Wear-resistant alloy material, wear-resistant plate, preparation method of wear-resistant plate and tunnel boring machine
By adding B and Y elements to the cobalt-based wear-resistant plate and using processes such as warm rolling, the problem of insufficient wear resistance of the existing wear-resistant plate is solved, the wear resistance and lifespan are significantly improved, and the replacement cycle is extended. This solves the problem of frequent wear of the sealing system during tunnel excavation.
Patent Information
- Application Number
- CN202410771089.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-15
Smart Images

Figure CN118773480A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of tunnel construction equipment, and in particular to a wear-resistant alloy material, a wear-resistant plate, a preparation method thereof, and a tunnel boring machine. Background Art
[0002] During the tunneling process of the tunnel boring machine, the main drive sealing system protects the main bearing and prevents the highly abrasive rock in the tunnel from entering the main bearing system, which is of great significance to the smooth excavation of the tunnel boring machine. However, due to the influence of the rock in the tunnel, the runway of the sealing system is easily worn, resulting in the failure to protect the main bearing. Therefore, the runway must be repaired after wear, but due to the environment in the tunnel, surfacing welding and grinding are time-consuming and labor-intensive, and may even delay the project schedule. Therefore, it is common to install a layer of cobalt-based wear-resistant plate on the outside of the runway of the tunnel boring machine. When the wear-resistant plate is worn, the wear-resistant plate can be replaced, thereby greatly reducing the time required to repair the sealing system.
[0003] However, as the tunnel mileage increases and the abrasiveness of the tunnel rock increases, the wear resistance and life of the existing cobalt-based wear-resistant plates cannot meet the project requirements. Long-mileage tunnels even need to replace the wear-resistant plates multiple times, delaying the project schedule. The wear resistance of conventionally produced wear-resistant plate materials is poor. As a Co-based high-temperature alloy material, this material has many alloy elements, so the rolling window is very narrow, resulting in many difficulties in actual production. Cold rolling is prone to edge cracking or even fracture.
[0004] Therefore, how to provide a new material and preparation method for the wear-resistant plate of the main drive sealing runway of the tunnel boring machine to improve the wear resistance of the wear-resistant plate is a problem that needs to be solved urgently. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a wear-resistant alloy material, a wear-resistant plate and a preparation method thereof and a tunnel boring machine. By adding B element and rare earth Y element to the wear-resistant alloy material, the wear resistance of the wear-resistant plate can be improved, and the plasticity can be improved, which is suitable for protecting the sealed runway of the main drive of the tunnel boring machine.
[0006] To achieve the above-mentioned purpose, the present invention provides a wear-resistant alloy material, wherein, in terms of mass percentage, the chemical composition of the wear-resistant plate material includes: 28.0%-35.0% Cr, 2.0%-4.5% Ni, 3.0%-6.0% W, 0.8%-2.0% Mo, 1.0%-1.8% Mn, 0.3%-2.0% Si, 0.9%-1.5% C, 2.0%-4.0% Fe, 0.1%-0.5% B, 0.5%-1.5% rare earth Y, and the balance is Co.
[0007] According to a specific embodiment of the present invention, preferably, the chemical composition of the wear-resistant alloy material comprises, by mass percentage, 30.0%-34.0% Cr, 3.0%-4.5% Ni, 4.0%-6.0% W, 1.3%-2.0% Mo, 1.2%-1.6% Mn, 1.0%-2.0% Si, 1.0%-1.5% C, 3.0%-4.0% Fe, 0.1%-0.3% B, 0.8%-1.5% rare earth Y, and the balance is Co.
[0008] The inventors of the present invention have found that each element in the chemical composition of the wear-resistant alloy material has the following effects:
[0009] Co: Co as a matrix can form FCC crystal structure at room temperature;
[0010] Cr: Cr is used for surface stabilization and helps to form carbides during solidification and heat treatment, improving wear resistance. However, too high a content will reduce the stability of the FCC structure and impair the mechanical properties of the alloy.
[0011] Ni: As an austenite stabilizing element, Ni can inhibit the transformation of Co from the FCC crystal structure to the HCP structure, but too high Ni content will lead to a decrease in the alloy's rupture strength;
[0012] W and Mo: contribute to solid solution strengthening and can form carbides with C;
[0013] Mn and Si: help increase the fluidity of the alloy, improve casting performance, and enhance melt deoxidation;
[0014] C: can form carbides with other elements to improve wear resistance, but too high a content will reduce plasticity;
[0015] Fe: can improve the strength and hardness of the alloy;
[0016] Rare earth element Y: Rare earth elements help reduce inclusions during the smelting process and improve the strength of the wear-resistant plate; in addition, they can improve the plasticity of the hot working process and increase the deformation of a single forging pass, thereby improving the distribution of carbides and improving wear resistance on the basis of the original strength improvement;
[0017] B: It can improve the strength and plasticity of the alloy. In addition, in the matrix of the cobalt-based alloy, adding 0.1-0.5% of the B element helps to form borides on the matrix, thereby improving the wear resistance of the wear-resistant plate.
[0018] According to a specific embodiment of the present invention, preferably, the carbides in the wear-resistant alloy material are distributed along the rolling direction, and the rolling direction is consistent with the wear direction. The inventors of the present invention found that the reason for the low wear resistance of the material is mainly due to the short length of the carbides that provide wear resistance, while the length direction of the carbides during service is consistent with the wear direction. The technical solution of the present invention increases the reduction rate through warm rolling, thereby promoting the distribution of carbides along the rolling direction, thereby obtaining longer carbides. These longer carbides along the rolling direction can effectively resist abrasive intrusion and improve wear resistance.
[0019] The present invention also provides a wear-resistant plate, wherein the wear-resistant plate is prepared by hot rolling and warm rolling of the above-mentioned wear-resistant alloy material.
[0020] According to a specific embodiment of the present invention, preferably, the hardness of the wear-resistant plate is ≥34HRC, and the wear weight loss after 10 hours of wear is ≤0.6g. More preferably, the hardness of the wear-resistant plate is 34-37HRC, and the wear weight loss after 10 hours of wear is 0.48-0.59g.
[0021] The present invention also provides a method for preparing the above-mentioned wear-resistant plate, wherein the preparation method comprises the following steps: smelting the above-mentioned wear-resistant alloy material and electroslag remelting to obtain an ingot; subjecting the ingot to homogenization treatment, blanking forging, hot rolling, warm rolling, solution heat treatment, and aging heat treatment in sequence to remove surface oxides to obtain a wear-resistant plate.
[0022] In the above preparation method, preferably, the smelting process is to form an electrode rod by vacuum induction smelting. The process of obtaining an ingot by electroslag remelting can further improve purity, reduce segregation, improve crystallization state, avoid metallurgical defects, and obtain an alloy ingot with high cleanliness, good crystal structure, and precise chemical composition.
[0023] In the above preparation method, preferably, the holding temperature of the homogenization treatment is 1260-1280°C and the holding time is 10-12h. In the present invention, the process can eliminate element segregation and segregation phase through long-term high-temperature heat treatment.
[0024] In the above preparation method, preferably, the heating temperature of the blank forging is 1200-1250°C, the holding time is 1-3h, and the forging ratio is 3.0-5.5.
[0025] According to a specific embodiment of the present invention, preferably, the total reduction rate of the hot rolling is 40%-60%, the holding temperature before rolling is 1200-1250°C, and the holding time before rolling is 30-90min. More preferably, the total reduction rate of the hot rolling is 50%-60%, the holding temperature before rolling is 1220-1250°C, and the holding time before rolling is 30-60min. The number of rolling passes is 1 or more.
[0026] According to a specific embodiment of the present invention, preferably, the total reduction rate of the warm rolling is 30%-70%, the holding temperature before rolling is 720-780°C, and the holding time before rolling is 10-30min. More preferably, the total reduction rate of the warm rolling is 30%-50%, the holding temperature before rolling is 720-760°C, and the holding time before rolling is 20-30min. The number of rolling passes is 1 or more. In the present invention, warm rolling replaces cold rolling, which helps to reduce the rolling load and thus enable a larger reduction rate to be adopted. By controlling the shape of carbides through a large reduction rate, the distribution of carbides along the rolling direction can be achieved, thereby effectively resisting the intrusion of abrasive particles in the rolling direction and improving wear resistance.
[0027] According to a specific embodiment of the present invention, preferably, the solution temperature of the solution heat treatment is 1200-1250°C, the holding time is 20-120min, and then air-cooled to room temperature. More preferably, the solution temperature of the solution heat treatment is 1220-1250°C, and the holding time is 20-60min. In the present invention, the solution heat treatment can solidify the molten steel, and dissolve the carbides precipitated in the subsequent cooling process, as well as the carbides or coarse strengthening phases further precipitated in the plastic deformation process, into the matrix as much as possible to obtain a single-phase structure, in preparation for the subsequent precipitation aging to precipitate uniform and fine strengthening phases.
[0028] According to a specific embodiment of the present invention, preferably, the aging temperature of the aging heat treatment is 750-820°C, the holding time is 2-5h, and then air-cooled to room temperature. More preferably, the aging temperature of the aging heat treatment is 750-780°C, and the holding time is 180-300min. In the present invention, the purpose of the aging treatment is to further precipitate fine carbides, increase the amount of strengthening phases, and further improve the strength.
[0029] In the above preparation method, preferably, the method for removing the surface oxide includes surface removal methods such as shot peening and / or machining. This method can remove the iron oxide scale on the surface of the plate after heat treatment and ensure the surface quality.
[0030] The present invention also provides a tunnel boring machine, wherein the above-mentioned wear-resistant plate is provided on the outer side of the main driving sealing runway of the tunnel boring machine.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) In the wear-resistant alloy material provided by the present invention, 0.1-0.5% of B element is added to the matrix of the cobalt-based alloy, which helps to form borides on the matrix and improve the wear resistance of the wear-resistant plate. In addition, rare earth helps to reduce inclusions during the smelting process, improve the strength of the wear-resistant plate, and can improve plasticity and increase the deformation of a single forging pass.
[0033] (2) The method for preparing the wear-resistant plate provided by the present invention replaces cold rolling with warm rolling, which helps to reduce the rolling load and thus achieve a greater reduction rate. Furthermore, by adopting a large forging and hot rolling reduction, the carbide can be relatively long along the rolling direction, thereby resisting the invasion of abrasive particles and improving wear resistance.
[0034] (3) The present invention adopts the method of element + process improvement for optimization. Through specific alloy elements, the wear resistance can be improved on the one hand, and the plasticity can be improved on the other hand. Furthermore, combined with the warm rolling process, a larger reduction rate can be achieved, which promotes the distribution of carbides along the rolling direction. Subsequent heat treatment helps to further promote the distribution of carbides, thereby improving wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the metallographic image of the wear-resistant plate prepared in Example 1.
[0036] Figure 2 This is the metallographic image of the wear-resistant plate of Comparative Example 2.
[0037] Figure 3 This is the metallographic image of the wear-resistant plate prepared in Comparative Example 3. DETAILED DESCRIPTION
[0038] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0039] Example 1
[0040] This embodiment provides a method for preparing a wear-resistant plate for a main drive sealing runway of a tunnel boring machine, comprising the following steps:
[0041] Step 1: Vacuum induction smelting to form electrode rods: Among them, the chemical composition of the wear-resistant plate material is 35.0% Cr, 3.0% Ni, 4.0% W, 1.3% Mo, 1.0% Mn, 0.5% Si, 1.2% C, 2.0% Fe, 0.3% B, 0.9% rare earth Y, and the balance is Co, in terms of mass percentage.
[0042] Step 2: Electroslag remelting to obtain an ingot.
[0043] Step 3: Homogenization treatment: The holding temperature is 1280°C and the holding time is 10 hours.
[0044] Step 4: Forging: heating temperature is 1250℃, holding time is 60min, forging ratio is 3.0.
[0045] Step 5: Hot rolling: The holding temperature in the furnace before rolling is 1200°C, the holding time is 90 minutes, and the reduction rate of hot rolling is 40%.
[0046] Step 6: Warm rolling: The holding temperature in the furnace before rolling is 780°C, the holding time is 10 minutes, and the reduction rate of warm rolling is 70%.
[0047] Step 7: Solution heat treatment: solution temperature is 1220℃, holding time is 70min, and air cooling to room temperature.
[0048] Step 8: Aging heat treatment: Aging temperature is 795°C, holding time is 3h, and air cooling to room temperature.
[0049] Step 9: Shot peening: remove the oxide on the surface of the plate after heat treatment to obtain a wear-resistant plate.
[0050] Example 2
[0051] This embodiment provides a method for preparing a wear-resistant plate for a main drive sealing runway of a tunnel boring machine, comprising the following steps:
[0052] Step 1: Vacuum induction smelting to form electrode rods: wherein, by mass percentage, the chemical composition of the wear-resistant plate material is 28.0% Cr, 2% Ni, 3.0% W, 1.8% Mo, 1.0% Mn, 0.3% Si, 0.9% C, 4.0% Fe, 0.5% B, 0.5% rare earth Y, and the balance is Co.
[0053] Step 2: Electroslag remelting to obtain an ingot.
[0054] Step 3: Homogenization treatment: The holding temperature is 1260°C and the holding time is 12h.
[0055] Step 4: Forging: heating temperature is 1230℃, holding time is 2h, forging ratio is 5.5.
[0056] Step 5: Hot rolling: The holding temperature in the furnace before rolling is 1230° C., the holding time is 60 min, and the reduction rate of hot rolling is 50%.
[0057] Step 6: Warm rolling: The holding temperature in the furnace before rolling is 750°C, the holding time is 15 minutes, and the reduction rate of warm rolling is 50%.
[0058] Step 7: Solution heat treatment: solution temperature is 1200℃, holding time is 120min, air cooling to room temperature.
[0059] Step 8: Aging heat treatment: Aging temperature is 820℃, holding time is 2h, and air cooling to room temperature.
[0060] Step 9: Shot peening: remove the oxide on the surface of the plate after heat treatment to obtain a wear-resistant plate.
[0061] Example 3
[0062] This embodiment provides a method for preparing a wear-resistant plate for a main drive sealing runway of a tunnel boring machine, comprising the following steps:
[0063] Step 1: Vacuum induction smelting to form electrode rods: Among them, the chemical composition of the wear-resistant plate material is 33.0% Cr, 4.5% Ni, 6.0% W, 2.0% Mo, 1.5% Mn, 2.0% Si, 1.5% C, 3.2% Fe, 0.1% B, 1.5% rare earth Y, and the balance is Co, in terms of mass percentage.
[0064] Step 2: Electroslag remelting to obtain an ingot.
[0065] Step 3: Homogenization treatment: The holding temperature is 1270°C and the holding time is 11h.
[0066] Step 4: Forging: heating temperature is 1200℃, holding time is 3h, forging ratio is 5.0.
[0067] Step 5: Hot rolling: The holding temperature in the furnace before rolling is 1250°C, the holding time is 30 minutes, and the reduction rate of hot rolling is 60%.
[0068] Step 6: Warm rolling: The holding temperature in the furnace before rolling is 720°C, the holding time is 30 minutes, and the reduction rate of warm rolling is 30%.
[0069] Step 7: Solution heat treatment: solution temperature is 1250℃, holding time is 20min, air cooling to room temperature.
[0070] Step 8: Aging heat treatment: Aging temperature is 750℃, holding time is 5h, and air cooling to room temperature.
[0071] Step 9: Shot peening: remove the oxide on the surface of the plate after heat treatment to obtain a wear-resistant plate.
[0072] Comparative Example 1
[0073] The wear-resistant plate is obtained by surface quenching 42CrMo steel (grade 42CrMo, standard GB / T 3077-2015), the quenching layer depth is 5mm, and the quenching layer hardness is 55HRC.
[0074] Comparative Example 2
[0075] The original Co-based wear-resistant plate is used with a hardness of 38HRC. The chemical composition includes: 30.8% Cr, 2.7% Ni, 4.0% W, 1.0% Mo, 1.4% Mn, 0.4% Si, 1.2% C, 0.9% Fe, and the balance is Co.
[0076] Comparative Example 3
[0077] This comparative example provides a method for preparing a wear-resistant plate, comprising the following steps:
[0078] Step 1: Vacuum induction smelting to form electrode rods: Among them, the chemical composition of the wear-resistant plate material is 33.0% Cr, 4.5% Ni, 6.0% W, 2.0% Mo, 1.5% Mn, 2.0% Si, 1.5% C, 3.2% Fe, 0.1% B, 1.5% rare earth Y, and the balance is Co, in terms of mass percentage.
[0079] Step 2: Electroslag remelting to obtain an ingot.
[0080] Step 3: Homogenization treatment: The holding temperature is 1270°C and the holding time is 11h.
[0081] Step 4: Forging: heating temperature is 1200℃, holding time is 3h, forging ratio is 5.0.
[0082] Step 5: Hot rolling: The holding temperature in the furnace before rolling is 1225°C, the holding time is 30 minutes, and the reduction rate of hot rolling is 30%.
[0083] Step 6: Warm rolling: The holding temperature in the furnace before rolling is 730°C, the holding time is 30 minutes, and the reduction rate of warm rolling is 20%.
[0084] Step 7: Solution heat treatment: solution temperature is 1180℃, holding time is 20min, air cooling to room temperature.
[0085] Step 8: Aging heat treatment: Aging temperature is 740℃, holding time is 10h, and air cooling to room temperature.
[0086] Step 9: Shot peening: remove the oxide on the surface of the plate after heat treatment to obtain a wear-resistant plate.
[0087] Comparative Example 4
[0088] This comparative example provides a method for preparing a wear-resistant plate. The preparation process is basically the same as that of comparative example 3, except that the solution heat treatment temperature in step seven is 1280°C, and the aging temperature in step eight is 880°C.
[0089] Comparative Example 5
[0090] This comparative example provides a method for preparing a wear-resistant plate, comprising the following steps:
[0091] Step 1: Vacuum induction smelting to form electrode rods: wherein, by mass percentage, the chemical composition of the wear-resistant plate material is 25.0% Cr, 5.0% Ni, 2.0% W, 0.5% Mo, 0.7% Mn, 0.1% Si, 0.6% C, 1.2% Fe, 0.03% B, 0.2% rare earth Y, and the balance is Co.
[0092] Step 2: Electroslag remelting to obtain an ingot.
[0093] Step 3: Homogenization treatment: The holding temperature is 1250°C and the holding time is 6 hours.
[0094] Step 4: Forging: heating temperature is 1180℃, holding time is 40min, forging ratio is 2.0.
[0095] Step 5: Hot rolling: The holding temperature in the furnace before rolling is 1180°C, the holding time is 20 minutes, and the reduction rate of hot rolling is 30%.
[0096] Step 6: Warm rolling: The holding temperature in the furnace before rolling is 700°C, the holding time is 5 minutes, and the reduction rate of warm rolling is 20%.
[0097] Step 7: Solution heat treatment: solution temperature is 1180℃, holding time is 15min, air cooling to room temperature.
[0098] Step 8: Aging heat treatment: Aging temperature is 740℃, holding time is 6h, and air cooling to room temperature.
[0099] Step 9: Shot peening: remove the oxide on the surface of the plate after heat treatment to obtain a wear-resistant plate.
[0100] Comparative Example 6
[0101] This comparative example provides a method for preparing a wear-resistant plate. The preparation process is basically the same as that of Example 1, except that the warm rolling in step six is changed to cold rolling, and the reduction rate of the cold rolling is 15%.
[0102] The performance of the wear-resistant plates provided in the above embodiments and comparative examples is tested below, and the testing process is as follows:
[0103] In order to compare the wear resistance of the wear-resistant plates provided by Examples 1-3 of the present invention and Comparative Examples 1-6, samples of the same size were selected for wet sand wear test. The wear test object was a nitrile rubber commonly used for tunneling machine seals, with a Shore hardness of 80, and the diameter of the nitrile rubber sample was 178 mm. The wear test was carried out under the conditions of a load of 200 N and a rotation speed of 200 r / min, and the wear test time was 10 h. The material hardness was tested before wear, and the wear weight loss was tested after the wear test, and the results are shown in Table 1.
[0104] Table 1. Rockwell hardness and wear weight loss after wear test of examples and comparative examples
[0105] Hardness, HRC Wear loss, g Example 1 35 0.59 Example 2 34 0.54 Example 3 37 0.48 Comparative Example 1 55 3.06 Comparative Example 2 38 0.67 Comparative Example 3 33 0.98 Comparative Example 4 35 1.12 Comparative Example 5 34 1.05 Comparative Example 6 36 0.87
[0106] As can be seen from Table 1, the wear weight loss of Examples 1-3 of the present invention is not only significantly lower than that of the surface-hardened 42CrMo steel, but also lower than that of the original Co-based wear-resistant plate; while the wear weight loss of Comparative Examples 4-6 increased after changing the process parameters and the element ratio of the alloy. Therefore, the technical solution of the present invention improves the wear resistance of the wear-resistant plate and helps to increase the life of the wear-resistant plate.
[0107] from Figure 1 , Figure 2 , Figure 3 It can be seen that compared with Comparative Example 2 (original Co-based wear-resistant plate) and Comparative Example 3, the carbides of Example 1 are longer along the rolling direction, and the rolling direction is consistent with the wear direction. Therefore, the wear-resistant plate prepared in Example 1 is beneficial to resist the invasion of abrasive particles due to its longer carbides, thereby reducing the weight loss due to wear.
Claims
1. A wear-resistant alloy material, wherein: The chemical composition of the wear-resistant alloy material includes, by mass percentage, 28.0%-35.0% Cr, 2.0%-4.5% Ni, 3.0%-6.0% W, 0.8%-2.0% Mo, 1.0%-1.8% Mn, 0.3%-2.0% Si, 0.9%-1.5% C, 2.0%-4.0% Fe, 0.1%-0.5% B, 0.5%-1.5% rare earth Y, and the balance is Co; Preferably, the chemical composition of the wear-resistant alloy material includes, by mass percentage, 30.0%-34.0% Cr, 3.0%-4.5% Ni, 4.0%-6.0% W, 1.3%-2.0% Mo, 1.2%-1.6% Mn, 1.0%-2.0% Si, 1.0%-1.5% C, 3.0%-4.0% Fe, 0.1%-0.3% B, 0.8%-1.5% rare earth Y, and the balance is Co.
2. The wear-resistant alloy material according to claim 1, wherein: The carbides in the wear-resistant alloy material are distributed along the rolling direction, and the rolling direction is consistent with the wear direction.
3. A wear-resistant plate, wherein: The wear-resistant plate is prepared by hot rolling or warm rolling using the wear-resistant alloy material according to claim 1 or 2.
4. The wear-resistant plate according to claim 3, wherein: The hardness of the wear-resistant plate is ≥34HRC, and the wear weight loss after 10h of wear is ≤0.6g; Preferably, the hardness of the wear-resistant plate is 34-37HRC, and the wear weight loss after 10 hours of wear is 0.48-0.59g.
5. The method for preparing the wear-resistant plate according to claim 3 or 4, wherein: The preparation method comprises the following steps: The wear-resistant alloy material according to claim 1 or 2 is smelted and electroslag remelted to obtain an ingot; The ingot is subjected to homogenization treatment, blanking forging, hot rolling, warm rolling, solution heat treatment and aging heat treatment in sequence to remove oxides on the surface and obtain a wear-resistant plate.
6. The preparation method according to claim 5, wherein: The total reduction rate of the hot rolling is 40%-60%, the holding temperature before rolling is 1200-1250°C, and the holding time before rolling is 30-90min; Preferably, the total reduction ratio of the hot rolling is 50%-60%, the holding temperature before rolling is 1220-1250° C., and the holding time before rolling is 30-60 min.
7. The preparation method according to claim 5, wherein: The total reduction rate of the warm rolling is 30%-70%, the holding temperature before rolling is 720-780°C, and the holding time before rolling is 10-30min; Preferably, the total reduction rate of the warm rolling is 30%-50%, the holding temperature before rolling is 720-760° C., and the holding time before rolling is 20-30 min.
8. The preparation method according to claim 5, wherein: The solution heat treatment has a solution temperature of 1200-1250°C and a holding time of 20-120 minutes; Preferably, the solution temperature of the solution heat treatment is 1220-1250° C., and the holding time is 20-60 min.
9. The preparation method according to claim 5, wherein: The aging temperature of the aging heat treatment is 750-820°C, and the holding time is 2-5h; Preferably, the aging temperature of the aging heat treatment is 750-780°C, and the holding time is 180-300 minutes.
10. A tunnel boring machine, wherein: The outer side of the main drive sealing runway of the tunnel boring machine is provided with the wear-resistant plate according to claim 3 or 4.