A lightning protection coating for wind turbine blades and its preparation method
By designing an insulating and conductive coating on wind turbine blades to protect against lightning strikes, and utilizing the properties of graphene and boron nitride, the problem of insufficient conductivity in existing coatings has been solved, achieving safe and effective lightning protection and improved weather resistance.
Patent Information
- Application Number
- CN202410862819.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing lightning protection coatings have insufficient conductivity on wind turbine blades, making them unable to effectively conduct lightning current. They may also increase blade weight and cost, affecting the efficiency and safety of wind turbine units.
The lightning protection coating consists of an insulating layer and a conductive layer. The insulating layer is composed of polyaspartic acid ester polyurea base material, isocyanate and insulating ceramic, while the conductive layer is composed of water-based polyaspartic acid ester polyurea, binder and conductive filler. The high conductivity of graphene and the high insulation of boron nitride are used to ensure the safe conduction of lightning current.
It improves the lightning protection capability of wind turbine blades, prevents lightning from directly hitting the blades, reduces blade weight and manufacturing costs, and provides additional rain erosion protection, extending service life.
Smart Images

Figure BDA0004919432430000051 
Figure BDA0004919432430000061
Abstract
Description
Technical Field
[0001] This invention belongs to the field of wind power generation technology, specifically relating to a lightning protection coating for wind turbine blades and its preparation method. Background Technology
[0002] Wind power is a clean and renewable energy source, with the wind turbine as its core equipment. A wind turbine mainly consists of a tower, blades, a generator, and a control system. Among these, the blades are one of the most critical components, their design and material selection directly affecting the turbine's performance and lifespan. However, during operation, wind turbine blades are subject to various environmental factors, such as lightning strikes and ultraviolet radiation. Lightning strikes can damage the blades, affecting the turbine's normal operation and potentially leading to serious safety accidents. Therefore, effectively preventing damage to the blades from lightning and ultraviolet radiation and improving the safety of wind turbines is a pressing issue in the field of wind power technology.
[0003] To address this issue, existing technologies primarily involve coating the blade surface with a lightning protection coating. This coating's main component is a conductive material, which rapidly conducts lightning current to the ground, preventing direct lightning strikes and protecting the blades from damage. Additionally, some technologies embed metal mesh or other conductive materials inside the blades to further enhance their lightning protection capabilities.
[0004] However, existing lightning protection technologies still have some problems. First, the conductivity of existing lightning protection coatings may be insufficient, failing to effectively conduct lightning current to the ground, allowing lightning to still strike the blades and cause damage. Second, existing lightning protection technologies may increase the weight of the blades, affecting the efficiency of the wind turbine. Furthermore, existing lightning protection technologies may increase the manufacturing cost of the blades, impacting the economic benefits of wind power generation. Therefore, how to ensure effective lightning protection while also providing UV resistance to the protective coating, without compromising blade performance or cost, is a pressing issue that needs to be addressed in the field of lightning protection technology. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a lightning protection coating for wind turbine blades and its preparation method, so as to solve the problems that existing coatings are difficult to completely prevent lightning from hitting the blades and reduce the efficiency of wind turbines due to increased blade mass.
[0006] To achieve the above objectives, the present invention employs the following technical solution:
[0007] A lightning protection coating for wind turbine blades includes an insulating layer disposed on the surface of the wind turbine blades, and a conductive layer disposed on the insulating layer.
[0008] The insulating layer is composed of polyaspartic acid ester polyurea base material, isocyanate, and insulating ceramic; the polyaspartic acid ester polyurea base material is composed of polyetheramine, diisocyanate, and polyaspartic acid ester resin; the insulating ceramic is composed of component A, component B, component C, and component D, wherein component A is triethoxysilane, component B is ethoxyphenyl silicone resin, component C is an insulating component, and component D is potassium hydroxide alkali adhesive; component C is composed of boron nitride, acrylate, organic amine, and dimethyl sulfoxide.
[0009] By mass fraction, the conductive layer is composed of 60-70% waterborne polyaspartic ester polyurea, 10-20% binder, and 10-30% conductive filler; the waterborne polyaspartic ester polyurea is composed of polyetheramine, diisocyanate, polyaspartic ester resin, and waterborne isocyanate; the binder is PTFE emulsion, and the conductive filler is graphene powder.
[0010] A further improvement of the present invention is that:
[0011] Preferably, the mass ratio of component A, component B and component C in the insulating ceramic is 1:1:1.5, and the mass content of component D in the insulating ceramic is 0.1% to 0.2%.
[0012] Preferably, in the insulating layer, the molar ratio of polyetheramine to diisocyanate in the polyaspartic ester polyurea base material is 1:(1-1.3), and the mass ratio of polyaspartic ester to polyetheramine is (3-8):1.
[0013] Preferably, in the insulating layer, the mass ratio of the polyaspartic acid ester polyurea base material to the insulating ceramic is (1-2.1):1, and the molar ratio of -NCO in the polyaspartic acid ester polyurea base material to -NH in the isocyanate is 1.2:1.
[0014] Preferably, the mass fractions of boron nitride, acrylate, organic amine and dimethyl sulfoxide in component C are 50%, 10%, 25% and 15%, respectively.
[0015] Preferably, the diisocyanate is any one or a mixture of isoflurone diisocyanate, hexamethylene diisocyanate and 4,4-dicyclohexylmethane diisocyanate;
[0016] The polyetheramine is any one or a mixture of polyetheramine M230, polyetheramine M1000 or polyetheramine M2000;
[0017] The polyaspartic ester is a mixture of F420 and F520, with a molar ratio of (4-5):1 between polyaspartic ester F420 and polyaspartic ester F520.
[0018] A method for preparing a lightning protection coating for wind turbine blades includes the following steps: spraying an insulating coating onto the wind turbine blade to obtain an insulating layer; spraying a conductive coating onto the insulating layer and drying it to obtain a conductive coating.
[0019] The preparation process of the insulating coating is as follows: a mixture of dried polyetheramine and polyaspartic acid ester resin is added dropwise to it in sequence, followed by the addition of dimethyl sulfoxide and then isocyanate. After mixing evenly, the insulating coating is obtained.
[0020] The preparation process of the conductive coating is as follows: a mixture of dried polyetheramine and polyaspartic acid ester resin is added, PTFE emulsion is added and stirred evenly, graphene powder is added, and after stirring evenly, diisocyanate is added; then water is added to dilute the mixture and water-based isocyanate is added, and after mixing evenly, the conductive coating is obtained.
[0021] Preferably, the preparation process of the ceramic matrix is as follows:
[0022] Triethoxysilane and dimethyl sulfoxide were stirred in a water bath. After stirring, ethoxyphenyl silicone resin was added, followed by stirring. Boron nitride, acrylic acid, and organic amine were then added and stirred until homogeneous to obtain a ceramic matrix.
[0023] Preferably, the pressure for spraying the insulating coating is 0.8-1.2 MPa, and the spraying time is 10-20 min.
[0024] Preferably, the pressure for spraying the conductive coating is 0.5-1.0 MPa, and the time is 10-20 min.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] This invention discloses a lightning protection coating for wind turbine blades, which consists of a conductive surface layer and an insulating bottom layer. The surface layer comprises a water-based polyaspartic ester polyurea, a binder, and conductive fillers. The water-based polyaspartic ester polyurea is made from polyetheramine, diisocyanate, polyaspartic ester resin, and water-based isocyanate. Polyetheramine is a hydrophilic monomer, giving the system good hydrophilicity, which facilitates the formation of a water film on the wind turbine blade surface, effectively buffering the impact of raindrops on the leading edge of the blade. Diisocyanate extends the chain of the system, increasing the molecular weight of the product. The -NCO groups can react with the -NH groups on the polyaspartic ester to form urea groups, thereby reducing the reactivity of the system. The binder is a PTFE emulsion, a high-molecular polymer dispersion with a solid content of 90%. It has a very low surface energy and good chemical stability, and can build molecular bridges between inorganic and organic substances, connecting two materials with different properties. The conductive filler is graphene, which has excellent electrical conductivity and extremely high electron mobility, exceeding 15,000 cm⁻¹ at room temperature.2 With a velocity of / V·s, graphene's migration rate can reach one-three-hundredth of the speed of light, far exceeding that of traditional semiconductors and conductors such as silicon and copper. Graphene's resistivity is approximately 10^-10⁻⁶ V·s. -6 With a conductivity of Ω·cm, it is one of the best-conducting materials known to date. The bottom layer is an insulating coating consisting of aspartic acid ester polyurea and insulating ceramics. The insulating component in the insulating ceramics is boron nitride, an inorganic material with high insulation and thermal conductivity, which can be used as an insulating filler in the preparation of polymer insulating coatings. Boron nitride can resist thermal decomposition and oxidation at high temperatures, maintaining its structural and performance stability. It can withstand rapid temperature changes without stress concentration and fracture due to thermal expansion and contraction. This invention improves the weather resistance and toughness of the coating while ensuring lightning protection for wind turbine blades.
[0027] This invention also discloses a method for preparing a lightning protection coating for wind turbine blades. The conductive layer on the surface is prepared by using water-based polyaspartic acid ester polyurea as the base material and graphene as the main conductive component. Due to its excellent conductivity and good stability, PTFE (polytetrafluoroethylene emulsion) is used as a binder to increase the affinity between graphene powder and organic polymers, crosslinking graphene and polyaspartic acid ester polyurea together, thereby increasing the conductivity of the surface coating. The underlying insulating layer comprises polyaspartic acid ester polyurea and insulating ceramic. The main insulating component of the insulating ceramic is boron nitride, which has high resistivity, good high-temperature stability, good thermal shock resistance, high strength, and corrosion resistance. It can increase the insulation of the underlying layer and improve the hardness and toughness of the coating, enhancing the overall resistance to rainwater erosion. Specifically, polyaspartic ester polyurea is made from polyetheramine, diisocyanate, polyaspartic ester resin, and isocyanate. Polyetheramine, as a hydrophilic monomer, gives the system good hydrophilicity, which facilitates the formation of a water film on the leading edge surface of wind turbine blades, effectively buffering the impact of raindrops on the blade's leading edge. Diisocyanate extends the chain of the system, increasing the molecular weight of the product, thereby increasing the solids content of the polyurea base material and improving solution stability. Furthermore, the -NCO groups can react with the -NH groups on the polyaspartic ester to form urea groups, thus reducing the system's reactivity. The modified polyaspartic ester polyurea is stable. When compounded with conductive fillers and insulating fillers, both the surface and bottom layers exhibit strong impact resistance and adhesion, and both coatings have low water absorption, effectively reducing rain erosion damage to the wetted surface.
[0028] This invention also has the following advantages:
[0029] 1. The lightning protection coating of this invention possesses excellent conductivity and insulation properties. If the lightning intensity is low, it can effectively conduct the lightning current to the ground, preventing direct lightning strikes to the blades. If the lightning intensity is high, even after the first conductive layer is breached, a second insulating layer remains, thus more effectively protecting the blades from damage and improving the safety of the wind turbine. 2. Because this invention's lightning protection coating does not require additional lightning protection devices or conductive mesh on the blades, it does not increase the blade weight and therefore does not affect the efficiency of the wind turbine. Compared to existing metal mesh or other conductive materials, this invention's lightning protection coating is lighter and more suitable for wind turbine blades. 3. The preparation process of this invention's lightning protection coating is simple and low-cost, and it does not increase the manufacturing cost of the blades, thus improving the economic efficiency of wind power generation. Compared to existing technologies, this invention's lightning protection coating is more economically valuable. 4. This invention's lightning protection coating can also provide additional protective functions, such as resistance to rain erosion, further improving the blade's service life and performance. Detailed Implementation
[0030] This invention discloses a method for preparing a lightning protection coating for wind turbine blades. The coating consists of a conductive surface layer and an insulating bottom layer, wherein the insulating layer has a thickness of 125–175 μm, and the conductive layer has a thickness of 120–135 μm. The composition of the coating is first described in a table below.
[0031] Table 1 Material composition of the coating of the present invention
[0032]
[0033]
[0034] The bottom layer is an insulating coating comprising polyaspartic acid ester polyurea base material, isocyanate, and insulating ceramic; wherein the polyaspartic acid ester polyurea base material is composed of polyetheramine, diisocyanate, and polyaspartic acid ester resin, and the mass ratio of polyaspartic acid ester polyurea base material to insulating ceramic is (1~2.1):1; the molar ratio of -NH in polyaspartic acid ester polyurea base material to -NCO in isocyanate is 1.2:1.
[0035] Specifically, the diisocyanate is any one or a mixture of isoflurone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.
[0036] Specifically, the polyetheramine is any one or a mixture of polyetheramine M230, polyetheramine M1000, or polyetheramine M2000.
[0037] Specifically, the polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is (4-5):1.
[0038] Specifically, the molar ratio of polyetheramine to diisocyanate is 1:(1 to 1.3).
[0039] Specifically, the mass ratio of polyaspartic acid ester to polyetheramine is (3-8):1.
[0040] The insulating ceramic consists of four components: A, B, C, and D. Component A is triethoxysilane, component B is ethoxyphenyl silicone resin, component C is the insulating component, specifically composed of boron nitride, acrylate, organic amine, and dimethyl sulfoxide in mass fractions of 50%, 10%, 25%, and 15%, respectively, and component D is the catalyst, namely potassium hydroxide alkaline adhesive. The specific preparation steps are as follows:
[0041] (1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker and place the beaker in an oil bath; slowly add 0.2 to 0.3 parts of potassium hydroxide into the beaker through a funnel, turn on the stirring and heat to 115-120℃. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain transparent potassium hydroxide alkaline gel, i.e. catalyst component D.
[0042] (2) Weigh components A, B and C of the ceramic respectively. The mass ratio of the three components in the ceramic is 1:1:1.5. Weigh catalyst component D in step (8). Its mass content is 0.1 to 0.2% of the mass of the insulating ceramic.
[0043] (3) Place component A, triethoxysilane, and dimethyl sulfoxide with catalyst component D in a 50°C water bath and stir for 0.5 to 1 hour at a stirring speed of 100 to 180 r / min.
[0044] (4) Add component B, ethoxyphenyl silicone resin, to the reaction product in step (3) and stir at room temperature for 2 to 2.5 hours at a stirring speed of 400 to 560 r / min.
[0045] (5) Add boron nitride, acrylic acid and organic amine from component C to the reaction product of step (4), stir at room temperature for 1 to 1.5 h at a stirring speed of 400 to 500 r / min to obtain insulating ceramic matrix.
[0046] (6) Weigh the polyetheramine and polyaspartic acid ester resin according to the above proportions, and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 100~105℃, -0.04~-0.07MPa, and 1~1.5h.
[0047] (7) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0048] (8) Weigh the ceramic base material in step (5) according to the above proportion and place it in a constant pressure funnel.
[0049] (9) Take the four-necked flask containing polyetheramine and polyaspartic acid ester resin from step (6) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 30-50°C.
[0050] (10) Open the constant pressure funnel in step (8) and add ceramic base material into the four-necked flask at a uniform speed for 0.5 to 1 hour.
[0051] (11) Open the constant pressure titration funnel in step (7) and add diisocyanate dropwise into the four-necked flask at a uniform rate for 1 to 1.5 hours.
[0052] (12) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 50-70°C and react at a constant temperature for 2-3 hours.
[0053] (13) Add dimethyl sulfoxide slowly dropwise to the reaction product of step (12) using a constant pressure titration funnel, and start stirring. The dropwise addition time is 0.5 to 1 h, the stirring speed is 1000 to 1300 r / min, and the stirring time is 0.3 to 0.5 h. In this step, dimethyl sulfoxide acts as a binder to solidify the insulating ceramic in polyurea.
[0054] (14) Weigh the isocyanate according to the weight of the reaction product polyaspartic acid ester-ceramic dispersion in step (13). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to obtain the insulating coating.
[0055] (15) The insulating coating from step (14) is loaded into a constant pressure sprayer. The spraying pressure is 0.8-1.2 MPa, the spraying temperature is room temperature, the spraying time is 10-20 minutes, and the coating is dried at room temperature for 10 minutes to obtain the bottom insulating coating, which has the characteristics of rain erosion resistance.
[0056] The conductive layer comprises waterborne polyaspartic ester polyurea, an adhesive, and a conductive filler, with the following mass contents: 60–70%, 10–20%, and 10–30%, respectively. The waterborne polyaspartic ester polyurea is composed of polyetheramine, diisocyanate, polyaspartic ester resin, and waterborne isocyanate; the adhesive is a PTFE emulsion with a solid content of 90%; and the conductive filler is graphene powder. The adhesive is used to fix the conductive filler within the waterborne polyaspartic ester polyurea.
[0057] Specifically, the diisocyanate is any one or a mixture of isoflurone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.
[0058] Specifically, the polyetheramine is any one or a mixture of polyetheramine M230, polyetheramine M1000, or polyetheramine 2000.
[0059] Specifically, the polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is (4-5):1.
[0060] Specifically, the molar ratio of polyetheramine to diisocyanate is 1:(1 to 1.3).
[0061] Specifically, the mass ratio of polyaspartic acid ester to polyetheramine is (3-8):1.
[0062] The specific fabrication process of the conductive layer includes the following steps:
[0063] (1) Weigh polyetheramine and polyaspartic acid ester according to the above proportions and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 100~105℃, -0.07~-0.04MPa, and 1~1.5h.
[0064] (2) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0065] (3) Weigh the binder and conductive filler according to the above proportions. Their mass contents in the coating are 10-20% and 10-30% respectively, and place them in constant pressure funnels respectively.
[0066] (4) Take the four-necked flask containing polyetheramine and polyaspartic acid ester from step (1) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 30-50°C.
[0067] (5) Open the constant pressure funnel containing the PTFE emulsion binder in step (3), and drop the binder into the four-necked flask in step (4). The dropping time is 1 to 2 hours, and start stirring. The stirring conditions are 40 to 70 r / min. Stop stirring after the dropping is completed.
[0068] (6) Open the constant pressure funnel containing the conductive filler from step (3), and add the conductive filler dropwise into the four-necked flask from step (5). The dropwise addition time is 1 to 2 hours, and start stirring at 50 to 60 r / min. Stop stirring after the dropwise addition is complete.
[0069] (7) Open the constant pressure titration funnel in step (2) and add diisocyanate dropwise into the four-necked flask at a uniform rate for 1 to 1.5 hours.
[0070] (8) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 50-70°C and react at a constant temperature for 2-3 hours.
[0071] (9) Replace the constant pressure titration funnel and slowly add deionized water to the reaction product of step (8), and turn on the stirring. If the dropping speed is too fast, it will easily lead to uneven dispersion and agglomeration. The dropping time is 0.5 to 1 hour, the stirring speed is 1000 to 1300 r / min, and the stirring time is 0.3 to 0.5 hours.
[0072] (10) Weigh the water-based isocyanate according to the weight of the modified polyaspartic acid ester resin of the reaction product in step (9). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to finally obtain the conductive coating.
[0073] The conductive coating from step (10) is loaded into a constant pressure sprayer. The spraying pressure is 0.5-1.0 MPa, the spraying temperature is room temperature, and the spraying time is 10-20 minutes. Finally, a conductive coating is obtained on the surface to ensure the adhesion and weather resistance of the lightning protection coating.
[0074] The following is a further explanation with reference to specific embodiments:
[0075] Example 1
[0076] Preparation of insulating layer
[0077] The bottom layer is an insulating coating comprising polyaspartic acid ester polyurea base material, isocyanate, and insulating ceramic; wherein the polyaspartic acid ester polyurea base material is composed of polyetheramine, diisocyanate, and polyaspartic acid ester resin, and the mass ratio of polyaspartic acid ester polyurea base material to insulating ceramic is 1.5:1; the molar ratio of -NH in polyaspartic acid ester polyurea base material to -NCO in isocyanate is 1.2:1.
[0078] The diisocyanate is isoflurone diisocyanate, and the polyetheramine is polyetheramine M230.
[0079] The polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is 4.5:1.
[0080] Specifically, the molar ratio of polyetheramine to diisocyanate is 1:1.2.
[0081] Specifically, the mass ratio of polyaspartic acid ester to polyetheramine is 5:1.
[0082] The insulating ceramic consists of four components: A, B, C, and D. Component A is triethoxysilane, component B is ethoxyphenyl silicone resin, component C is the insulating component, specifically composed of boron nitride, acrylate, organic amine, and dimethyl sulfoxide in mass fractions of 50%, 10%, 25%, and 15%, respectively, and component D is the catalyst, namely potassium hydroxide alkaline adhesive. The specific preparation steps are as follows:
[0083] (1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker and place the beaker in an oil bath; slowly add 0.25 parts of potassium hydroxide into the beaker through a funnel, turn on the stirring and heat to 118°C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain transparent potassium hydroxide alkaline gel, i.e. catalyst component D.
[0084] (2) Weigh components A, B and C of the ceramic respectively. The mass ratio of the three components in the ceramic is 1:1:1.5. Weigh catalyst component D in step (8). Its mass content is 0.15% of the mass of the insulating ceramic.
[0085] (3) Component A, triethoxysilane and dimethyl sulfoxide, and catalyst component D were placed in a 50°C water bath and stirred for 0.8 h at a stirring speed of 150 r / min.
[0086] (4) Add component B, ethoxyphenyl silicone resin, to the reaction product in step (3) and stir at room temperature for 2.2 h at a stirring speed of 500 r / min.
[0087] (5) Add boron nitride, acrylic acid and organic amine from component C to the reaction product of step (4), stir at room temperature for 1.2 h at a stirring speed of 450 r / min to obtain insulating ceramic matrix.
[0088] (6) Weigh the polyetheramine and polyaspartic acid ester resin according to the above proportions, and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 102℃, -0.05MPa, and 1.2h. The polyaspartic acid ester is a mixture of F420 and F520, and the molar ratio of polyaspartic acid ester F420 to polyaspartic acid ester F520 is 4.5:1. The polyetheramine is M230.
[0089] (7) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0090] (8) Weigh the insulating ceramic base material in step (5) according to the above proportion and place it in a constant pressure funnel, wherein the mass ratio of polyaspartic acid ester polyurea base material to insulating ceramic is 1.5:1.
[0091] (9) Take the four-necked flask containing polyetheramine and polyaspartic acid ester resin from step (6) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 40°C.
[0092] (10) Open the constant pressure funnel in step (8) and add ceramic base material into the four-necked flask at a uniform speed for 0.8 hours.
[0093] (11) Open the constant pressure titration funnel in step (7) and add diisocyanate dropwise into the four-necked flask at a constant speed for 1.2 hours.
[0094] (12) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 60°C and react at a constant temperature for 2.5 hours.
[0095] (13) Add dimethyl sulfoxide slowly dropwise to the reaction product of step (12) using a constant pressure titration funnel, and start stirring. The addition time is 0.8 h, the stirring speed is 1200 r / min, and the stirring time is 0.4 h. In this step...
[0096] (14) Weigh the isocyanate according to the weight of the reaction product polyaspartic acid ester-ceramic dispersion in step (13). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to obtain the insulating coating.
[0097] (15) The insulating coating from step (14) is loaded into a constant pressure sprayer. The spraying pressure is 1 MPa, the spraying temperature is room temperature, the spraying time is 15 minutes, and the coating is dried at room temperature for 10 minutes. Finally, the bottom insulating coating is obtained, which makes the insulating coating both rain erosion resistant.
[0098] Preparation of conductive layer:
[0099] The conductive layer comprises waterborne polyaspartic ester polyurea, an adhesive, and a conductive filler, with mass contents of 65%, 15%, and 20%, respectively. The waterborne polyaspartic ester polyurea is composed of polyetheramine, diisocyanate, polyaspartic ester resin, and waterborne isocyanate; the adhesive is a PTFE emulsion with a solid content of 90%; and the conductive filler is graphene powder. The adhesive is used to fix the conductive filler within the waterborne polyaspartic ester polyurea.
[0100] The diisocyanate is isoflurone diisocyanate, and the polyetheramine is polyetheramine M230.
[0101] The polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is 4.5:1.
[0102] The molar ratio of polyetheramine to diisocyanate is 1:1.2.
[0103] The mass ratio of polyaspartic acid ester to polyetheramine is 5:1.
[0104] The specific fabrication process of the conductive layer includes the following steps:
[0105] (1) Weigh the polyetheramine and polyaspartic acid ester resin according to the above proportions and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 102℃, -0.05MPa, and 1.2h. The polyaspartic acid ester is a mixture of F420 and F520, and the molar ratio of polyaspartic acid ester F420 to polyaspartic acid ester F520 is 4.5:1. The polyetheramine is M230.
[0106] (2) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0107] (3) Weigh the binder and conductive filler according to the above proportions and place them in constant pressure funnels respectively.
[0108] (4) Take the four-necked flask containing polyetheramine and polyaspartic acid ester from step (1) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 40°C.
[0109] (5) Open the constant pressure funnel containing the PTFE emulsion binder in step (3), drop the binder into the four-necked flask in step (4), add it over a period of 1.5 hours, and start stirring at 50 r / min. Stop stirring after the addition is complete.
[0110] (6) Open the constant pressure funnel containing the conductive filler from step (3), and add the conductive filler dropwise into the four-necked flask from step (5). The dropwise addition time is 1.5 hours, and start stirring at 55 r / min. Stop stirring after the dropwise addition is complete.
[0111] (7) Open the constant pressure titration funnel in step (2) and add diisocyanate dropwise into the four-necked flask at a constant speed for 1.2 hours.
[0112] (8) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 60°C and react at a constant temperature for 2.5 hours.
[0113] (9) Replace the constant pressure titration funnel and slowly add deionized water to the reaction product of step (8), and turn on the stirring. If the dropping speed is too fast, it is easy to cause uneven dispersion and agglomeration. The dropping time is 0.5 to 1 hour, the stirring speed is 1200 r / min, and the stirring time is 0.4 hours.
[0114] (10) Weigh the water-based isocyanate according to the weight of the modified polyaspartic acid ester resin of the reaction product in step (9). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to finally obtain the conductive coating.
[0115] Example 2
[0116] Preparation of insulating layer
[0117] The bottom layer is an insulating coating comprising polyaspartic acid ester polyurea base material, isocyanate, and insulating ceramic; wherein the polyaspartic acid ester polyurea base material is composed of polyetheramine, diisocyanate, and polyaspartic acid ester resin, and the mass ratio of polyaspartic acid ester polyurea base material to insulating ceramic is 1:1; the molar ratio of -NH in polyaspartic acid ester polyurea base material to -NCO in isocyanate is 1.2:1.
[0118] The diisocyanate is hexamethylene diisocyanate, and the polyetheramine is polyetheramine M1000.
[0119] The polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is 4:1.
[0120] Specifically, the molar ratio of polyetheramine to diisocyanate is 1:1.
[0121] Specifically, the mass ratio of polyaspartic acid ester to polyetheramine is 3:1.
[0122] The insulating ceramic consists of four components: A, B, C, and D. Component A is triethoxysilane, component B is ethoxyphenyl silicone resin, component C is the insulating component, specifically composed of boron nitride, acrylate, organic amine, and dimethyl sulfoxide in mass fractions of 50%, 10%, 25%, and 15%, respectively, and component D is the catalyst, namely potassium hydroxide alkaline adhesive. The specific preparation steps are as follows:
[0123] (1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker and place the beaker in an oil bath; slowly add 0.2 parts of potassium hydroxide into the beaker through a funnel, turn on the stirring and heat to 115°C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain transparent potassium hydroxide alkaline gel, i.e. catalyst component D.
[0124] (2) Weigh components A, B and C of the ceramic respectively. The mass ratio of the three components in the ceramic is 1:1:1.5. Weigh catalyst component D in step (8). Its mass content is 0.1% of the mass of the insulating ceramic.
[0125] (3) Component A, triethoxysilane and dimethyl sulfoxide, and catalyst component D were placed in a 50°C water bath and stirred for 0.5 h at a stirring speed of 100 r / min.
[0126] (4) Add component B, ethoxyphenyl silicone resin, to the reaction product in step (3), and stir at room temperature for 2 hours at a stirring speed of 500 r / min.
[0127] (5) Add boron nitride, acrylic acid and organic amine from component C to the reaction product of step (4), stir at room temperature for 1 hour at a stirring speed of 400 r / min to obtain insulating ceramic matrix.
[0128] (6) Weigh the polyetheramine and polyaspartic acid ester resin according to the above proportions, and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 100℃, -0.04MPa, and 1h.
[0129] (7) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0130] (8) Weigh the insulating ceramic base material in step (5) according to the above proportion and place it in a constant pressure funnel.
[0131] (9) Take the four-necked flask containing polyetheramine and polyaspartic acid ester resin from step (6) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 30°C.
[0132] (10) Open the constant pressure funnel in step (8) and add ceramic base material into the four-necked flask at a uniform speed for 0.5 hours.
[0133] (11) Open the constant pressure titration funnel in step (7) and add diisocyanate dropwise into the four-necked flask at a uniform rate for 1 hour.
[0134] (12) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 50°C and react at a constant temperature for 3 hours.
[0135] (13) Add dimethyl sulfoxide slowly dropwise to the reaction product of step (12) using a constant pressure titration funnel, and start stirring. The addition time is 0.5 h, the stirring speed is 1000 r / min, and the stirring time is 0.5 h. In this step...
[0136] (14) Weigh the isocyanate according to the weight of the reaction product polyaspartic acid ester-ceramic dispersion in step (13). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to obtain the insulating coating.
[0137] (15) The insulating coating from step (14) is loaded into a constant pressure sprayer. The spraying pressure is 0.8 MPa, the spraying temperature is room temperature, the spraying time is 20 minutes, and the coating is dried at room temperature for 10 minutes. Finally, the bottom insulating coating is obtained, which makes the insulating coating both rain erosion resistant.
[0138] Preparation of conductive layer:
[0139] The conductive layer comprises waterborne polyaspartic ester polyurea, an adhesive, and a conductive filler, with mass contents of 60%, 20%, and 20%, respectively. The waterborne polyaspartic ester polyurea is composed of polyetheramine, diisocyanate, polyaspartic ester resin, and waterborne isocyanate; the adhesive is a PTFE emulsion with a solid content of 90%; and the conductive filler is graphene powder. The adhesive is used to fix the conductive filler within the waterborne polyaspartic ester polyurea.
[0140] The diisocyanate is hexamethylene diisocyanate, and the polyetheramine is polyetheramine M1000.
[0141] The polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is 4:1.
[0142] The molar ratio of polyetheramine to diisocyanate is 1:1.
[0143] The mass ratio of polyaspartic acid ester to polyetheramine is 3:1.
[0144] The specific fabrication process of the conductive layer includes the following steps:
[0145] (1) Weigh the polyetheramine and polyaspartic acid ester resin according to the above proportions and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 100℃, -0.07MPa, and 1h.
[0146] (2) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0147] (3) Weigh the binder and conductive filler according to the above proportions and place them in constant pressure funnels respectively.
[0148] (4) Take the four-necked flask containing polyetheramine and polyaspartic acid ester from step (1) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 30°C.
[0149] (5) Open the constant pressure funnel containing the PTFE emulsion binder in step (3), drop the binder into the four-necked flask in step (4), add it over a period of 1 hour, and start stirring at 40 r / min. Stop stirring after the addition is complete.
[0150] (6) Open the constant pressure funnel containing the conductive filler from step (3), and add the conductive filler dropwise into the four-necked flask from step (5). The dropwise addition time is 1 hour, and start stirring at 50 r / min. Stop stirring after the dropwise addition is complete.
[0151] (7) Open the constant pressure titration funnel in step (2) and add diisocyanate dropwise into the four-necked flask at a constant speed for 1 hour.
[0152] (8) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 50°C and react at a constant temperature for 2 hours.
[0153] (9) Replace the constant pressure titration funnel and slowly add deionized water to the reaction product of step (8), and turn on the stirrer. If the dropping speed is too fast, it is easy to cause uneven dispersion and agglomeration. The dropping time is 0.5h, the stirring speed is 1000r / min, and the stirring time is 0.5h.
[0154] (10) Weigh the water-based isocyanate according to the weight of the modified polyaspartic acid ester resin of the reaction product in step (9). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to finally obtain the conductive coating.
[0155] Example 3
[0156] Preparation of insulating layer
[0157] The bottom layer is an insulating coating comprising polyaspartic acid ester polyurea base material, isocyanate, and insulating ceramic; wherein the polyaspartic acid ester polyurea base material is composed of polyetheramine, diisocyanate, and polyaspartic acid ester resin, and the mass ratio of polyaspartic acid ester polyurea base material to insulating ceramic is 2.1:1; the molar ratio of -NH in polyaspartic acid ester polyurea base material to -NCO in isocyanate is 1.2:1.
[0158] The diisocyanate is 4,4'-dicyclohexylmethane diisocyanate, and the polyetheramine is polyetheramine M2000.
[0159] The polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is 5:1.
[0160] Specifically, the molar ratio of polyetheramine to diisocyanate is 1:1.3.
[0161] Specifically, the mass ratio of polyaspartic acid ester to polyetheramine is 8:1.
[0162] The insulating ceramic consists of four components: A, B, C, and D. Component A is triethoxysilane, component B is ethoxyphenyl silicone resin, component C is the insulating component, specifically composed of boron nitride, acrylate, organic amine, and dimethyl sulfoxide in mass fractions of 50%, 10%, 25%, and 15%, respectively, and component D is the catalyst, namely potassium hydroxide alkaline adhesive. The specific preparation steps are as follows:
[0163] (1) Place 100 parts of octamethylcyclotetrasiloxane in a beaker and place the beaker in an oil bath; slowly add 0.2 parts of potassium hydroxide into the beaker through a funnel, turn on the stirring and heat to 120°C. After the potassium hydroxide is completely dissolved, cool to room temperature to obtain transparent potassium hydroxide alkaline gel, i.e. catalyst component D.
[0164] (2) Weigh components A, B and C of the ceramic respectively. The mass ratio of the three components in the ceramic is 1:1:1.5. Weigh the catalyst component D in step (8). Its mass content is 0.2% of the mass of the insulating ceramic.
[0165] (3) Component A, triethoxysilane and dimethyl sulfoxide, and catalyst component D were placed in a 50°C water bath and stirred for 1 hour at a stirring speed of 180 r / min.
[0166] (4) Add component B, ethoxyphenyl silicone resin, to the reaction product in step (3) and stir at room temperature for 2.5 h at a stirring speed of 560 r / min.
[0167] (5) Add boron nitride, acrylic acid and organic amine from component C to the reaction product of step (4), stir at room temperature for 1 hour at a stirring speed of 500 r / min to obtain insulating ceramic matrix.
[0168] (6) Weigh the polyetheramine and polyaspartic acid ester resin according to the above proportions, and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 105℃, -0.07MPa, and 1.5h.
[0169] (7) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0170] (8) Weigh the insulating ceramic base material in step (5) according to the above proportion and place it in a constant pressure funnel.
[0171] (9) Take the four-necked flask containing polyetheramine and polyaspartic acid ester resin from step (6) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 30°C.
[0172] (10) Open the constant pressure funnel in step (8) and add ceramic base material into the four-necked flask at a uniform speed for 1 hour.
[0173] (11) Open the constant pressure titration funnel in step (7) and add diisocyanate dropwise into the four-necked flask at a uniform rate for 1.5 hours.
[0174] (12) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 70°C and react at a constant temperature for 2 hours.
[0175] (13) Add dimethyl sulfoxide slowly dropwise to the reaction product of step (12) using a constant pressure titration funnel, and start stirring. The addition time is 1 hour, the stirring speed is 1300 r / min, and the stirring time is 0.3 hours.
[0176] (14) Weigh the isocyanate according to the weight of the reaction product polyaspartic acid ester-ceramic dispersion in step (13). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to obtain the insulating coating.
[0177] (15) The insulating coating from step (14) is loaded into a constant pressure sprayer. The spraying pressure is 1.2 MPa, the spraying temperature is room temperature, the spraying time is 10 minutes, and the coating is dried at room temperature for 10 minutes. Finally, the bottom insulating coating is obtained, which makes the insulating coating both rain erosion resistant.
[0178] Preparation of conductive layer:
[0179] The conductive layer comprises waterborne polyaspartic ester polyurea, an adhesive, and a conductive filler, with mass contents of 70%, 10%, and 20%, respectively. The waterborne polyaspartic ester polyurea is composed of polyetheramine, diisocyanate, polyaspartic ester resin, and waterborne isocyanate; the adhesive is a PTFE emulsion with a solid content of 90%; and the conductive filler is graphene powder. The adhesive is used to fix the conductive filler within the waterborne polyaspartic ester polyurea.
[0180] The diisocyanate is hexamethylene diisocyanate, and the polyetheramine is polyetheramine M1000.
[0181] The polyaspartic ester is a mixture of F420 and F520, and the molar ratio of polyaspartic ester F420 to polyaspartic ester F520 is 5:1.
[0182] The molar ratio of polyetheramine to diisocyanate is 1:1.3.
[0183] The mass ratio of polyaspartic acid ester to polyetheramine is 8:1.
[0184] The specific fabrication process of the conductive layer includes the following steps:
[0185] (1) Weigh the polyetheramine and polyaspartic acid ester resin according to the above proportions and place them in a four-necked flask for vacuum drying. The vacuum drying conditions are: 105℃, -0.04MPa, and 1.5h.
[0186] (2) Weigh the diisocyanate according to the above proportion and place it in a constant pressure titration funnel.
[0187] (3) Weigh the binder and conductive filler according to the above proportions and place them in constant pressure funnels respectively.
[0188] (4) Take the four-necked flask containing polyetheramine and polyaspartic acid ester from step (1) out of the vacuum drying oven, introduce nitrogen into it and turn on the stirrer to cool it down to 50°C.
[0189] (5) Open the constant pressure funnel containing the PTFE emulsion binder in step (3), drop the binder into the four-necked flask in step (4), add it over a period of 1 hour, and start stirring at 70 r / min. Stop stirring after the addition is complete.
[0190] (6) Open the constant pressure funnel containing the conductive filler from step (3), and add the conductive filler dropwise into the four-necked flask from step (5). The dropwise addition time is 2 hours, and start stirring at 60 r / min. Stop stirring after the dropwise addition is complete.
[0191] (7) Open the constant pressure titration funnel in step (2) and add diisocyanate dropwise into the four-necked flask at a uniform rate for 1.5 hours.
[0192] (8) After the titration is complete, rinse the constant pressure titration funnel with a certain amount of dipropylene glycol dimethyl ether and add it to the four-necked flask. Heat the mixture to 70°C and react at a constant temperature for 3 hours.
[0193] (9) Replace the constant pressure titration funnel and slowly add deionized water to the reaction product of step (8), and turn on the stirring. If the dropping speed is too fast, it will easily lead to uneven dispersion and agglomeration. The dropping time is 0.5h, the stirring speed is 1300r / min, and the stirring time is 0.3h.
[0194] (10) Weigh the water-based isocyanate according to the weight of the modified polyaspartic acid ester resin of the reaction product in step (9). The ratio of the two is calculated as n(—NCO):n(—NH)=1.2:1. Stir the two thoroughly and mix them evenly to finally obtain the conductive coating.
[0195] Example 4
[0196] In this embodiment, the mass contents of waterborne polyaspartic acid ester polyurea, binder and conductive filler in the conductive layer are 70%, 20% and 10% respectively, and the remaining uninvolved parts are the same as in Example 1.
[0197] Example 5
[0198] In this embodiment, the mass contents of waterborne polyaspartic acid ester polyurea, binder and conductive filler in the conductive layer are 65%, 15% and 20% respectively, and the remaining uninvolved parts are the same as in Example 1.
[0199] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A lightning protection coating for wind turbine blades, characterized in that, This includes an insulating layer disposed on the surface of the wind turbine blades, and a conductive layer disposed on the insulating layer; The insulating layer is composed of polyaspartic acid ester polyurea base material, isocyanate, and insulating ceramic; the polyaspartic acid ester polyurea base material is composed of polyetheramine, diisocyanate, and polyaspartic acid ester resin; the insulating ceramic is composed of component A, component B, component C, and component D, wherein component A is triethoxysilane, component B is ethoxyphenyl silicone resin, component C is an insulating component, and component D is potassium hydroxide alkali adhesive; component C is composed of boron nitride, acrylate, organic amine, and dimethyl sulfoxide. By mass fraction, the conductive layer is composed of 60-70% waterborne polyaspartic ester polyurea, 10-20% binder, and 10-30% conductive filler; the waterborne polyaspartic ester polyurea is composed of polyetheramine, diisocyanate, polyaspartic ester resin, and waterborne isocyanate; the binder is PTFE emulsion, and the conductive filler is graphene powder; The insulation layer has a thickness of 125~175um, and the conductive layer has a thickness of 120~135um.
2. The lightning protection coating for wind turbine blades according to claim 1, characterized in that, The mass ratio of component A, component B and component C in the insulating ceramic is 1:1:1.5, and the mass content of component D in the insulating ceramic is 0.1~0.2%.
3. The lightning protection coating for wind turbine blades according to claim 1, characterized in that, In the insulating layer, the molar ratio of polyetheramine to diisocyanate in the polyaspartic ester polyurea base material is 1:(1~1.3), and the mass ratio of polyaspartic ester to polyetheramine is (3~8):
1.
4. The lightning protection coating for wind turbine blades according to claim 1, characterized in that, In the insulating layer, the mass ratio of the polyaspartic acid ester polyurea base material to the insulating ceramic is (1~2.1):1, and the molar ratio of -NCO in the polyaspartic acid ester polyurea base material to -NH in the isocyanate is 1.2:
1.
5. The lightning protection coating for wind turbine blades according to claim 1, characterized in that, In component C, the mass fractions of boron nitride, acrylate, organic amine, and dimethyl sulfoxide are 50%, 10%, 25%, and 15%, respectively.
6. The lightning protection coating for wind turbine blades according to claim 1, characterized in that, The diisocyanate is any one or a mixture of isoflurone diisocyanate, hexamethylene diisocyanate and 4,4'-dicyclohexylmethane diisocyanate; The polyetheramine is any one or a mixture of polyetheramine M230, polyetheramine M1000 or polyetheramine M2000; Polyaspartic acid ester is a mixture of F420 and F520, with a molar ratio of (4~5):1 between polyaspartic acid ester F420 and polyaspartic acid ester F520.
7. A method for preparing the lightning protection coating for wind turbine blades according to claim 1, characterized in that, Includes the following steps: An insulating layer is obtained by spraying insulating coating onto wind turbine blades. A conductive coating is obtained by spraying a conductive coating onto an insulating layer and allowing it to dry. The preparation process of the insulating coating is as follows: a mixture of dried polyetheramine and polyaspartic acid ester resin is added dropwise to it in sequence, followed by the addition of dimethyl sulfoxide and then isocyanate. After mixing evenly, the insulating coating is obtained. The preparation process of the conductive coating is as follows: a mixture of dried polyetheramine and polyaspartic acid ester resin is added, PTFE emulsion is added and stirred evenly, graphene powder is added, and after stirring evenly, diisocyanate is added; then water is added to dilute the mixture and water-based isocyanate is added, and after mixing evenly, the conductive coating is obtained.
8. The method for preparing a lightning protection coating for wind turbine blades according to claim 7, characterized in that, The preparation process of the ceramic matrix is as follows: Triethoxysilane and dimethyl sulfoxide were stirred in a water bath. After stirring, ethoxyphenyl silicone resin was added, followed by stirring. Boron nitride, acrylic acid, and organic amine were then added and stirred until homogeneous to obtain a ceramic matrix.
9. A method for preparing a lightning protection coating for wind turbine blades according to claim 7, characterized in that, The pressure for spraying the insulating coating is 0.8-1.2 MPa, and the spraying time is 10-20 minutes.
10. A method for preparing a lightning protection coating for wind turbine blades according to claim 7, characterized in that, The pressure for spraying the conductive coating is 0.5-1.0 MPa, and the time is 10-20 min.
Citation Information
Patent Citations
Front edge protection wind power blade and forming method thereof
CN114589938A
Polyurea-ceramic composite coating for leading edge of wind power blade and preparation method of polyurea-ceramic composite coating
CN117050626A