paint that can remove formaldehyde for a long time. Summary of the invention

[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide an environmentally friendly water-based paint with long-term formaldehyde removal and a preparation method thereof.

[0006] The purpose of the present invention is achieved by the following technical solutions:

[0007] In a first aspect, the present invention provides an environmentally friendly water-based paint with a long-term formaldehyde removal, the components of which are calculated by weight and include:

[0008] 75-95 parts of water-based organosilicon-modified acrylic resin, 11-22 parts of activated bentonite, 8-16 parts of formaldehyde removal enhancer, 3.3-4.6 parts of pigment, 0.4-0.8 parts of wetting and dispersing aid, 0.5-1 parts of defoaming agent, 0.2-0.6 parts of leveling agent, 0.05-0.1 parts of film-forming aid and 26-42 parts of deionized water.

[0009] Preferably, the brand of the water-based silicone-modified acrylic resin is one of AD-1680 (Dongguan Aide Synthetic Materials Co., Ltd.), AC-749RG (Jili Water-based New Materials Technology Co., Ltd.), and J-611 (Jining Fangyu Chemical Co., Ltd.); more preferably J-611 (Jining Fangyu Chemical Co., Ltd.), which can be dried at room temperature.

[0010] Preferably, the activated bentonite is bentonite activated by a silane coupling agent.

[0011] Preferably, the preparation process of the activated bentonite comprises:

[0012] Bentonite, KH-560 coupling agent and anhydrous ethanol are mixed, and after heat treatment at 50-60°C for 8-12 hours, the solid is collected by filtration, washed and dried to obtain activated bentonite; wherein the particle size of the bentonite is 50±5μm, and the mass volume ratio of bentonite, KH-560 and anhydrous ethanol is 1g:(0.3-0.5)g:(10-20)mL.

[0013] Preferably, the formaldehyde removal enhancer is yttrium manganese borate @Co / Bi-MOFs, and the preparation method comprises:

[0014] S1. Preparation of Co / Bi-MOFs:

[0015] Weigh cobalt chloride (CoCl 2 ) and bismuth chloride (BiCl 3 ) was dissolved in N-methylpyrrolidone (NMP), and then biphenyl-3,3',5,5'-tetracarboxylic acid (H 4 BPTC), stirred evenly at room temperature, then poured into a reactor, the reactor was sealed and placed in an oven for heat preservation treatment, after the treatment, the precipitate was collected by filtration, washed with alcohol and dried to obtain Co / Bi-MOFs;

[0016] S2. Preparation of precursor:

[0017] Yttrium chloride (YCl 3 ), manganese chloride (MnCl 2 ) and boric acid (H 3 BO 3 ) is added into deionized water, stirred at 50-60°C until dissolved, Co / Bi-MOFs is added, ultrasonically dispersed evenly, and then the pH is adjusted to 9-10, the reaction solution is poured into a reactor, the reactor is sealed and placed in an oven for heat preservation treatment, after the treatment is completed, the precipitate is collected by filtration, washed with water and dried to obtain a precursor material;

[0018] S3, sintering treatment:

[0019] The precursor material is placed in a muffle furnace for sintering, and after the furnace is cooled, yttrium manganese borate@Co / Bi-MOFs is obtained.

[0020] Preferably, in S1, the mass volume ratio of cobalt chloride, bismuth chloride, biphenyl-3,3',5,5'-tetracarboxylic acid and N-methylpyrrolidone is (0.13-0.26) g:(0.32-0.64) g:(0.38-0.76) g:(15-20) mL.

[0021] Preferably, in S1, the temperature in the oven is 130-180°C, and the treatment time is 18-36h.

[0022] Preferably, in S2, the mass volume ratio of Co / Bi-MOFs, yttrium chloride, manganese chloride, boric acid and deionized water is 1 g:(0.15-0.3) g:(0.1-0.2) g:(0.1-0.3) g:(20-30) mL.

[0023] Preferably, in S2, the temperature in the oven is 200-250°C, and the treatment time is 15-30h.

[0024] Preferably, in S3, the sintering temperature is 350-450° C., and the sintering time is 2-4 hours.

[0025] Preferably, the pigment is one or a mixture of anatase titanium dioxide, pigment red, pigment yellow, pigment blue, pigment green, and pigment black.

[0026] Preferably, the wetting and dispersing aid is one of BYK-161, BYK-163, BYK-180, BYK-190 and BYK-199, or a mixture of more thereof.

[0027] Preferably, the defoaming agent is one of BYK-028, BYK-022, BYK-024 and BYK-094, or a mixture of more thereof.

[0028] Preferably, the leveling agent is one of TEGO-270, TEGO-410, TEGO-450, and TEGO-482, or a mixture of more thereof.

[0029] Preferably, the film-forming aid is one or a mixture of hexylene glycol, propylene glycol, dodecyl alcohol ester, propylene glycol ethyl ether, and propylene glycol butyl ether.

[0030] In a second aspect, the present invention provides a method for preparing an environmentally friendly water-based coating with a long-term formaldehyde removal, comprising the following steps:

[0031] Step 1, weighing water-based organosilicon-modified acrylic resin, activated bentonite, formaldehyde removal enhancer, pigment, wetting and dispersing aid, defoamer, leveling agent, film-forming aid and deionized water according to weight proportion, and mixing them into a mixer;

[0032] Step 2, set the stirring speed of the mixer to 200-400 r / min, and after stirring for 1-2 hours, obtain the desired water-based coating.

[0033] The beneficial effects of the present invention are:

[0034] 1. The present invention prepares an environmentally friendly water-based paint, which uses water-based silicone-modified acrylic resin as the main raw material, activated bentonite as the main filler, and a formaldehyde-removing enhancer as both a filler and a enhancer. In addition, pigments and additives are added. The prepared water-based paint not only has strong impact resistance, high surface hardness, and excellent salt spray resistance, but also has a long-term formaldehyde removal effect.

[0035] 2. Water-based silicone-modified acrylic resin has excellent mechanical properties, water resistance and weather resistance; activated bentonite has good formaldehyde absorption and is more compatible with coatings after activation; the formaldehyde removal enhancer is yttrium manganese borate @Co / Bi-MOFs, which not only has certain formaldehyde absorption, but also has excellent formaldehyde removal effect, and is the main component for formaldehyde removal in coatings.

[0036] 3. In the preparation of yttrium manganese borate @ Co / Bi-MOFs, bimetallic Co and Bi and chelating agent H 4 Metal organic frameworks (MOFs), namely Co / Bi-MOFs, are prepared by BPTC reaction. Then, bimetallic composite borates, namely yttrium manganese borate, are prepared on the MOFs material by in situ synthesis, and finally yttrium manganese borate@Co / Bi-MOFs is obtained.

[0037] 4. The present invention has been found through testing that, compared with the loading of yttrium borate or manganese borate alone on MOFs materials, the loading of yttrium manganese borate composite salt has a better formaldehyde removal effect, indicating that there is a certain synergistic effect between yttrium and manganese elements, making the formed boric acid composite salt have a stronger catalytic removal effect on formaldehyde.

[0038] 5. The yttrium manganese borate @ Co / Bi-MOFs prepared by the present invention is sintered at 350-450° C. in the subsequent synthesis process. Although the product obtained without sintering also has the effect of removing formaldehyde, after sintering, the crystal structure and porosity of the material are better improved, and the activity is further enhanced, so the formaldehyde removal effect is better and longer-lasting. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.

[0040] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0041] The present invention will be further described below in conjunction with the following examples.

[0042] Example 1

[0043] A long-term formaldehyde-removing environmentally friendly water-based paint, the components are calculated by weight and include:

[0044] 85 parts of water-based silicone modified acrylic resin, 16 parts of activated bentonite, 12 parts of formaldehyde removal enhancer, 3.9 parts of pigment, 0.6 parts of wetting and dispersing aid, 0.7 parts of defoaming agent, 0.4 parts of leveling agent, 0.08 parts of film-forming aid and 34 parts of deionized water.

[0045] The brand of water-based silicone-modified acrylic resin is J-611 (Jining Fangyu Chemical Co., Ltd.), which can be dried at room temperature; the pigment is anatase titanium dioxide R-666 and pigment blue 60 in a mass ratio of 1:0.2; the wetting and dispersing additive is BYK-161; the defoaming agent is BYK-028; the leveling agent is TEGO-270; and the film-forming additive is dodecanol ester.

[0046] The preparation process of activated bentonite includes:

[0047] Bentonite, KH-560 coupling agent and anhydrous ethanol were mixed, and after heat treatment at 55°C for 10 hours, the solid was collected by filtration, washed and dried to obtain activated bentonite; wherein the particle size of the bentonite was 50±5μm, and the mass volume ratio of bentonite, KH-560 and anhydrous ethanol was 1g:0.4g:15mL.

[0048] Wherein, the formaldehyde removal enhancer is yttrium manganese borate @Co / Bi-MOFs, and the preparation method includes:

[0049] S1. Preparation of Co / Bi-MOFs:

[0050] Weigh cobalt chloride (CoCl 2 ) and bismuth chloride (BiCl 3 ) was dissolved in N-methylpyrrolidone (NMP), and then biphenyl-3,3',5,5'-tetracarboxylic acid (H 4 BPTC), cobalt chloride, bismuth chloride, biphenyl-3,3',5,5'-tetracarboxylic acid and N-methylpyrrolidone in a mass volume ratio of 0.19 g: 0.48 g: 0.57 g: 20 mL, stirred at room temperature for 1 hour, then poured into a reactor, the reactor was sealed and placed in an oven at 150°C, and heat-treated for 27 hours. After the treatment, the precipitate was collected by filtration, washed with alcohol and dried to obtain Co / Bi-MOFs;

[0051] S2. Preparation of YMnB@Co / Bi-MOFs:

[0052] Yttrium chloride (YCl 3 ), manganese chloride (MnCl 2 ) and boric acid (H 3 BO 3 ) was added into deionized water, stirred at 55°C until dissolved, and then Co / Bi-MOFs was added. The mass volume ratio of Co / Bi-MOFs, yttrium chloride, manganese chloride, boric acid and deionized water was 1g:0.23g:0.15g:0.2g:25mL. Ultrasonic dispersion was performed uniformly, and then the pH was adjusted to 9-10. The reaction solution was poured into a reactor, which was sealed and placed in an oven at 230°C for 24h of heat preservation. After the treatment, the precipitate was collected by filtration, washed with water and dried to obtain a precursor material;

[0053] S3, sintering treatment:

[0054] The precursor material is placed in a muffle furnace for sintering at a temperature of 400°C for 3 hours. After cooling in the furnace, yttrium manganese borate@Co / Bi-MOFs is obtained.

[0055] The method for preparing the above-mentioned environmentally friendly water-based paint with long-term formaldehyde removal comprises the following steps:

[0056] Step 1, weighing water-based organosilicon-modified acrylic resin, activated bentonite, formaldehyde removal enhancer, pigment, wetting and dispersing aid, defoamer, leveling agent, film-forming aid and deionized water according to weight proportion, and mixing them into a mixer;

[0057] Step 2, set the stirring speed of the mixer to 300 r / min, and after stirring for 1 hour, obtain the desired water-based coating.

[0058] Example 2

[0059] A long-term formaldehyde-removing environmentally friendly water-based paint, the components are calculated by weight and include:

[0060] 75 parts of water-based silicone modified acrylic resin, 11 parts of activated bentonite, 8 parts of formaldehyde removal enhancer, 3.3 parts of pigment, 0.4 parts of wetting and dispersing aid, 0.5 parts of defoamer, 0.2 parts of leveling agent, 0.05 parts of film-forming aid and 26 parts of deionized water.

[0061] The brand of water-based silicone-modified acrylic resin is AD-1680 (Dongguan Aide Synthetic Materials Co., Ltd.); the pigment is anatase titanium dioxide and pigment red in a mass ratio of 1:0.3; the wetting and dispersing additive is BYK-163; the defoaming agent is BYK-022; the leveling agent is TEGO-410; and the film-forming additive is hexanediol.

[0062] The preparation process of activated bentonite includes:

[0063] Bentonite, KH-560 coupling agent and anhydrous ethanol were mixed, and after heat treatment at 50°C for 8 hours, the solid was collected by filtration, washed and dried to obtain activated bentonite; wherein the particle size of the bentonite was 50±5μm, and the mass volume ratio of bentonite, KH-560 and anhydrous ethanol was 1g:0.3g:10mL.

[0064] Wherein, the formaldehyde removal enhancer is yttrium manganese borate @Co / Bi-MOFs, and the preparation method includes:

[0065] S1. Preparation of Co / Bi-MOFs:

[0066] Weigh cobalt chloride and bismuth chloride and dissolve them in N-methylpyrrolidone, then add biphenyl-3,3',5,5'-tetracarboxylic acid, the mass volume ratio of cobalt chloride, bismuth chloride, biphenyl-3,3',5,5'-tetracarboxylic acid and N-methylpyrrolidone is 0.13g:0.32g:0.38g:15mL, stir at room temperature for 0.5h, then pour into a reactor, seal the reactor and place it in an oven at 130°C, keep warm for 36h, after the treatment, filter and collect the precipitate, wash with alcohol and dry to obtain Co / Bi-MOFs;

[0067] S2. Preparation of YMnB@Co / Bi-MOFs:

[0068] Yttrium chloride, manganese chloride and boric acid are added to deionized water, stirred at 50°C until dissolved, and then Co / Bi-MOFs are added. The mass volume ratio of Co / Bi-MOFs, yttrium chloride, manganese chloride, boric acid and deionized water is 1g:0.15g:0.1g:0.1g:20mL. Ultrasonic dispersion is performed uniformly, and then the pH is adjusted to 9-10. The reaction solution is poured into a reactor, and the reactor is sealed and placed in an oven at 200°C for insulation treatment for 15h. After the treatment, the precipitate is collected by filtration, washed with water and dried to obtain a precursor material;

[0069] S3, sintering treatment:

[0070] The precursor material is placed in a muffle furnace for sintering at a temperature of 350°C for 4 hours. After cooling in the furnace, yttrium manganese borate@Co / Bi-MOFs is obtained.

[0071] The method for preparing the above-mentioned environmentally friendly water-based paint with long-term formaldehyde removal comprises the following steps:

[0072] Step 1, weighing water-based organosilicon-modified acrylic resin, activated bentonite, formaldehyde removal enhancer, pigment, wetting and dispersing aid, defoamer, leveling agent, film-forming aid and deionized water according to weight proportion, and mixing them into a mixer;

[0073] Step 2, set the stirring speed of the mixer to 200 r / min, and after stirring for 2 hours, obtain the desired water-based coating.

[0074] Example 3

[0075] A long-term formaldehyde-removing environmentally friendly water-based paint, the components are calculated by weight and include:

[0076] 95 parts of water-based silicone modified acrylic resin, 22 parts of activated bentonite, 16 parts of formaldehyde removal enhancer, 4.6 parts of pigment, 0.8 parts of wetting and dispersing aid, 1 part of defoamer, 0.6 parts of leveling agent, 0.1 parts of film-forming aid and 42 parts of deionized water.

[0077] The brand of water-based silicone-modified acrylic resin is AC-749RG (Jili Water-based New Material Technology Co., Ltd.); the pigment is anatase titanium dioxide and pigment green in a mass ratio of 1:0.1; the wetting and dispersing additive is BYK-180; the defoaming agent is BYK-094; the leveling agent is TEGO-482; and the film-forming additive is propylene glycol ethyl ether.

[0078] The preparation process of activated bentonite includes:

[0079] Bentonite, KH-560 coupling agent and anhydrous ethanol are mixed, and after heat treatment at 60°C for 12 hours, the solid is collected by filtration, washed and dried to obtain activated bentonite; wherein the particle size of the bentonite is 50±5μm, and the mass volume ratio of bentonite, KH-560 and anhydrous ethanol is 1g:0.5g:20mL.

[0080] Wherein, the formaldehyde removal enhancer is yttrium manganese borate @Co / Bi-MOFs, and the preparation method includes:

[0081] S1. Preparation of Co / Bi-MOFs:

[0082] Weigh cobalt chloride and bismuth chloride and dissolve them in N-methylpyrrolidone, then add biphenyl-3,3',5,5'-tetracarboxylic acid, the mass volume ratio of cobalt chloride, bismuth chloride, biphenyl-3,3',5,5'-tetracarboxylic acid and N-methylpyrrolidone is 0.26g:0.64g:0.76g:20mL, stir at room temperature for 1.5h, then pour into a reactor, seal the reactor and place it in an oven at 180°C, keep warm for 18h, after the treatment, filter and collect the precipitate, wash with alcohol and dry to obtain Co / Bi-MOFs;

[0083] S2. Preparation of YMnB@Co / Bi-MOFs:

[0084] Yttrium chloride, manganese chloride and boric acid are added to deionized water, stirred at 60°C until dissolved, and then Co / Bi-MOFs are added, the mass volume ratio of Co / Bi-MOFs, yttrium chloride, manganese chloride, boric acid and deionized water is 1g:0.3g:0.2g:0.3g:30mL, ultrasonically dispersed evenly, and then the pH is adjusted to 9-10, and the reaction solution is poured into a reactor, the reactor is sealed and placed in an oven at 250°C, and heat-treated for 30h. After the treatment, the precipitate is collected by filtration, washed with water and dried to obtain a precursor material;

[0085] S3, sintering treatment:

[0086] The precursor material is placed in a muffle furnace for sintering at a temperature of 450°C and a sintering time of 2 hours. After cooling in the furnace, yttrium manganese borate@Co / Bi-MOFs is obtained.

[0087] The method for preparing the above-mentioned environmentally friendly water-based paint with long-term formaldehyde removal comprises the following steps:

[0088] Step 1, weighing water-based organosilicon-modified acrylic resin, activated bentonite, formaldehyde removal enhancer, pigment, wetting and dispersing aid, defoamer, leveling agent, film-forming aid and deionized water according to weight proportion, and mixing them into a mixer;

[0089] Step 2, set the stirring speed of the mixer to 400 r / min, and after stirring for 1 hour, obtain the desired water-based coating.

[0090] Comparative Example 1

[0091] An environmentally friendly water-based paint, which differs from Example 1 only in that the formaldehyde removal enhancer in the composition is Co / Bi-MOFs (prepared in the same way as S1 in Example 1), and the remaining components and steps are the same as those in Example 1.

[0092] Comparative Example 2

[0093] An environmentally friendly water-based paint, which differs from Example 1 only in that the formaldehyde removal enhancer in the composition is yttrium borate@Co / Bi-MOFs, and the remaining components and steps are the same as those in Example 1.

[0094] The preparation process of Yttrium borate@Co / Bi-MOFs includes:

[0095] S1. Preparation of Co / Bi-MOFs, the same as in Example 1;

[0096] S2, yttrium chloride (YCl 3 ) and boric acid (H 3 BO 3 ) was added into deionized water, stirred at 55°C until dissolved, and Co / Bi-MOFs was added, the mass volume ratio of Co / Bi-MOFs, yttrium chloride, boric acid and deionized water was 1g:0.38g:0.2g:25mL, and ultrasonic dispersion was uniform, and then the pH was adjusted to 9-10, and the reaction solution was poured into a reactor, and the reactor was sealed and placed in an oven at 230°C for insulation treatment for 24h. After the treatment, the precipitate was collected by filtration, washed with water and dried to obtain a precursor material;

[0097] S3: sintering treatment is the same as in Example 1.

[0098] Comparative Example 3

[0099] An environmentally friendly water-based paint, which differs from Example 1 only in that the formaldehyde removal enhancer in the composition is manganese borate @Co / Bi-MOFs, and the remaining components and steps are the same as Example 1.

[0100] The preparation process of manganese borate@Co / Bi-MOFs includes:

[0101] S1. Preparation of Co / Bi-MOFs, the same as in Example 1;

[0102] S2, manganese chloride (MnCl 2 ) and boric acid (H 3 BO 3) was added into deionized water, stirred at 55°C until dissolved, and then Co / Bi-MOFs was added, the mass volume ratio of Co / Bi-MOFs, manganese chloride, boric acid and deionized water was 1g:0.38g:0.2g:25mL, and ultrasonic dispersion was uniform, and then the pH was adjusted to 9-10, and the reaction solution was poured into a reactor, and the reactor was sealed and placed in an oven at 230°C for insulation treatment for 24h. After the treatment, the precipitate was collected by filtration, washed with water and dried to obtain the precursor material;

[0103] S3: sintering treatment is the same as in Example 1.

[0104] Experimental testing

[0105] First, the basic performance test was carried out. The coatings prepared in Example 1 and Comparative Examples 1-3 were coated on steel plates and dried at room temperature for 7 days before testing their impact resistance, surface hardness and salt spray resistance. The impact resistance test referenced GB / T1732-1993, the surface hardness test referenced GB / T 6739-2006, and the salt spray resistance test referenced GB / T1771-1991.

[0106] The second is the formaldehyde removal effect test, which refers to JC / T 1074-2008 "Purification Performance of Indoor Air Purification Function Coating Materials". Specifically, the coating is applied on the inner bottom surface of a closed test box (125cm×80cm×100cm) with a coating thickness of (2±0.02) mm, dried at room temperature for 7 days, and then a formaldehyde concentration of 10mg / m 3 , under the conditions of temperature (20±2)℃ and relative humidity (50±10)%, use 30W fluorescent lamp for continuous irradiation treatment, and calculate the formaldehyde removal rate by detecting the formaldehyde content at different times; and the long-term formaldehyde removal test is to add formaldehyde concentration to 20mg / m on time every day 3 , continue for 4 days, detect the formaldehyde content after the 5th day, and calculate the formaldehyde removal rate as a judgment of long-term effectiveness.

[0107] The test results are shown in the table below:

[0108] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Impact resistance 65cm 45cm 55cm 60cm Surface hardness 4H 2H 3H 4H Salt spray resistance Almost no foaming Foaming rate 20% Foaming rate 5% Foaming rate 5% 12h formaldehyde removal rate 78.1% 57.5% 67.7% 69.8% 24h formaldehyde removal rate 95.3% 84.6% 91.2% 92.4% 5d formaldehyde removal rate 81.8% 63.8% 72.5% 76.1%

[0109] It can be seen from the above table that compared with comparative examples 1-3, the water-based coating prepared in Example 1 of the present invention not only has better impact resistance and greater surface hardness, but also has better salt spray resistance. In addition, the formaldehyde removal rate of the water-based coating prepared in Example 1 of the present invention reached 95.3% in 24 hours, which is much higher than that of other comparative examples, indicating that it has a high formaldehyde removal effect; and the formaldehyde removal rate reached 81.8% after 5 days, indicating that it has a good long-term formaldehyde removal effect and has a good long-term formaldehyde removal effect.

[0110] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0111] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A long-term formaldehyde-removing environmentally friendly water-based paint, characterized in that: Ingredients are calculated by weight and include: 75-95 parts of waterborne organosilicon-modified acrylic resin, 11-22 parts of activated bentonite, 8-16 parts of formaldehyde removal enhancer, 3.3-4.6 parts of pigment, 0.4-0.8 parts of wetting and dispersing aid, 0.5-1 parts of defoamer, 0.2-0.6 parts of leveling agent, 0.05-0.1 parts of film-forming aid and 26-42 parts of deionized water; Wherein, the activated bentonite is bentonite activated by a silane coupling agent; the formaldehyde removal enhancer is yttrium manganese borate @Co / Bi-MOFs; The preparation method of the formaldehyde removal enhancer comprises: S1. Weigh cobalt chloride and bismuth chloride and dissolve them in N-methylpyrrolidone, then add biphenyl-3,3',5,5'-tetracarboxylic acid, stir evenly at room temperature, and then pour into a reactor. The reactor is sealed and placed in an oven for heat preservation. After the treatment, the precipitate is collected by filtration, washed with alcohol and dried to obtain Co / Bi-MOFs. S2, yttrium chloride, manganese chloride and boric acid are added to deionized water, stirred at 50-60°C until dissolved, Co / Bi-MOFs are added, ultrasonically dispersed evenly, and then the pH is adjusted to 9-10, the reaction solution is poured into a reactor, the reactor is sealed and placed in an oven for heat preservation treatment, after the treatment is completed, the precipitate is collected by filtration, washed with water and dried to obtain a precursor material; S3. The precursor material is placed in a muffle furnace for sintering. After the furnace is cooled, yttrium manganese borate@Co / Bi-MOFs is obtained.

2. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: The preparation process of the activated bentonite comprises: Bentonite, KH-560 coupling agent and anhydrous ethanol are mixed, and after heat treatment at 50-60°C for 8-12 hours, the solid is collected by filtration, washed and dried to obtain activated bentonite; wherein the particle size of the bentonite is 50±5μm, and the mass volume ratio of bentonite, KH-560 and anhydrous ethanol is 1g:(0.3-0.5)g:(10-20)mL.

3. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: In S1, the temperature in the oven is 130-180° C., and the treatment time is 18-36 h. The mass volume ratio of cobalt chloride, bismuth chloride, biphenyl-3,3',5,5'-tetracarboxylic acid and N-methylpyrrolidone is (0.13-0.26) g:(0.32-0.64) g:(0.38-0.76) g:(15-20) mL.

4. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: In S2, the temperature in the oven is 200-250°C, and the treatment time is 15-30h; the mass volume ratio of Co / Bi-MOFs, yttrium chloride, manganese chloride, boric acid and deionized water is 1g:(0.15-0.3)g:(0.1-0.2)g:(0.1-0.3)g:(20-30)mL.

5. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: In S3, the sintering temperature is 350-450° C., and the sintering time is 2-4 hours.

6. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: The pigment is one or a mixture of anatase titanium dioxide, pigment red, pigment yellow, pigment blue, pigment green, and pigment black.

7. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: The wetting and dispersing additive is a mixture of one or more of BYK-161, BYK-163, BYK-180, BYK-190, and BYK-199; the defoaming agent is a mixture of one or more of BYK-028, BYK-022, BYK-024, and BYK-094.

8. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: The leveling agent is one of TEGO-270, TEGO-410, TEGO-450, and TEGO-482, or a mixture of more thereof.

9. The environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: The film-forming aid is one or a mixture of hexylene glycol, propylene glycol, dodecyl alcohol ester, propylene glycol ethyl ether, and propylene glycol butyl ether.

10. A method for preparing the environmentally friendly water-based paint with long-term formaldehyde removal according to claim 1, characterized in that: The following steps are involved: Step 1, weighing water-based organosilicon-modified acrylic resin, activated bentonite, formaldehyde removal enhancer, pigment, wetting and dispersing aid, defoamer, leveling agent, film-forming aid and deionized water according to weight proportion, and mixing them into a mixer; Step 2, set the stirring speed of the mixer to 200-400 r / min, and after stirring for 1-2 hours, obtain the desired water-based coating.