Construction method of large-thickness gradient nanostructure on surface of high-strength steel
The austenite layer is formed through high-frequency induction heating and shot peening, and then ultrasonic rolling is used to prepare large-thickness gradient nanostructures, which solves the problems of poor cold plastic deformation ability of high-strength steel and limited thickness of gradient nanostructures, which significantly The strengthening effect and fatigue performance of the material are improved.
Patent Information
- Application Number
- CN202410754430.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
High-strength steel has poor cold plastic deformation ability, it is difficult to strengthen surface deformation, and the thickness of gradient nanostructures is limited, which makes it prone to fracture failure in harsh service environments, affecting equipment safety.
High-frequency induction heating is used to assist shot peening to form an austenite layer, and ultrasonic rolling treatment is used to prepare a large thickness gradient nanostructure, which increases the degree of surface hardening and residual compressive stress, and improves the material strengthening effect.
It significantly increases the thickness and hardening degree of the surface gradient nanostructure of high-strength steel, enhances the mechanical properties of the material, improves the fatigue performance and surface finishing effect, and makes up for the shortcomings of traditional methods.
Smart Images

Figure CN118773403A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for constructing a high-strength steel surface large-thickness gradient nanostructure, belonging to the technical field of gradient nanomaterials. Background Art
[0002] Gradient nanostructure refers to a material whose grain size changes in a gradient from the outside to the inside, including nanocrystals, ultrafine grains, deformed grains, and coarse-grained matrix from the surface to the inside. In this structure, there is no obvious interface between grains of different sizes, which is not easy to cause peeling, and the original chemical composition of the material is maintained during preparation, avoiding the introduction of impurities. Since the grain size is distributed in a gradient, the corresponding material strength and hardness also show a gradient distribution, and the nanocrystalline layer on the surface can effectively prevent the initiation of fatigue cracks due to its high strength and hardness, while the internal coarse-grained matrix can slow down the expansion of fatigue cracks due to its good plasticity. Therefore, constructing a gradient nanostructure on the surface of the material can effectively enhance the mechanical properties of the material, and increasing the thickness of the surface deformation layer of the gradient nanostructured material is crucial to improving the strengthening effect.
[0003] High-strength steel is a type of alloy steel used to manufacture structural parts that withstand higher stresses. Over the years, high-strength steel has been widely used in key load-bearing components in various industrial fields such as aerospace, metallurgy, mining, and national defense. The service environment of high-strength steel load-bearing components is usually relatively harsh, and fracture failure behavior often occurs, which seriously threatens the safe use of equipment and urgently needs to be surface strengthened. However, the high strength, high hardness and high deformation resistance of high-strength steel lead to its poor cold plastic deformation ability. Therefore, the thickness and hardening degree of the gradient nanostructure obtained on its surface by traditional surface deformation strengthening treatment are limited, and the surface strengthening effect is not obvious.
[0004] Under the premise of not affecting the matrix, the present invention uses high-frequency induction heating to austenitize the 1-2mm structure of the surface layer of high-strength steel, and immediately performs shot peening on the austenite layer to obtain a deeper gradient nanostructure, while further improving the hardening degree of the gradient nanostructure, increasing the range and amplitude of the compressive stress, and obtaining a better strengthening effect. In addition, ultrasonic rolling treatment after induction heating-assisted shot peening can effectively reduce the surface roughness of the material, improve the surface quality of the material, achieve surface finishing effect, increase the thickness of the surface gradient nanostructure, and enhance the surface strengthening effect. Summary of the invention
[0005] In view of the current situation that key load-bearing components of high-strength steel are in urgent need of surface strengthening, the present invention provides a method for constructing a high-strength steel surface high-thickness gradient nanostructure. The present invention solves the problems of poor cold plastic deformation ability of high-strength steel, great difficulty in surface deformation strengthening, and limited thickness of gradient nanostructure. The method first performs induction heating assisted shot peening treatment on the surface of high-strength steel load-bearing components through induction heating equipment and shot peening machine, and then performs ultrasonic rolling treatment on the components after induction heating assisted shot peening treatment to prepare a large thickness gradient nanostructure, achieving a significant strengthening effect.
[0006] The present invention is achieved through the following technical solutions.
[0007] A method for constructing a high-strength steel surface nanostructure with a large thickness gradient, the specific steps of which include:
[0008] S1: Process the surface of high-strength steel to make the surface roughness Ra6μm or less;
[0009] S2: The high-strength steel processed in S1 is subjected to induction heating assisted shot peening treatment;
[0010] S3: The high-strength steel treated by induction heating assisted shot peening in S2 is subjected to ultrasonic rolling treatment to obtain high-strength steel with a large thickness gradient nanostructure on the surface.
[0011] The specific process of S2 is:
[0012] S21: Preheat the high-strength steel processed by S1 to 230℃ and keep it warm for 3 minutes to avoid surface hardening after high-frequency heating and ensure that the surface maintains austenite during shot peening;
[0013] S22: Turn on induction heating, control the current frequency to 300kHz, heating time to 7s, and heat to A c1 The surface of high-strength steel material is instantly austenitized within 1-2mm depth.
[0014] S23: Shot peening treatment, adjust the spray gun so that the shot spray direction is perpendicular to the high-strength steel treated surface after S22 induction heating, and perform shot peening treatment.
[0015] The shot peening step in S23 includes: the shot particles are 0.2mm-1.5mm steel shot or ceramic shot, the air pressure is 0.4-0.8MPa, the distance between the nozzle and the material surface is controlled at 5cm-10cm, and the shot peening coverage is controlled at 100%-300%.
[0016] The S3 ultrasonic rolling treatment step comprises:
[0017] S31: The surface of the high-strength steel after S2 induction heating assisted shot peening is perpendicular to the direction of action of the rolling tool head, and the high-strength steel begins to rotate;
[0018] S32: Turn on the ultrasonic rolling equipment and use the ultrasonic rolling tool head to perform multiple ultrasonic rolling treatments along the axial direction of the component to make the surface roughness of the high-strength steel less than Ra0.1μm.
[0019] The steps in S32 include: the ultrasonic rolling tool head is a hard alloy sphere with a diameter of 2mm to 14mm, the relevant parameters of the ultrasonic rolling treatment are: static pressure 0 to 1500N, ultrasonic amplitude 1 to 20μm, ultrasonic frequency 20 to 40kHz, spindle speed 100 to 400r / min, feed speed 0.01 to 0.1mm / r, and the number of ultrasonic rolling treatment passes is 1 to 3 times.
[0020] The enhancement effect is improved mainly due to the following reasons:
[0021] 1. After the sample is preheated, high-frequency heating can austenitize the surface 1-2 mm structure and maintain the austenite state during the shot peening process. Shot peening of austenite structure with good plasticity can produce more severe plastic deformation and obtain a thicker gradient nanostructure.
[0022] 2. Shot peening will introduce residual compressive stress on the surface of the material, and when the austenite on the surface of the material is cooled below the martensite phase transition temperature, the austenite phase transforms to the martensite phase, the specific volume increases, and the volume expands, further introducing residual compressive stress on the surface.
[0023] 3. Ultrasonic rolling treatment can effectively reduce the surface roughness of the material, improve the surface quality of the material, and make the surface of the material undergo plastic deformation again, increase the thickness of the gradient nanostructure, and further enhance the strengthening effect.
[0024] The beneficial effects of the present invention are:
[0025] The present invention creatively uses high-frequency induction heating and shot peening to treat high-strength steel, first obtaining an austenitized surface layer on the surface of the high-strength steel, and then constructing a large thickness gradient nanostructure through shot peening, and obtaining a higher level of residual compressive stress, and then achieving a smooth effect through ultrasonic rolling treatment, and further increasing the thickness of the gradient nanostructure. This method makes up for the shortcomings of large surface deformation resistance, limited thickness of gradient nanostructure, and low residual compressive stress level, and achieves a significant strengthening effect by increasing the thickness of the gradient nanostructure on the surface of high-strength steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the method for constructing a high-strength steel surface nanostructure with a large thickness gradient according to the present invention;
[0027] Figure 2 This is the metallographic structure diagram of the surface layer of the original sample of 45CrNiMoVA steel in Comparative Example 1 of the present invention;
[0028] Figure 3 This is the metallographic structure diagram of the surface layer of the 45CrNiMoVA steel shot peening sample in Comparative Example 2 of the present invention;
[0029] Figure 4 This is the metallographic structure diagram of the surface layer of the 45CrNiMoVA steel ordinary shot peening + ultrasonic rolling sample in Comparative Example 3 of the present invention;
[0030] Figure 5 is the metallographic structure diagram of the surface layer of 45CrNiMoVA steel after being treated by the method in Example 1 of the present invention;
[0031] Figure 6 It is the surface microhardness distribution diagram of the original sample of 45CrNiMoVA steel in comparative example 1 of the present invention, the shot peening sample in comparative example 2 and the 45CrNiMoVA steel treated by the method in embodiment 1. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0033] Example 1
[0034] like Figure 1 As shown, the method for constructing a high-strength steel surface large thickness gradient nanostructure comprises the following specific steps:
[0035] S1: Process the surface of high-strength steel to make the surface roughness Ra6μm or less;
[0036] S2: The high-strength steel (Φ5×50mm 45CrNiMoVA steel) processed by S1 is subjected to induction heating assisted shot peening treatment; the specific process is as follows:
[0037] S21: Preheat the high-strength steel processed by S1 to 230℃ and keep it warm for 3 minutes to avoid surface hardening after high-frequency heating and ensure that the surface maintains austenite during shot peening;
[0038] S22: Turn on induction heating, control the current frequency to 300kHz, heating time to 7s, and heat to A c1 The surface of high-strength steel material is instantly austenitized within 1-2mm depth.
[0039] S23: Shot peening treatment, adjust the spray gun so that the shot spray direction is perpendicular to the high-strength steel treated surface after S22 induction heating, and perform shot peening treatment. The shot peening process is as follows: the shot is 0.8mm steel shot, the air pressure is 0.8MPa, the distance between the nozzle and the material surface is controlled at 5cm, and the shot peening coverage is controlled at 100%; the rotation speed of the high-strength steel is 110r / min;
[0040] S3: The high-strength steel treated by induction heating assisted shot peening in S2 is subjected to ultrasonic rolling treatment to obtain a high-strength steel with a large thickness gradient nanostructure on the surface. The ultrasonic rolling treatment process is as follows:
[0041] S31: The surface of the high-strength steel after S2 induction heating assisted shot peening is perpendicular to the direction of action of the rolling tool head, and the high-strength steel begins to rotate;
[0042] S32: Turn on the ultrasonic rolling equipment, and use the ultrasonic rolling tool head to perform multiple ultrasonic rolling treatments along the axial direction of the component to make the surface roughness of the high-strength steel less than Ra0.1μm; the ultrasonic rolling tool head is a cemented carbide sphere with a diameter of 4mm, and the relevant parameters of the ultrasonic rolling treatment are: static pressure 300N, ultrasonic amplitude 3μm, ultrasonic frequency 27kHz, spindle speed 110r / min, feed speed 0.08mm / r, the number of ultrasonic rolling treatments is 3 times, and the rotation speed of the high-strength steel is 110r / min.
[0043] Comparative Example 1
[0044] 45CrNiMoVA steel with a size of Φ5×50 mm was selected and the same turning process as step S1 of Example 1 was adopted to obtain a smooth machined surface with a surface roughness not exceeding Ra6 μm, which was used as the original sample of 45CrNiMoVA steel.
[0045] Comparative Example 2
[0046] A 45CrNiMoVA steel with a size of Φ5×50 mm was selected as a 45CrNiMoVA steel shot peening sample, and the same S1 and S2 processing steps as in Example 1 were adopted, but the ultrasonic rolling treatment in S3 was not performed.
[0047] Comparative Example 3
[0048] The 45CrNiMoVA steel with a size of Φ5×50mm is treated by ordinary shot peening combined with ultrasonic rolling:
[0049] S1: Process the surface of high-strength steel to make the surface roughness Ra6μm or less;
[0050] S2: Ordinary shot peening: Adjust the spray gun so that the shot spray direction is perpendicular to the high-strength steel treatment surface, and perform shot peening at room temperature. The shot peening process is as follows: the shot is 0.8mm steel shot, the air pressure is 0.8MPa, the distance between the nozzle and the material surface is controlled at 5cm, and the shot peening coverage is controlled at 100%; the rotation speed of the high-strength steel is 110r / min;
[0051] S3: The high-strength steel after ordinary shot peening was subjected to ultrasonic rolling treatment, wherein the ultrasonic rolling tool head was a cemented carbide sphere with a diameter of 4 mm, and the relevant parameters of the ultrasonic rolling treatment were: static pressure 300 N, ultrasonic amplitude 3 μm, ultrasonic frequency 27 kHz, spindle speed 110 r / min, feed speed 0.08 mm / r, ultrasonic rolling treatment passes 3 times, and the rotation speed of the high-strength steel was 110 r / min; finally, only high-strength steel with a strain layer thickness of 200 μm was obtained.
[0052] The components obtained by processing Example 1 and Comparative Example 1 were subjected to the following tests:
[0053] 1. Surface metallographic structure
[0054] The surface metallographic structures of the original samples, shot peening samples and samples treated by this method were observed. Figure 2 , 3 As shown in Figure 4, the surface tissue of the untreated sample is evenly distributed, and there is no obvious difference between the surface and the core. After induction heating assisted shot peening, a "white layer" of about 10μm can be generated on the surface of the material, mainly because the shot peening hits the surface of the material, causing the surface grains of the material to be refined. And it can be seen from the metallographic structure that induction heating assisted shot peening will increase the surface roughness of the material. However, after treatment by this method, the surface of the material produces more serious plastic deformation, the surface grains become small and narrow, and a gradient nanostructure of about 200μm is prepared on the surface. In addition, it can be seen that the craters introduced by shot peening are eliminated after ultrasonic rolling treatment, achieving the effect of "cutting peaks and filling valleys" and improving the surface quality of the material.
[0055] 2. Microhardness
[0056] The surface microhardness of the original sample, shot peened sample and sample treated by this method was tested. Compared with the original sample (Comparative Example 1), the surface microhardness of each sample after treatment was improved to varying degrees. In addition, compared with the shot peened sample (Comparative Example 2), the surface microhardness of the sample treated by this method (Example 1) was higher, the work hardening effect was more obvious, and the depth of the hardened layer was deeper, such as Figure 5 As shown in the figure, the depth of the gradient nanostructure obtained by the present invention is much higher than that of the samples processed by conventional ultrasonic rolling, shot peening or a simple combination of the two methods. The strain layer thickness of the sample is 400 μm. Compared with the high-strength steel with a strain layer thickness of 200 μm in Comparative Example 3, the strain layer thickness obtained by the present invention is much higher than the simple combination thickness of the two methods, which is expected to further significantly improve the fatigue performance of the component.
[0057] 3. Residual stress
[0058] The surface layer of the sample was stripped by electrolytic corrosion method, and the residual stress at a depth of 100 μm was measured. It was found that the residual stresses of the three samples in Example 1, Comparative Example 2 and Comparative Example 1 were -812±43 MPa, -762±58 MPa, and 50±11 MPa, respectively. It can be seen that shot peening of the surface austenite can obtain higher residual compressive stress, which is conducive to obtaining better fatigue strength.
[0059] In summary, after the treatment of the present invention, a gradient nanostructure with a large thickness can be constructed on the surface of high-strength steel, achieving a significant strengthening effect. This is mainly because the sample is preheated and subjected to high-frequency heating, which can austenitize the surface 1-2mm structure and maintain the austenite state during the shot peening process. Shot peening of austenite structures with good plasticity can produce more severe plastic deformation, and the thickness of the obtained gradient nanostructure far exceeds that of other methods. Moreover, ultrasonic rolling treatment as a subsequent treatment can reduce surface roughness, improve surface quality, and cause the material surface to plastically deform again, further increasing the strength of the gradient nanostructure. The method for constructing a high-thickness gradient nanostructure on the surface of high-strength steel provided by the present invention has a wide range of material applications.
[0060] Example 2
[0061] like Figure 1 As shown, the method for constructing a high-strength steel surface large thickness gradient nanostructure comprises the following specific steps:
[0062] S1: Process the surface of high-strength steel to make the surface roughness Ra6μm or less;
[0063] S2: The high-strength steel (Φ5×50mm 45CrNiMoVA steel) processed by S1 is subjected to induction heating assisted shot peening treatment; the specific process is as follows:
[0064] S21: Preheat the high-strength steel processed by S1 to 230℃ and keep it warm for 3 minutes to avoid surface hardening after high-frequency heating and ensure that the surface maintains austenite during shot peening;
[0065] S22: Turn on induction heating, control the current frequency to 300kHz, heating time to 7s, and heat to A c1 The surface of high-strength steel material is instantly austenitized within 1-2mm depth.
[0066] S23: Shot peening treatment, adjust the spray gun so that the shot spray direction is perpendicular to the high-strength steel treated surface after S22 induction heating, and perform shot peening treatment. The shot peening process is as follows: the shot is 0.2mm steel shot, the air pressure is 0.4MPa, the distance between the nozzle and the material surface is controlled at 8cm, and the shot peening coverage is controlled at 200%; the rotation speed of the high-strength steel is 200r / min;
[0067] S3: The high-strength steel treated by induction heating assisted shot peening in S2 is subjected to ultrasonic rolling treatment to obtain a high-strength steel with a large thickness gradient nanostructure on the surface. The ultrasonic rolling treatment process is as follows:
[0068] S31: The surface of the high-strength steel after S2 induction heating assisted shot peening is perpendicular to the direction of action of the rolling tool head, and the high-strength steel begins to rotate;
[0069] S32: Turn on the ultrasonic rolling equipment, and use the ultrasonic rolling tool head to perform multiple ultrasonic rolling treatments along the axial direction of the component to make the surface roughness of the high-strength steel less than Ra0.1μm; the ultrasonic rolling tool head is a cemented carbide sphere with a diameter of 2mm, and the relevant parameters of the ultrasonic rolling treatment are: static pressure 100N, ultrasonic amplitude 1μm, ultrasonic frequency 20kHz, spindle speed 200r / min, feed speed 0.02mm / r, the number of ultrasonic rolling treatments is 3 times, and the rotation speed of the high-strength steel is 200r / min.
[0070] Example 3
[0071] like Figure 1 As shown, the method for constructing a high-strength steel surface large thickness gradient nanostructure comprises the following specific steps:
[0072] S1: Process the surface of high-strength steel to make the surface roughness Ra6μm or less;
[0073] S2: The high-strength steel (Φ5×50mm 45CrNiMoVA steel) processed by S1 is subjected to induction heating assisted shot peening treatment; the specific process is as follows:
[0074] S21: Preheat the high-strength steel processed by S1 to 230℃ and keep it warm for 3 minutes to avoid surface hardening after high-frequency heating and ensure that the surface maintains austenite during shot peening;
[0075] S22: Turn on induction heating, control the current frequency to 300kHz, heating time to 7s, and heat to A c1 The surface of high-strength steel material is instantly austenitized within 1-2mm depth.
[0076] S23: Shot peening treatment, adjust the spray gun so that the shot spray direction is perpendicular to the high-strength steel treated surface after S22 induction heating, and perform shot peening treatment. The shot peening process is as follows: the shot is 1.5mm steel shot, the air pressure is 0.8MPa, the distance between the nozzle and the material surface is controlled at 10cm, and the shot peening coverage is controlled at 300%; the rotation speed of the high-strength steel is 400r / min;
[0077] S3: The high-strength steel treated by induction heating assisted shot peening in S2 is subjected to ultrasonic rolling treatment to obtain a high-strength steel with a large thickness gradient nanostructure on the surface. The ultrasonic rolling treatment process is as follows:
[0078] S31: The surface of the high-strength steel after S2 induction heating assisted shot peening is perpendicular to the direction of action of the rolling tool head, and the high-strength steel begins to rotate;
[0079] S32: Turn on the ultrasonic rolling equipment, and use the ultrasonic rolling tool head to perform multiple ultrasonic rolling treatments along the axial direction of the component to make the surface roughness of the high-strength steel less than Ra0.1μm; the ultrasonic rolling tool head is a cemented carbide sphere with a diameter of 14mm, and the relevant parameters of the ultrasonic rolling treatment are: static pressure 1500N, ultrasonic amplitude 20μm, ultrasonic frequency 40kHz, spindle speed 400r / min, feed speed 0.1mm / r, the number of ultrasonic rolling treatments is 3 times, and the rotation speed of the high-strength steel is 400r / min.
[0080] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for constructing a high-strength steel surface nanostructure with a large thickness gradient, characterized in that The specific steps include: S1: Process the surface of high-strength steel to make the surface roughness Ra6μm or less; S2: The high-strength steel processed in S1 is subjected to induction heating assisted shot peening treatment; S3: The high-strength steel treated by induction heating assisted shot peening in S2 is subjected to ultrasonic rolling treatment to obtain high-strength steel with a large thickness gradient nanostructure on the surface.
2. The method for constructing a high-strength steel surface nanostructure with a large thickness gradient according to claim 1, characterized in that: The specific process of S2 is: S21: preheat the high-strength steel processed in S1 to 230°C and keep it warm for 3 minutes; S22: Turn on induction heating, control the current frequency to 300kHz, heating time to 7s, and heat to A c1 The surface of high-strength steel material is instantly austenitized within 1-2mm depth. S23: Shot peening treatment, adjust the spray gun so that the shot spray direction is perpendicular to the high-strength steel treated surface after S22 induction heating, and perform shot peening treatment.
3. The method for constructing a high-strength steel surface nanostructure with a large thickness gradient according to claim 2, characterized in that: The shot peening step in S23 includes: the shot particles are 0.2mm-1.5mm steel shot or ceramic shot, the air pressure is 0.4-0.8MPa, the distance between the nozzle and the material surface is controlled at 5cm-10cm, and the shot peening coverage is controlled at 100%-300%.
4. The method for constructing a high-strength steel surface nanostructure with a large thickness gradient according to claim 1, characterized in that: The S3 ultrasonic rolling treatment step comprises: S31: The surface of the high-strength steel after S2 induction heating assisted shot peening is perpendicular to the direction of action of the rolling tool head, and the high-strength steel begins to rotate; S32: Turn on the ultrasonic rolling equipment and use the ultrasonic rolling tool head to perform multiple ultrasonic rolling treatments along the axial direction of the component to make the surface roughness of the high-strength steel less than Ra0.1μm.
5. The method for constructing a high-strength steel surface nanostructure with a large thickness gradient according to claim 4, characterized in that: The steps in S32 include: the ultrasonic rolling tool head is a hard alloy sphere with a diameter of 2mm to 14mm, the relevant parameters of the ultrasonic rolling treatment are: static pressure 0 to 1500N, ultrasonic amplitude 1 to 20μm, ultrasonic frequency 20 to 40kHz, spindle speed 100 to 400r / min, feed speed 0.01 to 0.1mm / r, and the number of ultrasonic rolling treatment passes is 1 to 3 times.