Preparation method and application of organic long-afterglow luminescent material

By combining phosphor tetraacetylethylenediamine with polyurethane materials and adding disperse dyes, high-efficiency, long-life organic long-afterglow polyurethane materials are prepared, which solves the problems of complex preparation of inorganic long-afterglow materials and insufficient luminous efficiency of organic long-afterglow materials. It achieves rich application scenarios and high-level anti-counterfeiting performance.

CN118772864APending Publication Date: 2024-10-15QINGDAO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410680794.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing inorganic long-afterglow materials suffer from expensive raw materials, poor processing performance and complicated preparation methods in commercial applications. In addition, the luminescence quantum efficiency and lifetime of organic long-afterglow materials are insufficient, which limits their wide application.

Method used

The phosphor tetraacetylethylenediamine is combined with a polyurethane material, and an organic long-afterglow luminescent polyurethane material is prepared through doping. Dispersed dyes are added to control the luminescent color, forming an organic long-afterglow material with high luminescence quantum efficiency and long phosphorescence lifetime.

Benefits of technology

It achieves high luminescence quantum efficiency and long life of organic long-afterglow materials, enriching its application fields, and provides a higher level of concealment and anti-counterfeiting properties by controlling color through dispersed dyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772864A_ABST
    Figure CN118772864A_ABST
Patent Text Reader

Abstract

The invention discloses application of tetraacetylethylenediamine, which is characterized in that tetraacetylethylenediamine is used as a phosphorescent guest molecule and is added into a host polyurethane material in a doping manner to obtain an organic long-afterglow luminescent polyurethane material with long phosphorescent life, and the dosage of the phosphor tetraacetylethylenediamine is 0.5-15% of the mass of polyurethane. The preparation method of the organic long-afterglow luminescent material comprises the following steps: (1) mixing a phosphor tetraacetylethylenediamine with a polyurethane solution to prepare a mixed solution; and (2) injecting the mixed solution prepared in the step (1) into a mold, drying and molding to prepare the organic long-afterglow luminescent material. Disperse dye can also be added to solve the problem that an existing organic long-afterglow luminescent material is single in luminescent color, more choices are provided for preparation of the organic long-afterglow luminescent material, and the organic long-afterglow luminescent material can be used for achieving information encryption and preparing anti-counterfeit labels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of long afterglow luminescent materials, and in particular to a preparation method and application of an organic long afterglow luminescent material. Background Art

[0002] Long afterglow is a special photoluminescence phenomenon. When the excitation light source is turned off, the material can still maintain luminescence for a long time in the visible light range. Long afterglow materials are widely used in various fields such as data encryption, information storage, bio-imaging, sensing, organic light-emitting diodes (OLEDs) due to their unique photophysical properties. At present, a variety of inorganic long afterglow materials with high luminous efficiency, high stability and ultra-long afterglow time have been developed, and the research on inorganic long afterglow materials has become increasingly mature. However, expensive raw materials, poor processing performance and relatively complex preparation methods (such as high-temperature solid-state processes) have become the biggest obstacles to the commercialization of inorganic afterglow materials. In recent years, organic long afterglow materials have attracted much attention due to their large Stokes shift, ultra-long excited state lifetime and rich excited state properties. This type of material has many applications in the field of optoelectronic information: in the field of bio-imaging, long afterglow materials can eliminate spontaneous background fluorescence interference in organisms with the help of time-resolved technology and improve the signal-to-noise ratio of imaging; in the field of chemical sensing, since the triplet excitons of organic long afterglow luminescent molecules are sensitive to oxygen and are easily quenched, they can also be used as oxygen sensors.

[0003] Compared with inorganic long afterglow materials, organic long afterglow materials have the advantages of low toxicity, low cost, flexible molecular design and easy functionalization, so organic long afterglow materials have greater appeal and potential in the field of luminescence. At present, the research on organic long afterglow materials mainly focuses on improving the luminescence quantum efficiency and lifetime. Summary of the invention

[0004] In view of the above problems existing in the prior art, the present invention provides a preparation method and application of an organic long afterglow luminescent material. The present invention utilizes the long afterglow property of the phosphor tetraacetylethylenediamine, uses it as a phosphorescent guest molecule, and adds it to the main polyurethane material by doping to obtain an organic long afterglow luminescent polyurethane material with a long phosphorescence life. Disperse dyes can also be added to solve the problem of single luminescent color of existing organic long afterglow luminescent materials, providing more options for the preparation of organic long afterglow luminescent materials.

[0005] The technical solution of the present invention is as follows:

[0006] The first object of the present invention is to provide an application of tetraacetylethylenediamine as a phosphor for preparing an organic long afterglow luminescent material.

[0007] The second object of the present invention is to provide an organic long afterglow luminescent material, wherein the raw materials of the organic long afterglow luminescent material include phosphor tetraacetylethylenediamine and polyurethane; the amount of phosphor tetraacetylethylenediamine used is 0.5-15% of the mass of polyurethane.

[0008] The third object of the present invention is to provide a method for preparing an organic long afterglow luminescent material, the method comprising the following steps:

[0009] (1) mixing phosphor tetraacetylethylenediamine with a polyurethane solution to prepare a mixed solution;

[0010] (2) injecting the mixed solution obtained in step (1) into a mold, drying and molding, and obtaining an organic long afterglow luminescent material.

[0011] In one embodiment of the present invention, in step (1), the solid content of the polyurethane solution is 20-40%.

[0012] In one embodiment of the present invention, in step (1), the polyurethane in the polyurethane solution is one or more of 88395AU from Bayer, Germany, 1065AU from Covestro, Germany, and HF-1070AP from Huafeng Group.

[0013] In one embodiment of the present invention, in step (1), the solvent of the polyurethane solution is one or more of acetone, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), and N-methylpyrrolidone (NMP).

[0014] In one embodiment of the present invention, in step (1), the amount of the phosphor tetraacetylethylenediamine used is 0.5-15% of the mass of the polyurethane in the polyurethane solution.

[0015] In one embodiment of the present invention, in step (2), the drying and molding temperature is 25-120°C.

[0016] In one embodiment of the present invention, the raw materials of the organic long afterglow luminescent material further include disperse dyes; the amount of disperse dyes used is 0.01-1% of the mass of the polyurethane.

[0017] In one embodiment of the present invention, the method for preparing the organic long afterglow luminescent material comprises the following steps:

[0018] (1) mixing phosphor tetraacetylethylenediamine with a polyurethane solution to prepare a mixed solution;

[0019] (2) adding disperse dye to the mixed solution obtained in step (1), stirring evenly, to obtain a colored mixed solution;

[0020] (3) injecting the colored mixed solution obtained in step (2) into a mold, drying and molding, and obtaining an organic long afterglow luminescent material.

[0021] In one embodiment of the present invention, in step (2), the disperse dye is one or more of red, yellow and blue disperse dyes.

[0022] In one embodiment of the present invention, in step (2), the disperse dye is one or more of disperse red 145, disperse yellow 114, and disperse blue 183.

[0023] In one embodiment of the present invention, the amount of disperse dye used is 0.01-1% of the mass of polyurethane in the polyurethane solution.

[0024] In one embodiment of the present invention, in step (3), the drying and molding temperature is 25-120°C.

[0025] The fourth object of the present invention is to provide an application of the organic long afterglow luminescent material for realizing information encryption or preparing anti-counterfeiting labels.

[0026] The beneficial technical effects of the present invention are:

[0027] The present invention uses tetraacetylethylenediamine as a phosphorescent ligand and dopes it into a polyurethane material to obtain an organic long-lasting polyurethane, which has a strong luminescent quantum efficiency and a long phosphorescence life, and provides more application directions for tetraacetylethylenediamine, enriching its application fields and application scenarios.

[0028] The long afterglow luminescent material of the present invention provides rigid conditions for tetraacetylethylenediamine molecules based on the rich hydrogen bond network between the polyurethane material and the tetraacetylethylenediamine phosphor, which can effectively constrain the movement of the long afterglow molecules, inhibit the non-radiative transition of the triplet excitons of the long afterglow molecules and prolong their life. In addition, some polyurethane materials have good mechanical properties, ductility, flexibility, etc., which provides the possibility for the practical application of organic long afterglow luminescent materials.

[0029] The addition of the disperse dye of the present invention can adjust the long afterglow luminescence color to obtain an organic long afterglow luminescent polyurethane. After turning off the ultraviolet light, the afterglow color can be clearly identified, and the product has a high degree of concealment, is easy to use, and can be easily identified. It can be applied to various types of packaging, high-end clothing, etc. Its rich afterglow color can achieve a higher level of anti-counterfeiting, is difficult to imitate, and has good application prospects. It also provides a new method and idea for the preparation of ultra-long organic long afterglow materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The room temperature phosphorescence spectra of the polyurethane beads prepared in Example 1 at different excitation wavelengths.

[0031] Figure 2The room temperature phosphorescence lifetime of the polyurethane beads prepared in Example 1 at different emission wavelengths.

[0032] Figure 3 This is the information encryption application of the polyurethane material obtained in Example 5 and Comparative Examples 3 and 4.

[0033] Figure 4 This is the anti-counterfeiting performance of the polyurethane material obtained in Example 5. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0035] The raw materials used in the embodiments of the present invention are commercially available unless otherwise specified.

[0036] Example 1

[0037] A method for preparing a spherical long afterglow luminescent polyurethane material, the preparation method comprising the following steps:

[0038] Acetone was selected as a solvent to obtain a polyurethane solution with a solid content of 30% (88395AU from Bayer, Germany), tetraacetylethylenediamine was added to the polyurethane solution (the mass fraction of tetraacetylethylenediamine in the polyurethane was 8%) to obtain a mixed solution, and then the polyurethane mixed solution doped with tetraacetylethylenediamine was injected into a polytetrafluoroethylene mold and baked at 50° C. for 3 hours to obtain a uniform spherical long afterglow luminescent polyurethane material.

[0039] At room temperature, the prepared beads were tested for phosphorescence spectrum and lifetime at different wavelengths. Figure 1 and Figure 2 As shown. Figure 1 It can be seen that the sphere has different phosphorescence emission peaks at different wavelengths, with strong phosphorescence emission at 503nm and 543nm. Compared with the phosphor tetraacetylethylenediamine, its phosphorescence emission position has a significant red shift. Figure 2 It can be seen that no matter it is 503nm emission or 543nm emission, the life of the ball is more than 1s, with an ultra-long life. The life of the phosphor tetraacetylethylenediamine is 643ms, and its doping in polyurethane has the effect of enhancing the life. The prepared ball was turned off after being irradiated with ultraviolet light for a few seconds, and the decay of the long afterglow was observed. The ball still had a long afterglow luminescence performance of about 6s after the ultraviolet light was turned off. The polyurethane material doped with tetraacetylethylenediamine has strong phosphorescent emission and a long life, and can be used as an energy donor to carry out the next step of preparing multi-color long afterglow polyurethane materials.

[0040] Example 2

[0041] A method for preparing a spherical long afterglow luminescent polyurethane material, the preparation method comprising the following steps:

[0042] Acetone was selected as a solvent to obtain a polyurethane solution with a solid content of 30% (88395AU from Bayer, Germany), tetraacetylethylenediamine was added to the polyurethane solution (the mass fraction of tetraacetylethylenediamine in the polyurethane was 15%) to obtain a mixed solution, and then the polyurethane mixed solution doped with tetraacetylethylenediamine was injected into a polytetrafluoroethylene mold and baked at 50° C. for 3 hours to obtain a uniform spherical long afterglow luminescent polyurethane material.

[0043] Example 3

[0044] A method for preparing a spherical long afterglow luminescent polyurethane material, the preparation method comprising the following steps:

[0045] Acetone was selected as a solvent to obtain a polyurethane solution with a solid content of 30% (88395AU from Bayer, Germany), tetraacetylethylenediamine was added to the polyurethane solution (the mass fraction of tetraacetylethylenediamine in the polyurethane was 0.5%) to obtain a mixed solution, and then the polyurethane mixed solution doped with tetraacetylethylenediamine was injected into a polytetrafluoroethylene mold and baked at 50° C. for 3 hours to obtain a uniform spherical long afterglow luminescent polyurethane material.

[0046] Example 4

[0047] A method for preparing a spherical long afterglow luminescent polyurethane material, the preparation method comprising the following steps:

[0048] DMAC was selected as a solvent to obtain a polyurethane solution with a solid content of 25% (1065AU from Covestro, Germany), tetraacetylethylenediamine was added to the polyurethane solution (the mass fraction of tetraacetylethylenediamine in the polyurethane was 10%) to obtain a mixed solution, and then the tetraacetylethylenediamine-doped polyurethane mixed solution was injected into a polytetrafluoroethylene mold and baked at 80°C for 3 hours to obtain a uniform spherical long afterglow luminescent polyurethane material.

[0049] Example 5

[0050] A method for preparing an organic long afterglow luminescent material, the method comprising the following steps:

[0051] Acetone is selected as a solvent to obtain a polyurethane solution with a solid content of 35% (88395AU from Bayer, Germany); tetraacetylethylenediamine is added to the polyurethane solution (the mass fraction of tetraacetylethylenediamine in the polyurethane is 6%), and the mixture is stirred at room temperature for 2 hours; disperse dye is added to the mixed solution of tetraacetylethylenediamine and polyurethane, and the mixture is stirred evenly to obtain a colored mixed solution; wherein the doping amount of the disperse dye is 0.2% of the mass of the polyurethane in the mixed solution; and the obtained colored mixed solution is then injected into a polytetrafluoroethylene mold, and baked at 60° C. for 3 hours to obtain a uniform spherical colored long afterglow luminescent polyurethane material;

[0052] The disperse dyes are disperse red 145, disperse yellow 114 and disperse blue 183, which are mixed in 6 different ratios (mass ratio) to obtain a series of long afterglow luminescent polyurethane materials of different colors. Among them, the ratios of disperse blue 183: disperse yellow 114: disperse red 145 are 1:0:0; 1:1:0; 1:0:1; 0:1:0; 0:1:1; 0:0:1.

[0053] At room temperature, the prepared long afterglow luminescent polyurethane beads of different colors were subjected to phosphorescence spectrum and life test. According to the different dyes added and the ratio, the long afterglow luminescence position and life of the long afterglow luminescent polyurethane beads are shown in Table 1. The luminescence position of the long afterglow luminescent polyurethane beads of different colors can almost cover the full color spectrum (436nm-650nm). The prepared beads were turned off after being irradiated with ultraviolet light for a few seconds, and the attenuation of the long afterglow was observed. The beads still had a long afterglow of about 4-6s after the ultraviolet light was turned off. Multicolor long afterglow luminescent polyurethane materials can be simply prepared by adding disperse dyes to polyurethane materials doped with tetraacetylethylenediamine in different ratios.

[0054] Table 1

[0055]

[0056] Comparative Example 1

[0057] Acetone was selected as the solvent to obtain a polyurethane solution with a solid content of 30% (88395AU from Bayer, Germany). The polyurethane solution was injected into a polytetrafluoroethylene mold and dried at 60°C for 3 hours to obtain uniform polyurethane beads. The prepared beads were irradiated with an ultraviolet lamp for a few seconds and then turned off to observe the decay of the long afterglow. The beads did not have long afterglow luminescence performance after the ultraviolet lamp was turned off.

[0058] Comparative Example 2

[0059] Acetone is selected as a solvent to obtain a polyacrylate solution with a solid content of 30%, tetraacetylethylenediamine is added to the polyacrylate solution (the mass fraction of tetraacetylethylenediamine in the polyacrylate is 8%) to obtain a mixed solution, and then the tetraacetylethylenediamine-doped polyacrylate mixed solution is injected into a polytetrafluoroethylene mold and baked at 50° C. for 3 hours to obtain a long afterglow polyacrylate material. This luminescent material has uneven luminescence due to the lack of interaction between tetraacetylethylenediamine and polyacrylate and poor compatibility.

[0060] Comparative Example 3

[0061] Acetone was used as solvent to obtain a polyurethane solution with a solid content of 30% (88395AU from Bayer, Germany), and Disperse Red 145 was added to the polyurethane solution and stirred evenly to obtain a colored polyurethane solution; wherein the total doping amount of Disperse Red 145 was 0.2% of the mass of the polyurethane;

[0062] The obtained colored polyurethane solution was then injected into a polytetrafluoroethylene mold and baked at 60°C for 3 hours to obtain uniform spherical red polyurethane beads.

[0063] Disperse Red 145 was replaced by Disperse Yellow 114 and Disperse Blue 183 to obtain yellow and blue polyurethane beads, respectively.

[0064] The prepared colored polyurethane beads were irradiated with ultraviolet light for a few seconds and then turned off to observe the decay of the long afterglow. The beads did not have long afterglow luminescence performance after the ultraviolet light was turned off.

[0065] Comparative Example 4

[0066] Acetone was used as a solvent to obtain a polyurethane solution with a solid content of 30% (88395AU from Bayer, Germany), and disperse blue 183 and disperse yellow 114 were added to the polyurethane solution in a mass ratio of 1:1, and stirred evenly to obtain a colored polyurethane solution; wherein the total doping amount of disperse blue 183 and disperse yellow 114 was 0.2% of the mass of the polyurethane;

[0067] Then the obtained colored polyurethane solution was injected into a polytetrafluoroethylene mold and baked at 60°C for 3 hours to obtain uniform green polyurethane beads. The prepared green polyurethane beads were irradiated with ultraviolet light for a few seconds and then turned off to observe the decay of the long afterglow. The beads did not have long afterglow luminescence performance after the ultraviolet light was turned off.

[0068] At room temperature, the materials prepared in Examples 1-4 and Comparative Examples 1-4 were subjected to phosphorescence spectrum and lifetime tests, and the results are shown in Table 2. The long afterglow luminescent polyurethane materials in Examples 1-4 have a lifetime of more than 1 s, and the luminescent position is stable at about 500nm / 540nm, while the polyurethane materials obtained in Comparative Examples 1, 3, and 4 have no phosphorescence lifetime and no characteristic phosphorescence emission position. The phosphorescence lifetime of the polyacrylate material obtained in Comparative Example 2 is less than 500ms, which is lower than that of the tetraacetylethylenediamine powder material, and the luminescent position is consistent with that of the tetraacetylethylenediamine powder material. It does not have the same red shift effect as the polyurethane material, and the polyacrylate material does not have the effect of extending the lifetime of tetraacetylethylenediamine.

[0069] Table 2

[0070]

[0071] Test example:

[0072] (1) Information Encryption

[0073] The luminescent polyurethane materials of Example 5 (disperse blue: disperse yellow: disperse red = 0:1:0 and 0:1:1) and the colored polyurethanes of Comparative Examples 3 and 4 were respectively made into letter shapes to form the words "QDU COLOR SCIENCE", wherein the yellow words "DOI" are the luminescent polyurethane materials obtained in Example 5 (disperse blue: disperse yellow: disperse red = 0:1:0), the orange-red words "URCE" are the luminescent polyurethane materials obtained in Example 5 (disperse blue: disperse yellow: disperse red = 0:1:1), the blue words "QCSC" are the polyurethane materials obtained in Comparative Example 3, and the green words "OLEN" are the polyurethane materials obtained in Comparative Example 4. Under visible light and ultraviolet light, all the information of "QDU COLOR SCIENCE" is displayed. Within 2 seconds after the ultraviolet light is turned off, only the words "DOI" and "URCE" in Example 5 are displayed. When the ultraviolet light is turned off for 4 seconds, only the three words "DOI" in Example 5 are displayed, which is the actual information, achieving the purpose of information encryption. The actual pictures of visible light irradiation, ultraviolet irradiation and long afterglow are as follows Figure 3 shown.

[0074] (2) Anti-counterfeiting performance

[0075] A logo is printed on the luminescent polyurethane material obtained in Example 5 (disperse blue: disperse yellow: disperse red = 1:1:0), and the clothing is irradiated with an ultraviolet lamp to present a complete clothing and logo pattern. When the ultraviolet lamp is turned off, only the logo pattern continues to glow, achieving the effect and purpose of multiple and high-end anti-counterfeiting of textiles; the actual pictures of visible light irradiation, ultraviolet irradiation and long afterglow are as follows Figure 4 shown.

[0076] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. An organic long afterglow luminescent material, characterized in that: The raw materials of the organic long afterglow luminescent material include phosphor tetraacetylethylenediamine and polyurethane; the amount of phosphor tetraacetylethylenediamine used is 0.5-15% of the mass of polyurethane.

2. A method for preparing the organic long afterglow luminescent material according to claim 1, characterized in that: The preparation method comprises the following steps: (1) mixing phosphor tetraacetylethylenediamine with a polyurethane solution to prepare a mixed solution; (2) injecting the mixed solution obtained in step (1) into a mold, drying and molding, and obtaining an organic long afterglow luminescent material.

3. The preparation method according to claim 2, characterized in that: In step (1), the solid content of the polyurethane solution is 20-40%.

4. The preparation method according to claim 2, characterized in that: In step (1), the polyurethane in the polyurethane solution is one or more of 88395AU from Bayer, Germany, 1065AU from Covestro, Germany, and HF-1070AP from Huafeng Group.

5. The preparation method according to claim 2, characterized in that: In step (1), the solvent of the polyurethane solution is one or more of acetone, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

6. The preparation method according to claim 2, characterized in that: In step (2), the drying and molding temperature is 25-120°C.

7. The organic long afterglow luminescent material according to claim 1, characterized in that: The raw materials of the organic long afterglow luminescent material also include disperse dyes; the amount of disperse dyes used is 0.01-1% of the mass of polyurethane.

8. The organic long afterglow luminescent material according to claim 7, characterized in that: The preparation method thereof comprises the following steps: (1) mixing phosphor tetraacetylethylenediamine with a polyurethane solution to prepare a mixed solution; (2) adding disperse dye to the mixed solution obtained in step (1), stirring evenly, to obtain a colored mixed solution; (3) injecting the colored mixed solution obtained in step (2) into a mold, drying and molding, and obtaining an organic long afterglow luminescent material.

9. The organic long afterglow luminescent material according to claim 8, characterized in that: In step (2), the disperse dye is one or more of red, yellow and blue disperse dyes.

10. An application of the organic long afterglow luminescent material according to any one of claims 1 or 7-8, characterized in that: Used to encrypt information or prepare anti-counterfeiting labels.