Mixed ceramic ball bearing lubricating grease and preparation method thereof

By increasing the base oil content of the grease and combining calcium sulfonate complex and polyurea calcium salt thickeners, the problem of lubrication failure of hybrid ceramic ball bearings in high-speed environments is solved, and the extreme pressure anti-wear performance and high-temperature life are enhanced, achieving Provide long-term effective lubrication protection.

CN118772933APending Publication Date: 2024-10-15WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410723556.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Hybrid ceramic ball bearings are prone to fatigue damage and increased contact stress due to lubrication failure in high-speed environments. The insufficient base oil content and thickener composite structure of existing greases lead to aging and reduced service life.

Method used

Increase the base oil content of the grease, and enhance the extreme pressure and anti-wear performance through the combination of complex calcium sulfonate thickener and polyurea calcium salt thickener to form a complex thickener system to meet the lubrication needs under high contact stress .

Benefits of technology

The base oil content and extreme pressure and anti-wear properties of the grease are improved, extending the service life of hybrid ceramic ball bearings at high temperatures and high speeds. It has excellent antioxidant, adhesion, water resistance and colloid stability, providing long-term lubrication Protect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772933A_ABST
    Figure CN118772933A_ABST
Patent Text Reader

Abstract

The invention provides mixed ceramic ball bearing lubricating grease which comprises the following raw materials in parts by weight: 68-80 parts of base oil, 21.2-31.7 parts of a composite thickening agent system formed by compounding a composite calcium sulfonate thickening agent and a polyurea calcium salt thickening agent, and 1-1.5 parts of an additive, and the mass ratio of the polyurea calcium salt thickening agent in the composite thickening agent system is 10-30%. A composite thickening agent system formed by compounding the composite calcium sulfonate thickening agent and the polyurea calcium salt thickening agent has good base oil thickening ability, the extreme pressure anti-wear performance and the oxidation resistance of the lubricating grease are enhanced, and the lubricating requirement of the mixed ceramic ball bearing under high contact stress can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lubricating grease, and in particular to a mixed ceramic ball bearing lubricating grease and a preparation method thereof. Background Art

[0002] Hybrid ceramic ball bearings are a new type of bearing developed from traditional metal steel bearings. They are suitable for high-speed light-load and ultra-high-speed light-load conditions, and have broad application prospects and huge economic benefits. Ceramic ball bearings can be divided into full ceramic ball bearings and hybrid ceramic ball bearings. The balls and inner and outer rings of full ceramic ball bearings are all made of ceramic materials. The high hardness, high brittleness and small thermal expansion coefficient make the rings not only difficult to process, but also easy to crack the rings due to the difference in thermal expansion and contraction when the bearings are installed in steel equipment. Hybrid ceramic ball bearings only have ceramic balls and inner and outer rings are made of bearing steel. Compared with ordinary steel ball bearings, hybrid ceramic balls have low density and light weight. The inertial centrifugal force and gyroscopic torque are greatly reduced when rotating at high speed, which enables them to be used in higher speed conditions. In addition, ceramic materials have excellent high-temperature performance and good rolling fatigue strength under high-temperature conditions.

[0003] A large number of tests have shown that in precision bearings working under high-speed conditions, the ball is the weakest part. About 70% of high-speed bearing failures are caused by fatigue damage to the ball to varying degrees. The elastic modulus of ceramic materials is larger than that of bearing steel materials. Under the same speed and load conditions, the contact area between the maximum load-bearing ball of the hybrid ceramic ball bearing and the inner and outer rings is smaller than the contact area between the maximum load-bearing rolling element of the steel bearing and the inner and outer rings, so the contact stress is higher. Under greater stress, the hybrid ceramic ball bearing is more prone to fatigue spalling. Lubrication failure has become the primary factor restricting the operating reliability and service life of ceramic ball bearings. However, there are few research reports on hybrid ceramic ball bearing greases. Therefore, it is of great significance to carry out performance research on hybrid ceramic ball bearing greases.

[0004] Composite calcium sulfonate grease is a new type of multi-effect grease with excellent properties of other composite soap-based greases, especially its excellent extreme pressure performance, which greatly improves the bearing capacity when used in hybrid ceramic bearings. However, its special thickener composite structure makes its soap content higher than that of common lithium-based and polyurea greases. Insufficient base oil content can easily lead to lubrication failure, especially under high-speed rotation conditions, which can easily cause excessive local temperature rise in the contact pair, leading to grease aging and thus reducing its service life. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the present invention provides a hybrid ceramic ball bearing grease and a preparation method thereof, which increases the base oil content of the grease and enhances the extreme pressure and anti-wear properties of the grease.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] In the first aspect, the present invention provides a hybrid ceramic ball bearing grease, comprising the following raw materials in parts by weight: 68 to 80 parts of base oil, 21.2 to 31.7 parts of a composite thickener system formed by a composite calcium sulfonate thickener and a polyurea calcium salt thickener, and 1 to 1.5 parts of an additive, wherein the mass proportion of the polyurea calcium salt thickener in the composite thickener system is 10% to 30%.

[0008] Furthermore, the composite thickener system comprises the following components in parts by weight: 10.1 to 20.3 parts of high base calcium sulfonate, 0.7 to 1.5 parts of a conversion agent, 0.9 to 2 parts of a fatty acid, 0.4 to 0.7 parts of a small molecule acid, 0.8 to 1.7 parts of calcium hydroxide, 1.1 to 4.2 parts of a diisocyanate, 0.5 to 1.6 parts of an organic diamine, 0.2 to 0.8 parts of an organic monoamine, and 0.2 to 0.8 parts of an acid anhydride; the high base calcium sulfonate, the conversion agent, the fatty acid, the small molecule acid and part of the calcium hydroxide are reacted to obtain a composite calcium sulfonate thickener; the diisocyanate, the organic monoamine, the organic diamine, the acid anhydride and part of the calcium hydroxide are reacted to obtain a polyurea calcium salt thickener.

[0009] Furthermore, the molar ratio of diisocyanate: diamine: monoamine is n+1: n: 1, wherein n is a positive integer, and the diisocyanate can be appropriately excessive during actual feeding, not exceeding 110% of the standard amount.

[0010] According to the above scheme, the total base value of the high base calcium sulfonate is 300-450 mgKOH / g

[0011] According to the above scheme, the conversion agent is one or more of low molecular alcohol, low molecular acid, and ethylene glycol monomethyl ether, the low molecular alcohol is one or more of methanol, ethanol, isopropanol, or n-butanol, and the low molecular acid is one or both of formic acid and acetic acid;

[0012] The fatty acid is selected from dodecyl hydroxystearic acid or stearic acid, preferably dodecyl hydroxystearic acid;

[0013] The small molecule acid is boric acid or a mixture of boric acid and other acids, wherein the other acids are selected from one or more of acetic acid, propionic acid, oxalic acid, succinic acid and oxalic acid. When the small molecule acid is a mixture of boric acid and other acids, the boric acid accounts for 60-80% of the small molecule acid.

[0014] According to the above scheme, the diisocyanate is diphenylmethane ~4,4~ diisocyanate or toluene diisocyanate, preferably diphenylmethane ~4,4~ diisocyanate;

[0015] The organic diamine is selected from one or more of p-phenylenediamine, o-phenylenediamine, 4,4-diphenylenediamine, ethylenediamine, propylenediamine, and 1,6-hexanediamine; the organic monoamine is selected from one or more of aniline, m-chloroaniline, p-chloroaniline, p-toluidine, dodecylamine, tetradecylamine, hexadecylamine, and octadecylamine, preferably octadecylamine, p-toluidine, or cyclohexylamine.

[0016] According to the above scheme, the acid anhydride is succinic anhydride.

[0017] According to the above scheme, the base oil is one or both of hydrogenated mineral oil and polyalphaolefin synthetic oil.

[0018] According to the above scheme, the additives include a friction reducer and an antioxidant in a mass ratio of (0.5-1): (0.5-1).

[0019] According to the above scheme, the friction reducing agent is selected from one or two of nano tungsten disulfide and molybdenum selenide; the antioxidant is selected from one or two of organic amine antioxidants and organic sulfides;

[0020] According to the above scheme, the purity of the nano tungsten disulfide is greater than 99.9%.

[0021] According to the above scheme, the organic amine antioxidant is selected from a mixture of one or more of dialkyl diphenylamine, nonyl diphenylamine and phenyl-α-naphthylamine, and the organic sulfide is phenothiazine.

[0022] In a second aspect, the present invention provides a method for preparing the above-mentioned hybrid ceramic ball bearing grease, and the hybrid ceramic ball bearing grease is prepared according to the raw materials of composite calcium sulfonate thickener and polyurea calcium salt thickener, base oil and additives.

[0023] According to the above scheme, the following steps are included:

[0024] S1. The first part of the base oil, the high base calcium sulfonate and the conversion agent are mixed and heated until the material thickens;

[0025] S2. Add small molecule acid, fatty acid and the first part of calcium hydroxide to carry out saponification reaction at a certain temperature, and heat and dehydrate after the reaction is completed;

[0026] S3. A second portion of the base oil, an organic diamine and a diisocyanate are added to react, and after the reaction is complete, a monoamine and a third portion of the base oil are added to react to form a polyurea intermediate;

[0027] S4. Heating and adding purified water to hydrolyze the polyurea intermediate, adding anhydride and the fourth part of the base oil to react;

[0028] S5. The remaining calcium hydroxide aqueous solution was added to react, and the remaining base oil was added after completion;

[0029] S6. After heating and dehydration, add additives, cool down and homogenize, and grind into fat.

[0030] According to the above scheme, the first part of base oil, the second part of base oil, the third part of base oil and the fourth part of base oil account for 42.1% to 59.3%, 8.2% to 20.3%, 6.2% to 12.5% ​​and 14.2% to 31.9% of the total mass of the base oil respectively, and the first part of calcium hydroxide accounts for 15% to 30% of the total mass of the calcium hydroxide.

[0031] According to the above scheme, the heating temperature in step S1 is 85-100°C, the reaction temperature in step S2 is 95-100°C, the reaction temperature in step S3 is 82-95°C, the temperature for hydrolysis of the polyurea intermediate in step S4 is 100-110°C, and the temperature for reaction of adding anhydride and base oil is 110-120°C.

[0032] The beneficial effects of the present invention are as follows: the present invention prepares a hybrid ceramic ball bearing grease by compounding a composite calcium sulfonate thickener and a polyurea calcium salt thickener, thereby increasing the base oil content of the grease, which is beneficial to ensuring sufficient lubrication of the hybrid ceramic ball bearing; the polyurea calcium salt thickener further enhances the extreme pressure and anti-wear performance of the composite calcium sulfonate grease, and can meet the lubrication requirements of the hybrid ceramic ball bearing under high contact stress; the grease has excellent antioxidant performance, slow aging speed at high temperature and high speed, and has a long high-temperature bearing life; in addition, the grease also has excellent adhesion, water resistance, colloid stability, high dropping point and other properties, and can play a long-term and effective lubrication and protection role for the hybrid ceramic ball bearing. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The fiber structure diagram of the thickener after removing the base oil from the hybrid ceramic ball bearing grease prepared in Example 1 of the present invention, the composite calcium sulfonate grease prepared in Comparative Example 2, and the polyurea calcium salt composite grease prepared in Comparative Example 3;

[0034] Figure 2 The thixotropic curves and thixotropic ring areas of the composite calcium sulfonate grease in Comparative Example 2 of the present invention and the hybrid ceramic ball bearing grease in Examples 1, 2 and 3;

[0035] Figure 3 The friction coefficient of the composite calcium sulfonate grease in Comparative Example 2 of the present invention and the hybrid ceramic ball bearing grease in Examples 1, 2 and 3 in a reciprocating friction test;

[0036] Figure 4 The SEM micrograph and EDS element distribution of the wear scar on the sample surface after the friction test;

[0037] Figure 5 The distribution of element contents on the wear scar on the sample surface after the friction test;

[0038] Figure 6 The invention discloses a synergistic mechanism of two thickeners in the mixed ceramic ball bearing grease prepared by the invention in terms of rheological properties and tribological properties. DETAILED DESCRIPTION

[0039] The principles and features of the present invention are described below in conjunction with the accompanying drawings and specific embodiments. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0040] It should be noted that in the description of the embodiments of the present application, the description of the term "some specific embodiments" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same implementation or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0041] In the present invention, the inventors obtained the hybrid ceramic ball bearing grease by replacing part of the composite calcium sulfonate thickener in the calcium sulfonate composite grease with a polyurea calcium salt thickener.

[0042] In the first aspect, the present invention provides a hybrid ceramic ball bearing grease, comprising the following raw materials in parts by weight: 68 to 80 parts of base oil, 21.2 to 31.7 parts of a composite thickener system formed by a composite calcium sulfonate thickener and a polyurea calcium salt thickener, and 1 to 1.5 parts of an additive, wherein the mass proportion of the polyurea calcium salt thickener in the composite thickener system is 10% to 30%.

[0043] The addition of polyurea calcium salt thickener will reduce the thermal decomposition temperature of grease. When the proportion of polyurea calcium salt thickener exceeds 30%, the thermal decomposition temperature will be greatly reduced.

[0044] The addition of polyurea calcium salt thickener can reduce the apparent viscosity of grease and improve its fluidity.

[0045] In some specific embodiments, the composite thickener system includes the following components in parts by weight: 10.1 to 20.3 parts of high base calcium sulfonate, 0.7 to 1.5 parts of conversion agent, 0.9 to 2 parts of fatty acid, 0.4 to 0.7 parts of small molecule acid, 0.8 to 1.7 parts of calcium hydroxide, 1.1 to 4.2 parts of diisocyanate, 0.5 to 1.6 parts of organic diamine, 0.2 to 0.8 parts of organic monoamine, and 0.2 to 0.8 parts of acid anhydride; the high base calcium sulfonate, conversion agent, fatty acid, small molecule acid and part of calcium hydroxide are reacted to obtain a composite calcium sulfonate thickener; the diisocyanate, organic monoamine, organic diamine, acid anhydride and part of calcium hydroxide are reacted to obtain a polyurea calcium salt thickener.

[0046] Furthermore, the molar ratio of diisocyanate: diamine: monoamine is n+1: n: 1, wherein n is a positive integer, and the diisocyanate can be appropriately excessive during actual feeding, not exceeding 110% of the standard amount.

[0047] In some specific embodiments, the conversion agent is one or more of low molecular alcohol, low molecular acid, and ethylene glycol monomethyl ether, the low molecular alcohol is one or more of methanol, ethanol, isopropanol, or n-butanol, and the low molecular acid is one or both of formic acid and acetic acid;

[0048] The fatty acid is selected from dodecyl hydroxystearic acid or stearic acid;

[0049] The small molecule acid is boric acid or a mixture of boric acid and other acids, wherein the other acids are selected from one or more of acetic acid, propionic acid, oxalic acid, succinic acid and oxalic acid. When the small molecule acid is a mixture of boric acid and other acids, the boric acid accounts for 60-80% of the small molecule acid.

[0050] In some specific embodiments, the diisocyanate is diphenylmethane-4,4-diisocyanate or toluene diisocyanate;

[0051] The organic diamine is selected from one or more of p-phenylenediamine, o-phenylenediamine, 4,4-diphenylenediamine, ethylenediamine, propylenediamine, and 1,6-hexanediamine; the organic monoamine is selected from one or more of aniline, m-chloroaniline, p-chloroaniline, p-toluidine, dodecylamine, tetradecylamine, hexadecylamine, and octadecylamine. According to the above scheme, the base oil is one or both of hydrogenated mineral oil and polyalphaolefin synthetic oil.

[0052] In some specific embodiments, the additive includes a friction reducer and an antioxidant in a mass ratio of (0.5-1):(0.5-1).

[0053] In a second aspect, the present invention provides a method for preparing the above-mentioned hybrid ceramic ball bearing grease, and the hybrid ceramic ball bearing grease is prepared according to the raw materials of composite calcium sulfonate thickener and polyurea calcium salt thickener, base oil and additives.

[0054] In some specific embodiments, the steps include:

[0055] S1. The first part of the base oil, the high base calcium sulfonate and the conversion agent are mixed and heated until the material thickens;

[0056] S2. Add small molecule acid, fatty acid and the first part of calcium hydroxide to carry out saponification reaction at a certain temperature, and heat and dehydrate after the reaction is completed;

[0057] S3. A second portion of the base oil, an organic diamine and a diisocyanate are added to react, and after the reaction is complete, a monoamine and a third portion of the base oil are added to react to form a polyurea intermediate;

[0058] S4. Heating and adding purified water to hydrolyze the polyurea intermediate, adding anhydride and the fourth part of the base oil to react;

[0059] S5. The remaining calcium hydroxide aqueous solution was added to react, and the remaining base oil was added after completion;

[0060] S6. After heating and dehydration, add additives, cool down and homogenize, and grind into fat.

[0061] In some specific embodiments, the first part of base oil, the second part of base oil, the third part of base oil and the fourth part of base oil account for 42.1% to 59.3%, 8.2% to 20.3%, 6.2% to 12.5% ​​and 14.2% to 31.9% of the total mass of the base oil, respectively, and the first part of calcium hydroxide accounts for 15% to 30% of the total mass of the calcium hydroxide.

[0062] In some specific embodiments, the heating temperature in step S1 is 85-100°C, the reaction temperature in step S2 is 95-100°C, the reaction temperature in step S3 is 82-95°C, the temperature for hydrolysis of the polyurea intermediate in step S4 is 100-110°C, and the temperature for reaction of adding anhydride and base oil is 110-120°C.

[0063] The preparation principle of polyurea calcium salt thickener is as follows:

[0064]

[0065] Where M is a metal element and x is the charge number carried by the metal ion M.

[0066] On the basis of the above-mentioned embodiments, the present invention provides the following specific examples to further illustrate the present invention. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. The experimental methods without specifying specific conditions in the following examples are usually based on the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by mass.

[0067] Example 1

[0068] The present embodiment provides a hybrid ceramic ball bearing grease (CSCPG) having the following formula: 71.8 parts of base oil; 19.2 parts of overbased calcium sulfonate; 1.4 parts of a converting agent; 1.9 parts of a fatty acid; 0.7 parts of a small molecule acid; 1.8 parts of calcium hydroxide; 1.3 parts of a diisocyanate; 0.5 parts of an organic diamine; 0.2 parts of an organic monoamine; 0.2 parts of an acid anhydride; 0.5 parts of a friction reducer; and 0.5 parts of an antioxidant.

[0069] Among them, the base oil is PAO16, the high alkalinity calcium sulfonate is a synthetic calcium sulfonate T106 with a total alkalinity of 400 mgKOH / g, the conversion agent is composed of acetic acid and ethylene glycol monomethyl ether in a mass ratio of 1:1, the fatty acid is dodecylhydroxystearic acid, the small molecule acid is boric acid, the diisocyanate is MDI, the organic diamine is diaminodiphenylmethane, the organic monoamine is octadecylamine, the friction reducer is nano-tungsten disulfide and molybdenum selenide in a mass ratio of 1:1, and the antioxidant is dialkyldiphenylamine and phenyl-α-naphthylamine in a mass ratio of 1:1.

[0070] The preparation method of the above grease composition comprises the following steps:

[0071] S1: Add overbased calcium sulfonate, 57.4 parts of base oil and a conversion agent into a reactor, and stir at 85-100° C. until the material becomes thick;

[0072] S2: heating to 95-100°C, adding small molecule acid, fatty acid and 1.6 parts of calcium hydroxide for saponification reaction, stirring at constant temperature for 60-90 minutes, and when the reaction system becomes thick, heating to 120-140°C for dehydration for 20-40 minutes;

[0073] S3: The temperature is adjusted to 82-95° C., 8.7 parts of base oil are added, the organic diamine and diisocyanate are reacted for 40-60 minutes, and the organic monoamine and 2.8 parts of base oil are added and the reaction is continued for 30-50 minutes to generate a polyurea intermediate;

[0074] S4: heating to 100-110° C., adding purified water to hydrolyze the polyurea intermediate, heating to 110-120° C., adding anhydride and 2.9 parts of base oil, and reacting for 60-80 minutes;

[0075] S5: Add 0.2 parts of calcium hydroxide aqueous solution and react for 40 to 60 minutes, then add the remaining base oil and stir thoroughly;

[0076] S6: heating to 120-140°C for dehydration for 60-90 minutes, then adding friction reducer and antioxidant, cooling and homogenizing, and grinding into fat.

[0077] Example 2

[0078] The present embodiment provides a hybrid ceramic ball bearing grease (CSCPG) having the following formula: 73 parts of base oil; 15.9 parts of overbased calcium sulfonate; 1.2 parts of a converting agent; 1.6 parts of a fatty acid; 0.6 parts of a small molecule acid; 1.5 parts of calcium hydroxide; 2.6 parts of a diisocyanate; 1.3 parts of an organic diamine; 1 part of an organic monoamine; 0.3 parts of an acid anhydride; 0.5 parts of a friction reducer; and 0.5 parts of an antioxidant.

[0079] Among them, the base oil is a mixture of 500SN and PAO16 in a mass ratio of 1:1, the high base number calcium sulfonate is a synthetic calcium sulfonate T106 with a total base number of 400 mgKOH / g, the conversion agent is composed of acetic acid, ethylene glycol monomethyl ether and water in a mass ratio of 1:2:4, the fatty acid is dodecylhydroxystearic acid, the small molecule acid is composed of boric acid and acetic acid in a mass ratio of 7:3, the diisocyanate is MDI, the organic diamine is diaminodiphenylmethane, the organic monoamine is octadecylamine, the friction reducer is nano tungsten disulfide, and the antioxidant is dialkyldiphenylamine and phenyl-α-naphthylamine in a mass ratio of 1:1.

[0080] The preparation method of the above grease composition comprises the following steps:

[0081] S1: Add overbased calcium sulfonate, 50.7 parts of base oil and a conversion agent into a reactor, and stir at 85-100° C. until the material becomes thick;

[0082] S2: heating to 95-100°C, adding small molecule acid, fatty acid and 1.3 parts of calcium hydroxide for saponification reaction, stirring at constant temperature for 60-90 minutes, and when the reaction system becomes thick, heating to 120-140°C for dehydration for 20-40 minutes;

[0083] S3: The temperature is adjusted to 82-95° C., 13.4 parts of base oil are added, the organic diamine and diisocyanate are reacted for 40-60 minutes, and the organic monoamine and 4.4 parts of base oil are added and the reaction is continued for 30-50 minutes to generate a polyurea intermediate;

[0084] S4: heating to 100-110° C., adding purified water to hydrolyze the polyurea intermediate, heating to 110-120° C., adding anhydride and 4.5 parts of base oil, and reacting for 60-80 minutes;

[0085] S5: Add 0.2 parts of calcium hydroxide aqueous solution and react for 40 to 60 minutes, then add the remaining base oil and stir thoroughly;

[0086] S6: Heat to 120-140℃ and dehydrate for 60-90 minutes, then add friction reducer and antioxidant, cool down and homogenize, grind into fat. The test results of typical physical and chemical performance indicators are shown in Table 1.

[0087] Example 3

[0088] The present embodiment provides a hybrid ceramic ball bearing grease (CSCPG) having the following formula: 77.3 parts of base oil; 11.8 parts of high base calcium sulfonate; 0.9 parts of conversion agent; 1.1 parts of fatty acid; 0.4 parts of small molecule acid; 1.4 parts of calcium hydroxide; 3.2 parts of diisocyanate; 1.2 parts of organic diamine; 0.6 parts of organic monoamine; 0.6 parts of acid anhydride; 0.5 parts of friction reducer; and 1 part of antioxidant.

[0089] The base oil is a mixture of hydrogenated mineral oil 500SN and polyalphaolefin synthetic oil PAO10 in a mass ratio of 1:1, the high base number calcium sulfonate is a synthetic calcium sulfonate T106 with a total base number of 400 mg KOH / g, the conversion agent is composed of acetic acid and ethylene glycol monomethyl ether in a mass ratio of 1:2, the fatty acid is dodecylhydroxystearic acid, the small molecule acid is composed of boric acid and acetic acid in a mass ratio of 7:3, the diisocyanate is MDI, the organic diamine is diaminodiphenylmethane, the organic monoamine is cyclohexylamine, the friction reducer is nano-tungsten disulfide and molybdenum selenide in a mass ratio of 1:1, and the antioxidant is dialkyldiphenylamine.

[0090] The preparation method of the above grease composition comprises the following steps:

[0091] S1: Add overbased calcium sulfonate, 45.7 parts of base oil and conversion agent into a reactor, and stir at 85-100° C. until the material becomes thick;

[0092] S2: heating to 95-100°C, adding small molecule acid, fatty acid and 1 part of calcium hydroxide for saponification reaction, stirring at constant temperature for 60-90 minutes, and when the reaction system becomes thick, heating to 120-140°C for dehydration for 20-40 minutes;

[0093] S3: The temperature is adjusted to 82-95° C., 19.1 parts of base oil are added, the organic diamine and diisocyanate are reacted for 40-60 minutes, and the monoamine and 6.2 parts of base oil are added and the reaction is continued for 30-50 minutes to generate a polyurea intermediate;

[0094] S4: heating to 100-110° C., adding purified water to hydrolyze the polyurea intermediate, heating to 110-120° C., adding anhydride and 6.3 parts of base oil, and reacting for 60-80 minutes;

[0095] S5: Add 0.4 parts of calcium hydroxide aqueous solution and react for 40 to 60 minutes, then add the remaining base oil and stir thoroughly;

[0096] S6: heating to 120-140°C for dehydration for 60-90 minutes, then adding friction reducer and antioxidant, cooling and homogenizing, and grinding into fat.

[0097] Comparative Example 1

[0098] This comparative example is selected from commercially available composite calcium sulfonate-based grease, which meets the requirements of No. 2 grease in GB / T 33585-2017 standard. The base oil is mineral oil. The test results of various typical physical and chemical performance indicators are shown in Table 1.

[0099] Comparative Example 2

[0100] This comparative example provides a composite calcium sulfonate grease (CSCG) having the following formula: 71.4 parts of base oil; 20.7 parts of high base calcium sulfonate; 1.8 parts of conversion agent; 2.4 parts of fatty acid; 0.9 parts of small molecule acid; 1.8 parts of calcium hydroxide; 0.5 parts of friction reducer; and 0.5 parts of antioxidant.

[0101] Among them, the base oil is a mixture of 500SN and PAO16 in a mass ratio of 1:1, the high alkalinity calcium sulfonate is a synthetic calcium sulfonate T106 with a total alkalinity of 400 mgKOH / g, the conversion agent is composed of acetic acid and ethylene glycol monomethyl ether in a mass ratio of 1:1, the fatty acid is dodecylhydroxystearic acid, the small molecule acid is boric acid, the friction reducer is nano tungsten disulfide, and the antioxidant is dialkyl diphenylamine and phenyl-α-naphthylamine in a mass ratio of 1:1.

[0102] The preparation method of the above grease composition comprises the following steps:

[0103] S1: Add overbased calcium sulfonate, 65.2 parts of base oil and conversion agent into a reactor, and stir at 85-100° C. until the material becomes thick;

[0104] S2: heating to 95-100°C, adding small molecule acid, fatty acid and 1.6 parts of calcium hydroxide for saponification reaction, stirring at constant temperature for 60-90 minutes, and when the reaction system becomes thick, heating to 120-140°C for dehydration for 20-40 minutes;

[0105] S3: Add 0.2 parts of calcium hydroxide aqueous solution and react for 40 to 60 minutes, then add the remaining base oil and stir thoroughly;

[0106] S4: heating to 120-140°C for dehydration for 60-90 minutes, then adding friction reducer and antioxidant, cooling and homogenizing, and grinding into fat.

[0107] Comparative Example 3

[0108] This comparative example provides a polyurea calcium salt composite grease, and the formula of the polyurea calcium salt composite grease is as follows: 79.5 parts of base oil; 9.2 parts of diisocyanate; 5.1 parts of organic diamine; 3.1 parts of organic monoamine; 1.3 parts of acid anhydride; 0.8 parts of calcium hydroxide; 0.5 parts of friction reducer; and 0.5 parts of antioxidant.

[0109] The base oil is a mixture of 500SN and PAO16 in a mass ratio of 1:1, the diisocyanate is MDI, the organic diamine is diaminodiphenylmethane, the organic monoamine is octadecylamine, the friction reducer is nano tungsten disulfide and molybdenum selenide in a mass ratio of 1:1, and the antioxidant is dialkyldiphenylamine and phenyl-α-naphthylamine in a mass ratio of 1:1.

[0110] The preparation method of the above grease composition comprises the following steps:

[0111] S1: Add diamine and 19.8 parts of base oil into a reactor, stir and dissolve the diamine at 82-95° C., add diisocyanate and 13.2 parts of base oil to react for 40-60 minutes, then add organic monoamine and 6.8 parts of base oil to continue reacting for 30-50 minutes to generate a polyurea intermediate;

[0112] S2: heating to 100-110° C., adding purified water to hydrolyze the polyurea intermediate, heating to 110-120° C., adding anhydride and 13.2 parts of base oil, and reacting for 60-80 minutes;

[0113] S3: Add calcium hydroxide aqueous solution and react for 40 to 60 minutes, then add the remaining base oil and stir thoroughly;

[0114] S4: heating to 120-140°C for dehydration for 60-90 minutes, then adding friction reducer and antioxidant, cooling and homogenizing, and grinding into fat.

[0115] Figure 1 The fiber structure diagrams of the thickeners after removing the base oil from the hybrid ceramic ball bearing grease prepared in Example 1, the composite calcium sulfonate grease prepared in Comparative Example 2, and the polyurea calcium salt composite grease prepared in Comparative Example 3 are respectively shown. It can be seen from the figure that the thickener of the composite calcium sulfonate grease exhibits a lamellar structure with a large surface area, and the lamellar layers are stacked disorderly to form a large number of pores, which can adsorb and store the base oil; the thickener of the polyurea calcium salt composite grease presents a dense rod-like or strip-like structure, which are entangled with each other to form a certain network structure, thereby adsorbing the base oil therein; and the thickener of the prepared hybrid ceramic ball bearing grease has both a lamellar structure with a large surface area and a rod-like structure that is agglomerated with each other. The thickeners of the two structures are intertwined to form a denser composite structure, which is conducive to locking the base oil more firmly therein.

[0116] Figure 2 The thixotropic curves and thixotropic ring areas of the composite calcium sulfonate grease in Comparative Example 2 and the hybrid ceramic ball bearing grease in Examples 1, 2 and 3 are shown. Thixotropy refers to a phenomenon in which the fiber structure is gradually destroyed under the action of shear force and can gradually recover after the external force is removed. Figure 2 a is the change of apparent viscosity of the four greases with shear rate under the segmented continuous shear mode. In the first stage of continuous shear, the apparent viscosity of the grease decreases significantly with the increase of shear rate. In the second stage, since the shear rate remains constant, the apparent viscosity of the grease remains basically unchanged. In the third stage, the apparent viscosity of the grease increases with the decrease of the shear rate, but the value is significantly smaller than the apparent viscosity at the same shear rate in the first stage, thus forming a closed area called a thixotropic ring, the size of which reflects the structural recovery ability of the grease after the soap fiber structure is destroyed. Figure 2 b is a comparison of the areas of the thixotropic rings of the four greases. It can be seen that the thixotropic ring area of ​​Comparative Example 2 is the largest, indicating that the energy required to destroy its structure is the largest, and the time required for structural recovery after the external force is removed is also the longest. The thixotropic ring areas of Examples 1-3 are all smaller than that of Comparative Example 2, and the higher the content of the polyurea composite thickener in the examples, the smaller the thixotropic ring area of ​​the grease, indicating that the addition of the polyurea composite thickener can improve the thixotropy of the composite calcium sulfonate grease and enhance its structural stability and shear resistance.

[0117] Figure 3 is the friction coefficient of the composite calcium sulfonate grease in Comparative Example 2 and the hybrid ceramic ball bearing grease in Examples 1, 2 and 3 in the reciprocating friction test, wherein 3a is the variation law of the friction coefficient over time. From the trend of the curve, it can be seen that the friction coefficient first increases to a certain peak value, then gradually decreases and finally stabilizes. Figure 3 b is the average value and standard deviation of the friction coefficient. It can be seen that the average friction coefficient of comparative example 2 is the largest, followed by the average friction coefficients of examples 1 and 2, which are 0.121 and 0.117 respectively, and the average friction coefficient of example 3 is the smallest, which is 0.112. This shows that the addition of polyurea composite thickener can reduce the friction coefficient of composite calcium sulfonate grease on the surface of GCr15 bearing steel, and the higher the content of polyurea composite thickener, the smaller the average friction coefficient, which can be reduced by up to 10.4% ((0.125-0.112) / 0.0125). The standard deviation of the friction coefficient shows a similar rule to the average value. The standard deviation of the friction coefficient of examples 1 to 3 is significantly lower than that of comparative example 2, indicating that the friction coefficient of examples 1 to 3 fluctuates less and the friction process is more stable.

[0118] Figure 4 The SEM micrographs and EDS element distribution of the wear marks on the sample surface after the friction test. From the micrographs, it can be more clearly seen that the surface wear of Comparative Example 2 is the most serious ( Figure 4 a), its surface not only has furrows and peeling pits, but also has a lot of scattered wear debris. The wear surface of Example 1 has obvious divisions ( Figure 4 e), only furrows and spalling pits were found in the narrower area in the middle. The wear scar surfaces of Examples 2 and 3 were relatively smooth ( Figure 4 i, 4m), no obvious peeling pits were found, but there were also differences between the two. First, there were tiny wear debris on the surface of Example 3, while there were none on the surface of Example 2. Second, the wear scar boundary of Example 3 was more obvious than that of Example 2, indicating that the deformation and wear of Example 3 were more serious than those of Example 2. Figure 4 j-41) and Example 3 ( Figure 4From the surface element distribution of the wear scar surface of Example 3, it can be found that the distribution of O and Ca elements on the wear scar surface shows a great correlation with the wear scar shape, that is, the content of the two elements on the wear surface is significantly higher than that on the non-wear surface, while there is no such phenomenon on the surface of Example 2.

[0119] Figure 5 The distribution of element content of the wear scar on the surface of the sample after the friction test. Figure 5 It can also be seen that the content of the two elements O and Ca in the wear surface of Example 3 is significantly higher than that in Example 2, indicating that more chemical reactions occurred on the wear surface of Example 3 to generate CaCO3 or CaO, which acted as solid lubricants between the friction pairs and provided positive tribological behavior. Therefore, the friction coefficient of Example 3 is the smallest, but more tribochemical reactions increase its wear amount, and the matrix of the wear surface is easier to fall off, thereby forming Figure 4 Surface wear debris shown in m.

[0120] Figure 6 The present invention discloses a synergistic mechanism of two thickeners in the mixed ceramic ball bearing grease prepared in the present invention in terms of rheological properties and tribological properties. The composite calcium sulfonate thickener and the polyurea calcium salt thickener have a significant effect on the rheological properties and tribological properties of the grease after being combined. Figure 6 Figure a shows the molecular structure of high-base calcium sulfonate, which contains a short polar group and a long hydrophobic group. The polar group is a metal salt compound of an organic acid, and the hydrophobic group is an oil-soluble alkyl chain. During the thickening process of the grease, the alkyl chain can dissolve in the base oil, so that the three-dimensional structure of calcium carbonate wrapped in the calcium sulfonate can be dispersed in the base oil. However, the alkyl chain and the base oil are linked by van der Waals force, which is a weak interaction force. Therefore, in order to form a stable colloidal dispersion system, the structural skeleton of the thickener must have sufficient strength. Figure 1 It can be seen from a that the composite calcium sulfonate thickener fiber presents a lamellar structure that is not easy to store oil. Therefore, in the thickening process of grease, the lamellar thickener must be densely and staggeredly stacked to form a stable three-dimensional structure, such as Figure 6 As shown in Fig. e, the rod-shaped polyurea calcium salt thickener itself has a certain structural strength and oil storage capacity. It can fill the aforementioned oil storage pores, thereby providing structural support for the new thickener system and reducing the density of the composite calcium sulfonate thickener layer. Therefore, the new thickener system has less resistance to overcome when deformed by external force, that is, the structural strength of the grease is weakened, its fluidity is better, and a larger strain is generated under a smaller shear stress ( Figure 6 d, 6e). As for the reason why the composite calcium sulfonate thickener and polyurea calcium salt can be stably combined, Figure 6 b and 6c, where Figure 6b shows the molecular structure of calcium sulfonate, where R is the aforementioned oily alkyl chain, and polyurea calcium salt composite thickener is added to the composite calcium sulfonate thickener, and the urea molecule containing carboxyl ( Figure 6 c) It shares a calcium ion with calcium sulfonate, which provides conditions for the combination of polyurea calcium salt composite thickener and composite calcium sulfonate thickener. The interaction between calcium ions and hydroxyl groups in the new thickener system is a strong interaction, which will break when subjected to continuous shear, and can recover quickly after the external force is removed. This is also the reason why the hybrid ceramic ball bearing grease of the present invention has better thixotropic properties than the composite calcium sulfonate grease.

[0121] Table 1 shows the test results of typical physical and chemical performance indicators of the embodiments and comparative examples.

[0122] Table 1

[0123]

[0124] By comparing the typical physical and chemical performance indicators of the embodiments and the comparative examples, it can be seen that the raw material components of the grease composition provided by the present invention can cooperate with each other and work synergistically with each other, the synthetic quality is stable, and the advantages of the composite calcium sulfonate thickener and the polyurea calcium salt thickener are integrated. It has excellent extreme pressure and anti-wear properties and a long high-temperature bearing life, as well as excellent mechanical stability, colloidal stability and water resistance.

[0125] The grease contains both a composite calcium sulfonate thickener and a polyurea calcium salt thickener, which effectively reduces the proportion of calcium sulfonate soap compared with traditional composite calcium sulfonate-based greases, and a higher base oil content is conducive to ensuring sufficient lubrication of hybrid ceramic ball bearings; the polyurea calcium salt thickener further enhances the extreme pressure and anti-wear properties of the composite calcium sulfonate grease, and can meet the lubrication requirements of hybrid ceramic ball bearings under high contact stress; the grease has excellent antioxidant properties, slow aging speed at high temperature and high speed, and has a longer high-temperature bearing life; in addition, the grease also has excellent adhesion, water resistance, colloid stability, high dropping point and other properties, and can provide long-term and effective lubrication and protection for hybrid ceramic ball bearings.

[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A hybrid ceramic ball bearing grease, characterized in that: The invention comprises the following raw materials in parts by weight: 68 to 80 parts of base oil, 21.2 to 31.7 parts of a composite thickener system formed by a composite calcium sulfonate thickener and a polyurea calcium salt thickener, and 1 to 1.5 parts of an additive, wherein the mass proportion of the polyurea calcium salt thickener in the composite thickener system is 10% to 30%.

2. The hybrid ceramic ball bearing grease according to claim 1, characterized in that: The composite thickener system comprises the following components in parts by weight: 10.1-20.3 parts of high base calcium sulfonate, 0.7-1.5 parts of a conversion agent, 0.9-2 parts of a fatty acid, 0.4-0.7 parts of a small molecule acid, 0.8-1.7 parts of calcium hydroxide, 1.1-4.2 parts of a diisocyanate, 0.5-1.6 parts of an organic diamine, 0.2-0.8 parts of an organic monoamine, and 0.2-0.8 parts of an acid anhydride; the high base calcium sulfonate, the conversion agent, the fatty acid, the small molecule acid and part of the calcium hydroxide are reacted to obtain a composite calcium sulfonate thickener; the diisocyanate, the organic monoamine, the organic diamine, the acid anhydride and part of the calcium hydroxide are reacted to obtain a polyurea calcium salt thickener.

3. The hybrid ceramic ball bearing grease according to claim 2, characterized in that: The conversion agent is one or more of low molecular alcohol, low molecular acid, and ethylene glycol monomethyl ether, the low molecular alcohol is one or more of methanol, ethanol, isopropanol, or n-butanol, and the low molecular acid is one or both of formic acid and acetic acid; The fatty acid is selected from dodecyl hydroxystearic acid or stearic acid; The small molecule acid is boric acid or a mixture of boric acid and other acids, wherein the other acids are selected from one or more of acetic acid, propionic acid, oxalic acid, succinic acid and oxalic acid. When the small molecule acid is a mixture of boric acid and other acids, the boric acid accounts for 60-80% of the small molecule acid.

4. The hybrid ceramic ball bearing grease according to claim 2, characterized in that: The diisocyanate is diphenylmethane-4,4-diisocyanate or toluene diisocyanate; The organic diamine is selected from one or more of p-phenylenediamine, o-phenylenediamine, 4,4-diphenylenediamine, ethylenediamine, propylenediamine, and 1,6-hexanediamine; The organic monoamine is selected from one or more of aniline, m-chloroaniline, p-chloroaniline, p-toluidine, dodecylamine, tetradecylamine, hexadecylamine and octadecylamine.

5. The hybrid ceramic ball bearing grease according to any one of claims 1 to 4, characterized in that: The base oil is one or both of hydrogenated mineral oil and polyalphaolefin synthetic oil.

6. The hybrid ceramic ball bearing grease according to any one of claims 1 to 4, characterized in that: The additives include a friction reducer and an antioxidant in a mass ratio of (0.5-1):(0.5-1).

7. The method for preparing a hybrid ceramic ball bearing grease according to any one of claims 1 to 6, characterized in that: The mixed ceramic ball bearing grease is prepared according to the raw materials of the composite calcium sulfonate thickener and the polyurea calcium salt thickener, the base oil and the additives.

8. The method for preparing the hybrid ceramic ball bearing grease according to claim 7, characterized in that: The steps include: S1. The first part of the base oil, the high base calcium sulfonate and the conversion agent are mixed and heated until the material thickens; S2. Add small molecule acid, fatty acid and the first part of calcium hydroxide to carry out saponification reaction at a certain temperature, and heat and dehydrate after the reaction is completed; S3. A second portion of the base oil, an organic diamine and a diisocyanate are added to react, and after the reaction is complete, a monoamine and a third portion of the base oil are added to react to form a polyurea intermediate; S4. Heating and adding purified water to hydrolyze the polyurea intermediate, adding anhydride and the fourth part of the base oil to react; S5. The remaining calcium hydroxide aqueous solution was added to react, and the remaining base oil was added after completion; S6. After heating and dehydration, add additives, cool down and homogenize, and grind into fat.

9. The method for preparing hybrid ceramic ball bearing grease according to claim 8, characterized in that: The first part of base oil, the second part of base oil, the third part of base oil and the fourth part of base oil account for 42.1% to 59.3%, 8.2% to 20.3%, 6.2% to 12.5% ​​and 14.2% to 31.9% of the total mass of the base oil respectively, and the first part of calcium hydroxide accounts for 15% to 30% of the total mass of the calcium hydroxide.

10. The method for preparing hybrid ceramic ball bearing grease according to claim 8, characterized in that: In step S1, the temperature is heated to 85-100°C, in step S2, the reaction temperature is 95-100°C, in step S3, the reaction temperature is 82-95°C, in step S4, the temperature for hydrolysis of the polyurea intermediate is 100-110°C, and the temperature for reaction of adding anhydride and base oil is 110-120°C.