Cyan / blue light quantum confinement CsPbBr3 composite material as well as preparation method and application thereof
Through the post-synthetic tailoring and encapsulation method of amino-containing silane coupling agent and polymethylhydrogensiloxane, the stability and cost problems of cyan/blue light quantum confinement CsPbBr3 composite materials in the existing technology are solved, and high quantum efficiency is achieved. and stability, suitable for full spectrum lighting and optical communication fields.
Patent Information
- Application Number
- CN202411262157.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-09-10
AI Technical Summary
It is difficult to prepare cyan/blue light quantum confinement CsPbBr3 composite materials with high fluorescence quantum yield and high stability using existing technology, and the preparation process is costly and the material is unstable under polar molecules, heat and light stimulation.
Amino-containing silane coupling agent and polymethylhydrogensiloxane were used to prepare quantum-confined CsPbBr3 composite materials with adjustable fluorescence wavelength through post-synthetic tailoring and in-situ encapsulation methods, and the interaction between the silane coupling agent and the CsPbBr3 lattice was used. Tailored and protected nanoparticles through polymer network encapsulation, inhibiting self-aggregation and external environmental erosion.
Achieved the preparation of cyan/blue light quantum confinement CsPbBr3 composite materials with high quantum efficiency and stability at room temperature. The fluorescence wavelength is adjustable, the quantum yield remains above 80%, and the stability to polar solvents, heat and ultraviolet light is significant. promote.
Smart Images

Figure CN118772879A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of preparation of semiconductor optoelectronic materials, and specifically relates to a cyan / blue light quantum confined CsPbBr3 composite material with high fluorescence quantum yield and high stability, and a preparation method and application thereof. Background Art
[0002] All-inorganic perovskite nanocrystals (CsPbX3, X = Cl, Br, I) show great application potential in optoelectronic devices such as light-emitting diodes, solar cells, photodetectors, lasers, etc. due to their excellent optical properties, such as high photoluminescence quantum yield (PLQY), good emission purity, wide emission range, and low material cost.
[0003] At present, there are a large number of technical routes for the preparation of efficient and stable green or red fluorescent all-inorganic nanocrystals (such as CsPbBr3 and CsPbI3, etc.). However, the development of cyan / blue fluorescent perovskite nanocrystals is obviously lagging behind, and cyan / blue luminescent components are indispensable in full-spectrum lighting, optical communications, and full-color display. In the existing technology, there are two methods for preparing cyan / blue light perovskite nanocrystals: component engineering and dimension engineering. Component engineering mainly controls the mixed halide perovskite nanocrystals (CsPbCl X Br 3-X ) to achieve cyan / blue fluorescence, but Cl and Br elements will phase separate under electric field or light stimulation, resulting in spectral shift; the key to dimensional engineering is to reduce a certain dimension or overall size of CsPbBr3 nanocrystals to below their exciton Bohr radius to obtain quantum confined CsPbBr3 nanocrystals, fundamentally avoiding the spectral instability caused by phase separation. However, these quantum confined nanocrystals usually have a large surface area to volume ratio, so the defect density is high, the PLQY is low, and they are easy to aggregate, resulting in spectral red shift.
[0004] In order to achieve bright and stable cyan / blue fluorescence emission, an appropriate matrix should be selected to suppress the self-aggregation of quantum confined perovskite nanocrystals and protect them from environmental stimuli such as polar molecules, heat and light. Based on this, existing technical routes mostly use porous materials such as mesoporous silica (Angew. Chem. Int. Ed. 2018, 57, 8881), molecular sieves (Mater. Horiz., 2023, 10, 5079) and mesoporous alumina to in situ grow and stabilize quantum confined CsPbBr3. The independent nanospaces in the porous matrix can act as templates to limit and separate the growth of perovskite nanoparticles, thereby achieving the quantum confinement effect. However, these porous templates are usually prepared by high-temperature calcination (over 500 oC), which makes the cost of preparing quantum confined CsPbBr3 composite materials extremely high. In addition, the porous structure is difficult to resist the penetration of polar molecules for a long time, which is not conducive to the long-term stability of quantum confined CsPbBr3.
[0005] The present invention adopts amino silane coupling agent and polymethylhydrogensiloxane, and obtains a quantum confined CsPbBr3 composite material with adjustable fluorescence wavelength in the cyan and blue light regions, high quantum efficiency and high stability through post-synthesis tailoring and in-situ packaging. The composite material can be widely used in full-spectrum lighting, optical communication, full-color display and other fields. Summary of the invention
[0006] In order to overcome the above-mentioned shortcomings and deficiencies in the prior art, the present invention provides a cyan / blue light quantum confined CsPbBr3 composite material and a preparation method and application thereof.
[0007] The technical solution of the present invention is as follows:
[0008] A method for preparing a cyan / blue light quantum confined CsPbBr3 composite material comprises the following steps:
[0009] (1) synthesizing CsPbBr3 nanocrystals and dispersing them in an organic solvent to obtain a CsPbBr3 nanocrystal dispersion;
[0010] The organic solvent is selected from toluene, ethyl acetate, dichloromethane or n-hexane;
[0011] In the obtained CsPbBr3 nanocrystal dispersion, the mass fraction of CsPbBr3 nanocrystals is 1-2%, preferably 1-1.5%;
[0012] CsPbBr3 nanocrystals have green fluorescence and can be synthesized by known methods, such as high temperature hot injection method (Nano Lett., 2015, 15, 3692), ligand-assisted reprecipitation method (Adv. Funct. Mater., 2016, 26,2435) or emulsion synthesis method (ACS Appl. Mater., Interfaces 2015, 7, 28128);
[0013] (2) in an air environment and under stirring conditions, adding an amino silane coupling agent and polymethylhydrogensiloxane to the CsPbBr3 nanocrystal dispersion obtained in step (1), stirring for 0.5 to 2 h, and then centrifuging. The obtained precipitate is dispersed again in an organic solvent, and after a second centrifugation, the precipitate is collected and vacuum dried to obtain the cyan / blue light quantum confined CsPbBr3 composite material (powder);
[0014] The molar ratio of the amino-containing silane coupling agent to Pb in the CsPbBr3 nanocrystals is 20-80:1;
[0015] The volume ratio of polymethyl hydrogen siloxane to amino-containing silane coupling agent is 1 to 4:1;
[0016] The amino-containing silane coupling agent is selected from 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 2-aminoethylaminomethyltriethoxysilane, 3-(2-aminoethyl)-aminopropyltriethoxysilane, 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 11-aminoundecyltriethoxysilane, 4-anilinotriethoxysilane, preferably 3-aminopropyltriethoxysilane or 3-aminopropyltrimethoxysilane;
[0017] The ambient temperature and relative humidity of the continuous stirring environment are 10~40 o C, 20~80%, preferably 15~30 o C. 30~60%;
[0018] The definition of organic solvent is the same as in step (1);
[0019] During centrifugation, the speed is 3000~8000 rpm and the centrifugation time is 5~10 minutes;
[0020] Vacuum drying temperature 30~70 o C, time 2~10 h, preferably temperature 40~60 o C, time 4~6 h.
[0021] The invention relates to a cyan / blue light quantum confined CsPbBr3 composite material prepared by the preparation method.
[0022] The cyan / blue light quantum confined CsPbBr3 composite material of the present invention can be applied to full-spectrum lighting, optical communication, full-color display and other fields.
[0023] The technical principles of the present invention are as follows:
[0024] The present invention adopts a top-down strategy, first synthesizing CsPbBr3 nanocrystals, then introducing an amino-containing silane coupling agent into the CsPbBr3 nanocrystal dispersion, and utilizing its strong interaction with the CsPbBr3 lattice to "cut" the CsPbBr3 nanocrystals to reduce their size and achieve the quantum confinement effect; and the luminescent color can be regulated in the cyan and blue light regions by changing the molar ratio of the amino-containing silane coupling agent to Pb. At the same time, the terminal alkoxy of the silane coupling agent will undergo a hydrolysis reaction to form silanol under the drive of trace moisture in the solvent and air. The silanol reacts with hydrogen-containing silicone oil to form a polymer network in situ to separate the quantum confined CsPbBr3 nanoparticles from each other and inhibit their aggregation. At the same time, the polymer network plays a packaging role to block the external environment from corroding the quantum confined CsPbBr3.
[0025] The advantages and beneficial effects of the present invention are:
[0026] (1) The present invention does not require high temperature and special equipment, and can realize the preparation of quantum confined CsPbBr3 composite materials at room temperature and air environment, and the raw materials are common and easily available.
[0027] (2) The present invention uses amino-containing silane coupling agents to tailor the structure of green fluorescent CsPbBr3 nanocrystals. The fluorescence wavelength of the obtained quantum confined CsPbBr3 composite material can be arbitrarily adjusted in the cyan and blue light regions, and the emission line width is only 15nm. At the same time, the passivation effect of the amino-containing silane coupling agent on the quantum confined CsPbBr3 keeps its quantum yield above 80%.
[0028] (3) The present invention utilizes the cross-linking reaction of hydrogenated silicone oil and silane coupling agent to form a polymer network, and in situ encapsulates the quantum confined CsPbBr3 to significantly improve its stability to polar solvents, heat and ultraviolet light. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 : Fluorescence spectrum and physical picture of the quantum confined CsPbBr3 composite material prepared in Example 1.
[0030] Figure 2 : Fluorescence spectrum and physical picture of the quantum confined CsPbBr3 composite material prepared in Example 2.
[0031] Figure 3 : Fluorescence spectrum and physical picture of the quantum confined CsPbBr3 composite material prepared in Example 3.
[0032] Figure 4 : Fluorescence spectrum and physical picture of the quantum confined CsPbBr3 composite material prepared in Example 4.
[0033] Figure 5 : Fluorescence spectrum and physical picture of CsPbBr3 nanocrystals prepared in Comparative Example 1.
[0034] Figure 6 : Transmission electron microscopy images of the quantum confined CsPbBr3 composite material prepared in Example 3 and the CsPbBr3 nanocrystals prepared in Comparative Example 1.
[0035] Figure 7 : Changes in fluorescence intensity over time of the quantum confined CsPbBr3 composite material prepared in Example 3 and the CsPbBr3 nanocrystals prepared in Comparative Example 1 under polar solvent immersion (a), thermal aging (b) and ultraviolet illumination (c).
[0036] Figure 8: Actual picture of the composite material powder prepared in Comparative Example 2.
[0037] Fig. 9 : X-ray diffraction patterns of the composite materials prepared in Example 3 and Comparative Example 2. DETAILED DESCRIPTION
[0038] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.
[0039] Embodiment 1:
[0040] 1.47 g PbBr2, 10 mL oleic acid, 10 mL oleylamine and 40 mL 1-octadecene were added to a 100 mL three-necked flask and heated to 120 °C. o The reaction was carried out at 30 min and then the temperature was raised to 180 o C, quickly inject 2 mL of cesium oleate (11wt%, solvent is octadecene (ODE), the same below), react for 10 s, take it out, and cool it to 0 o C, place the reaction solution in a centrifuge tube, add 20 mL of ethyl acetate, centrifuge at 8000 rpm for 10 min, then disperse the precipitate in toluene, centrifuge again at 6000 rpm for 10 min, take the supernatant to obtain CsPbBr3 nanocrystal dispersion, dilute its concentration to 1.5wt% for later use.
[0041] Take 2 mL of the above CsPbBr3 nanocrystal dispersion, add 100 μL of 3-aminopropyltriethoxysilane and 200 μL of polymethylhydrogensiloxane in sequence under vigorous stirring, and o C and 50% humidity for 2 h, then the reaction solution was centrifuged at 5000 rpm for 10 min, the resulting precipitate was dispersed in toluene again, centrifuged a second time (5000 rpm, 10 min) and then centrifuged at 60 o C vacuum drying for 5 h to obtain quantum confined CsPbBr3 composite powder. Its fluorescence spectrum and physical figure are shown in Figure 1 As shown, the PLQY is 84%.
[0042] Embodiment 2:
[0043] Dissolve 0.04 g PbBr2 and 0.05 g CsBr in 2 mL DMF, add 200 μL oleic acid and 100 μL oleylamine, and mix evenly to form a precursor solution. Take 5 mL toluene, stir vigorously, quickly inject 200 μL of the precursor solution, then add 2 mL ethyl acetate, centrifuge at 9000 rpm for 9 min, and disperse the precipitate again in 5 mL toluene, centrifuge at 5000 rpm for 9 min, collect the supernatant, and obtain a CsPbBr3 nanocrystal dispersion, which is diluted to 1wt% for later use.
[0044] Take 2 mL of the above CsPbBr3 nanocrystal dispersion, add 250 μL of 3-(2-aminoethyl)-aminopropyltrimethoxysilane and 500 μL of polymethylhydrogensiloxane in sequence under vigorous stirring, and o C and 50% humidity for 2 h, then the reaction solution was centrifuged at 8000 rpm for 10 min, the resulting precipitate was dispersed in toluene again, centrifuged a second time (8000 rpm, 10 min) and then centrifuged at 50 o C vacuum drying for 8 h to obtain quantum confined CsPbBr3 composite powder. Its fluorescence spectrum and physical figure are shown in Figure 2 As shown, the PLQY is 82%.
[0045] Embodiment 3:
[0046] 1.47 g PbBr2, 10 mL oleic acid, 10 mL oleylamine and 40 mL 1-octadecene were added to a 100 mL three-necked flask and heated to 120 °C. o The reaction was carried out at 30 min and then the temperature was raised to 180 o C, quickly inject 4 mL of cesium oleate, react for 10 s, take it out, cool it to room temperature in an ice water bath, put the reaction solution in a centrifuge tube, add 20 mL of ethyl acetate, centrifuge at 8000 rpm for 10 min, then disperse the precipitate in dichloromethane, centrifuge it again at 6000 rpm in a centrifuge for 10 min, take the supernatant, obtain the CsPbBr3 nanocrystal dispersion, dilute its concentration to 2wt% for later use.
[0047] Take 2 mL of the above CsPbBr3 nanocrystal dispersion, add 300 μL of 3-aminopropyltriethoxysilane and 900 μL of polymethylhydrogensiloxane in sequence under vigorous stirring, and o C and 50% humidity for 2 h, then the reaction solution was centrifuged at 5000 rpm for 10 min, the resulting precipitate was dispersed in dichloromethane again, centrifuged a second time (5000 rpm, 10 min) and then centrifuged at 40o C vacuum drying for 6 h to obtain quantum confined CsPbBr3 composite material powder. Its fluorescence spectrum and physical figure are shown in Figure 3 As shown, the PLQY is 79%.
[0048] Embodiment 4:
[0049] Dissolve 0.06 g PbBr2 and 0.08 g CsBr in 4 mL DMF, add 300 μL oleic acid and 200 μL oleylamine, and mix evenly to form a precursor solution. Take 5 mL toluene, stir vigorously, quickly inject 250 μL of the precursor solution, then add 2 mL ethyl acetate, centrifuge at 9000 rpm for 9 min, and disperse the precipitate again in 5 mL toluene, centrifuge at 5000 rpm for 9 min, collect the supernatant, and obtain a CsPbBr3 nanocrystal dispersion, which is diluted to 1wt% for later use.
[0050] Take 2 mL of the above CsPbBr3 nanocrystal dispersion, add 350 μL of 3-aminopropyltrimethoxysilane and 700 μL of polymethylhydrogensiloxane in sequence under vigorous stirring, and o C and 70% humidity for 0.5 h, then the reaction solution was centrifuged at 7000 rpm for 10 min, the resulting precipitate was dispersed in toluene again, centrifuged a second time (7000 rpm, 10 min) and then centrifuged at 60 o C vacuum drying for 6 h to obtain quantum confined CsPbBr3 composite powder. Its fluorescence spectrum and physical picture are shown in Figure 4 As shown, the PLQY is 78%.
[0051] Comparative Example 1:
[0052] Referring to Example 3, the difference is that 3-aminopropyltriethoxysilane is not added, and the other preparation processes and conditions are the same as those of Example 3 to obtain CsPbBr3 nanocrystals, whose fluorescence spectrum and physical figure are shown in FIG. Figure 5 As shown, the PLQY is 86%.
[0053] Figure 6 Transmission electron microscope (TEM) images of the quantum confined CsPbBr3 composite material prepared in Example 3 and the CsPbBr3 nanocrystal prepared in Comparative Example 1. Figure 6 It can be seen that amino-containing silane coupling agents can "tailor" CsPbBr3 nanocrystals to reduce their size and achieve quantum confinement effect.
[0054] Figure 7 The quantum confined CsPbBr3 composite material prepared in Example 3 and the CsPbBr3 nanocrystals prepared in Comparative Example 1 were immersed in a polar solvent and thermally aged (70o C) and the change of fluorescence intensity under ultraviolet light conditions, Figure 7 It can be seen that the stability of quantum confined CsPbBr3 composite materials is significantly stronger than that of CsPbBr3 nanocrystals.
[0055] Comparative Example 2:
[0056] Referring to Example 3, the difference is that polymethylhydrogensiloxane is not added, and the other preparation processes and conditions are the same as those of Example 3. The actual picture of the obtained composite material powder is as follows: Figure 8 As shown, there is no obvious fluorescence emission under UV light excitation.
[0057] Fig. 9 The X-ray diffraction (XRD) diagrams of the composite materials prepared in Example 3 and Comparative Example 2 are shown in FIG. Fig. 9 It can be seen that the perovskite nanocrystals in the composite material prepared in Example 3 exist in the form of CsPbBr3, while in the composite material prepared in Comparative Example 2, CsPbBr3 is converted into Cs4PbBr6, indicating that the addition of polymethylhydrogensiloxane can inhibit the phase transition of quantum confined CsPbBr3.
Claims
1. A cyan / blue light quantum confinement CsPbBr 3 A method for preparing a composite material, It is characterized in that The steps include: (1) Synthesis of CsPbBr 3 Nanocrystals, dispersed in organic solvents, obtained CsPbBr 3 Nanocrystal dispersion; (2) In an air environment and under stirring conditions, add the CsPbBr obtained in step (1) to 3 Amino silane coupling agent and polymethylhydrogensiloxane are added to the nanocrystal dispersion, and the mixture is stirred for 0.5 to 2 h, and then centrifuged. The resulting precipitate is dispersed in an organic solvent again, and after a second centrifugation, the precipitate is collected and vacuum dried to obtain the cyan / blue light quantum confined CsPbBr 3 Composite materials.
2. The cyan / blue light quantum confined CsPbBr as claimed in claim 1 3 A method for preparing a composite material, It is characterized in that In step (1) or step (2), the organic solvent is selected from toluene, ethyl acetate, dichloromethane or n-hexane.
3. The cyan / blue light quantum confined CsPbBr as claimed in claim 1 3 A method for preparing a composite material, It is characterized in that Step (1) CsPbBr 3 In the nanocrystal dispersion, CsPbBr 3 The mass fraction of nanocrystals is 1~2%.
4. The cyan / blue light quantum confined CsPbBr as claimed in claim 1 3 A method for preparing a composite material, It is characterized in that In step (2), an aminosilane coupling agent and CsPbBr 3 The molar ratio of Pb in the nanocrystals is 20~80:
1.
5. The cyan / blue light quantum confinement CsPbBr as claimed in claim 1 3 A method for preparing a composite material, It is characterized in that In step (2), the volume ratio of polymethyl hydrogen siloxane to the amino-containing silane coupling agent is 1-4:
1.
6. The cyan / blue light quantum confined CsPbBr as claimed in claim 1 3 A method for preparing a composite material, It is characterized in that In step (2), the amino-containing silane coupling agent is selected from one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 2-aminoethylaminomethyltriethoxysilane, 3-(2-aminoethyl)-aminopropyltriethoxysilane, 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 11-aminoundecyltriethoxysilane and 4-anilinotriethoxysilane.
7. The cyan / blue light quantum confinement CsPbBr as claimed in claim 1 3 A method for preparing a composite material, It is characterized in that In step (2), during centrifugation, the rotation speed is 3000-8000 rpm and the centrifugation time is 5-10 minutes.
8. Cyan / blue light quantum confined CsPbBr prepared by the preparation method according to any one of claims 1 to 7 3 Composite materials.
9. The cyan / blue light quantum confined CsPbBr as claimed in claim 8 3 Application of composite materials in full-spectrum lighting, optical communications, and full-color display.
Citation Information
Patent Citations
Organic-inorganic hybrid perovskite quantum dot and preparation method thereof
CN106634961A
Preparation method for modified carbon quantum dot / silicone rubber fluorescent composite material
CN109181309A
Perovskite composite material and preparation method thereof
CN109837084A
Preparation method of super-amphiphobic fluorescent micro-nano pellets
CN110408214A
Red and green light perovskite quantum dot stable fluorescent powder based on SiO2 coating and preparation
CN110872510A