Molybdenum disulfide-based nano composite coating and preparation method thereof

By forming the Mo-S-C-N top layer on the MoS2 coating, the problem of insufficient wear resistance and bearing capacity of the single-layer MoS2 coating is solved, and long and high wear life are achieved in a vacuum environment, with an average friction coefficient of 0.019 and wear Lifespan reaches 3.8×105 turns.

CN118773558APending Publication Date: 2024-10-15LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410765902.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The single-layer MoS2 coating has shortcomings in wear resistance and bearing capacity, especially in vacuum environments that are susceptible to infiltration of oxygen and water vapor, resulting in deterioration of tribological properties and low hardness, making it difficult to meet long-life and wear-resistant applications. Require.

Method used

The molybdenum disulfide-based nanocomposite coating is adopted with a double-layer structure, the bottom layer is a MoS2 coating, and the top layer is a Mo-S-C-N coating. It is prepared by physical vapor deposition technology, and the deposition parameters are adjusted to form a MoS2 layer with a thickness of 1000nm and 300~1000nm. The Mo-S-C-N layer has an elemental composition of 26 to 35.7 at.%, S is 21.87 to 45 at.%, C is 17 to 28.73 at.%, and N is 8.5 to 13.7 at.%, so as to improve the coating Wear resistance and bearing capacity.

Benefits of technology

It achieves long life and high wear life in a vacuum environment, with an average friction coefficient of 0.019 and a wear life of 3.8×105 turns, which significantly improves the wear resistance and bearing capacity of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773558A_ABST
    Figure CN118773558A_ABST
Patent Text Reader

Abstract

The invention provides a molybdenum disulfide-based nano-composite coating and a preparation method thereof, the nano-composite coating is of a double-layer structure, the bottom layer is a MoS2 coating, the top layer is a Mo-S-C-N coating, the thickness of the nano-composite coating is 1300-2000 nm, the thickness of a single layer of the MoS2 coating is 1000 nm, the thickness of a single layer of the Mo-S-C-N coating is 300-1000 nm, and the thickness of the MoS2 coating is 1000 nm. The Mo-S-C-N coating comprises the following elemental components in percentage by atom: 26 to 35.7 at.% of Mo, 21.87 to 45 at.% of S, 17 to 28.73 at.% of C and 8.5 to 13.7 at.% of N, and the double-layer coating is prepared by adopting physical vapor deposition. The method has the beneficial effect that the tribological performance of the composite coating in the vacuum environment is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a molybdenum disulfide-based nanocomposite coating and a preparation method thereof, and relates to the technical field of surface protection of moving parts. Background Art

[0002] As a typical representative of transition metal sulfides, MoS2 is used as one of the main solid lubricating materials on the surface of space mechanical motion mechanisms due to its easily sheared layered structure and excellent lubrication performance. However, most MoS2 coatings grow perpendicular to the substrate surface and have a typical loose columnar crystal structure, which makes the active edge faces very easy to be exposed, increasing the oxidation sites. This leads to the coating's pore structure being easily infiltrated by oxygen, water vapor and other reactive substances during storage, transportation and launch, thereby deteriorating the tribological properties of the coating. Although the MoS2 coating has a low friction coefficient in a vacuum environment, the prepared coating itself has a low hardness, and its load-bearing capacity is obviously not enough to meet the requirements of long life, wear resistance and variable working conditions. It can be seen that the single-layer pure phase MoS2 coating is insufficient in wear resistance and load-bearing capacity due to the columnar crystal structure. Summary of the invention

[0003] The invention provides a molybdenum disulfide-based nanocomposite coating and a preparation method thereof, which solves the technical problem that a single-layer MoS2 coating in the prior art is insufficient in terms of wear resistance and bearing capacity.

[0004] The present invention is implemented in this way: the nanocomposite coating has a double-layer structure, the bottom layer is a MoS2 coating, and the top layer is a Mo-SCN coating. The element composition in the Mo-SCN coating is as follows according to atomic percentage: Mo is 26-35.7 at.%, S is 21.87-45 at.%, C is 17-28.73 at.%, and N is 8.5-13.7 at.%. The thickness of the MoS2 coating is 1000 nm, and the thickness of the Mo-SCN coating is 300-1000 nm.

[0005] The preparation method of the molybdenum disulfide-based nanocomposite coating comprises the following steps: (1) Substrate pretreatment After cleaning, blow dry the substrate and set aside; (2) Pre-sputtering cleaning of substrate The substrate obtained in step (1) was pre-sputtered and cleaned for 20 minutes; (3) Bottom layer deposition Physical vapor deposition was used to deposit the bottom MoS2 coating. The deposition parameters were as follows: argon flow rate was 70 sccm, deposition pressure was 0.3 Pa, substrate bias was continuously adjusted to 0 V, radio frequency power was applied to the MoS2 target, the sputtering power of the MoS2 target was continuously increased to 600 W, the rotating frame speed was 0.5 r / min, and the deposition time was 80 min.

[0006] (4) Top coating deposition After the bottom layer deposition is completed, the argon flow rate is maintained at 70 sccm, nitrogen is introduced, the nitrogen flow rate is 5-15 sccm, the sputtering power of the MoS2 target is maintained at 600 W, a DC power supply is applied to the pure C target, the deposition current is adjusted to 0.5-1.5 A, the rotating frame speed is 0.5 r / min, the deposition time is 50 min, and the Mo-SCN coating is deposited.

[0007] As a further preference, the pre-sputtering cleaning conditions of step (2) are: vacuum degree lower than 0.001 Pa, argon gas is introduced, the argon gas flow rate is 30 sccm, the etching pressure is 0.2 Pa, the rotation speed is 5 r / min, and the substrate bias is -400 V.

[0008] As a further preference, the nitrogen flow rate in step (4) is 15 sccm.

[0009] As a further preference, the deposition current in step (4) is 1.5 A.

[0010] As a further preference, the substrate in step (1) is a 9Cr18 alloy steel substrate.

[0011] The beneficial effect of the present invention is that by constructing a double-layer structure of a molybdenum disulfide-based nanocomposite coating, a long life of the coating in a vacuum environment is achieved, and the preparation method is simple and has strong operability. When the vacuum degree is lower than 0.001Pa, the composite coating has a long wear life in a vacuum environment. The composite coating provided by the present invention has an average friction coefficient of 0.019 and a wear life of 3.8×10 5 lock up. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0013] Figure 1 is the friction coefficient result of the composite coating of Example 1 under vacuum environment; Figure 2 is the friction coefficient result of the composite coating of Example 2 under vacuum environment; Figure 3 This is the friction coefficient result of the composite coating of Example 3 in a vacuum environment. DETAILED DESCRIPTION

[0014] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0015] A method for preparing a molybdenum disulfide-based nanocomposite coating, the specific steps are as follows: (1) Preprocessing The 9Cr18 alloy steel substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then dried and placed in a drying chamber for later use. (2) Pre-sputtering cleaning The 9Cr18 alloy steel substrate treated in step (1) is placed in a vacuum chamber and evacuated to a vacuum degree of less than 0.001 Pa, ion etching of the substrate surface was started, Ar was introduced, the Ar flow rate was 30 sccm, the etching pressure was 0.2 Pa, the rotation speed was 5 r / min, the substrate bias voltage was -400 V, and the steel block sample was pre-sputtered and cleaned for 20 minutes with Ar plasma; (3) Deposition of MoS2 coating Physical vapor deposition technology was used, the Ar flow rate was increased to 70 sccm, the deposition pressure was 0.3 Pa, the substrate bias was continuously adjusted to 0 V, a radio frequency power supply was applied to the MoS2 target, the sputtering power of the MoS2 target was continuously increased to 600 W within 4 minutes, the rotating frame speed was 0.5 r / min, the deposition time was 80 min, and the MoS2 coating was deposited; (4) Deposition of Mo-SCN coating The Ar flow rate was kept constant at 70 sccm, N2 was introduced, the N2 flow rate was 5 sccm, and the sputtering power of the MoS2 target was kept constant at 600 W. At this time, a DC power supply was applied to the pure C target, the deposition current was adjusted to 0.5 A, the rotating frame speed was 0.5 r / min, the deposition time was 50 min, and the Mo-SCN coating was deposited.

[0016] The thickness of the composite coating prepared in Example 1 is about 1300 nm, the thickness of the single-layer MoS2 coating is 1000 nm, the thickness of the single-layer Mo-SCN coating is 300 nm, and the elemental compositions in the Mo-SCN coating are as follows in atomic percentage: Mo is 29.5 at.%, S is 45 at.%, C is 17 at.%, and N is 8.5 at.%.

[0017] The tribological properties of the composite coating obtained in Example 1 were tested using a CSM vacuum friction tester. The friction test was started when the vacuum degree was lower than 0.001 Pa. During the friction process, the load applied was 3 N, the speed was 500 r / min, and the friction coefficient protection value was set to 0.05. Figure 1 The coating was subjected to 1.8×10 5 After 3 cycles, the friction coefficient reached 0.05, and the average friction coefficient during the friction process was 0.026. Example

[0018] A method for preparing a molybdenum disulfide-based nanocomposite coating, the specific steps are as follows: (1) Preprocessing The 9Cr18 alloy steel substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then dried and placed in a drying chamber for later use. (2) Pre-sputtering cleaning The 9Cr18 alloy steel substrate treated in step (1) is placed in a vacuum chamber and evacuated to a vacuum degree of less than 0.001 Pa, ion etching of the substrate surface was started, Ar was introduced, the Ar flow rate was 30 sccm, the etching pressure was 0.2 Pa, the rotation speed was 5 r / min, the substrate bias voltage was -400 V, and the steel block sample was pre-sputtered and cleaned for 20 minutes with Ar plasma; (3) Deposition of MoS2 coating Physical vapor deposition technology was used, the Ar flow rate was increased to 70 sccm, the deposition pressure was 0.3 Pa, the substrate bias was continuously adjusted to 0 V, a radio frequency power supply was applied to the MoS2 target, the sputtering power of the MoS2 target was continuously increased to 600 W within 4 min, the rotating frame speed was 0.5 r / min, the deposition time was 80 min, and the MoS2 coating was deposited; (4) Deposition of Mo-SCN coating The Ar flow rate was kept constant at 70 sccm, N2 was introduced, the N2 flow rate was 10 sccm, and the sputtering power of the MoS2 target was kept constant at 600 W. At this time, a DC power supply was applied to the pure C target, the deposition current was adjusted to 1 A, the rotating frame speed was 0.5 r / min, the deposition time was 50 min, and the Mo-SCN coating was deposited.

[0019] The thickness of the composite coating prepared in Example 2 is about 1700 nm, the thickness of the single-layer MoS2 coating is 1000 nm, the thickness of the single-layer Mo-SCN coating is 700 nm, and the elemental compositions in the Mo-SCN coating are as follows in atomic percentage: Mo is 26 at.%, S is 38.2 at.%, C is 23 at.%, and N is 12.8 at.%.

[0020] The tribological properties of the composite coating of Example 2 were tested using a CSM vacuum friction tester. The friction test was started when the vacuum degree was lower than 0.001 Pa. During the friction process, the load applied was 3 N, the speed was 500 r / min, and the friction coefficient protection value was set to 0.05. Figure 2 The coating was subjected to 3.2×10 5 After 3 cycles, the friction coefficient reached 0.05, and the average friction coefficient during the friction process was 0.026. Example

[0021] A method for preparing a molybdenum disulfide-based nanocomposite coating, the specific steps are as follows: (1) Preprocessing The 9Cr18 alloy steel substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then dried and placed in a drying chamber for later use. (2) Pre-sputtering cleaning The 9Cr18 alloy steel substrate treated in step (1) is placed in a vacuum chamber and evacuated to a vacuum degree of less than 0.001 Pa, ion etching of the substrate surface was started, Ar was introduced, the flow rate was 30 sccm, the etching pressure was 0.2 Pa, the rotation speed was 5 r / min, the substrate bias voltage was -400 V, and the steel block sample was pre-sputtered and cleaned for 20 minutes with Ar plasma; (3) Deposition of MoS2 coating Physical vapor deposition technology was used, the Ar flow rate was increased to 70 sccm, the deposition pressure was 0.3 Pa, the substrate bias was continuously adjusted to 0 V, a radio frequency power supply was applied to the MoS2 target, the sputtering power of the MoS2 target was continuously increased to 600 W within 4 min, the rotating frame speed was 0.5 r / min, the deposition time was 80 min, and the MoS2 coating was deposited; (4) Deposition of Mo-SCN coating The Ar flow rate was kept constant at 70 sccm, N2 was introduced, the N2 flow rate was 15 sccm, and the sputtering power of the MoS2 target was kept constant at 600 W. At this time, a DC power supply was applied to the pure C target, the deposition current was adjusted to 1.5 A, the rotating frame speed was 0.5 r / min, the deposition time was 50 min, and the Mo-SCN coating was deposited.

[0022] The thickness of the composite coating prepared in Example 3 is about 2000 nm, wherein the thickness of the single-layer MoS2 coating is 1000 nm, and the thickness of the single-layer Mo-SCN coating is 1000 nm. The elemental compositions in the Mo-SCN coating are as follows in atomic percentage: Mo is 35.7 at.%, S is 21.87 at.%, C is 28.73 at.%, and N is 13.7 at.%.

[0023] The tribological properties of the coating obtained in Example 3 were tested using a CSM vacuum friction tester. The friction test was started when the vacuum degree was lower than 0.001 Pa. During the friction process, the load applied was 3 N, the speed was 500 r / min, and the friction coefficient protection value was set to 0.05. Figure 3 The coating was subjected to 3.8×10 5 After 3 cycles, the friction coefficient reached 0.05, and the average friction coefficient during the friction process was 0.019.

[0024] The beneficial effect of the present invention is that by constructing a double-layer structure of a molybdenum disulfide-based nanocomposite coating, a long life of the coating in a vacuum environment is achieved, and the preparation method is simple and has strong operability. When the vacuum degree is lower than 0.001Pa, the composite coating has a long wear life in a vacuum environment. The composite coating provided by the present invention has an average friction coefficient of 0.019 and a wear life of 3.8×10 5 lock up.

[0025] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Molybdenum disulfide-based nanocomposite coating, characterized in that: The nanocomposite coating has a double-layer structure, with a bottom layer being a MoS2 coating and a top layer being a Mo-SCN coating. The elemental compositions in the Mo-SCN coating are as follows in terms of atomic percentage: Mo is 26 to 35.7 at.%, S is 21.87 to 45 at.%, C is 17 to 28.73 at.%, and N is 8.5 to 13.7 at.%. The thickness of the MoS2 coating is 1000 nm, and the thickness of the Mo-SCN coating is 300 to 1000 nm.

2. The method for preparing the molybdenum disulfide-based nanocomposite coating according to claim 1, characterized in that: The steps include: (1) Substrate pretreatment After cleaning, blow dry the substrate and set aside; (2) Pre-sputtering cleaning of substrate The substrate obtained in step (1) was pre-sputtered and cleaned for 20 minutes; (3) Bottom layer deposition Physical vapor deposition was used to deposit the bottom MoS2 coating. The deposition parameters were as follows: argon flow rate was 70 sccm, deposition pressure was 0.3 Pa, substrate bias was continuously adjusted to 0 V, radio frequency power was applied to the MoS2 target, the sputtering power of the MoS2 target was continuously increased to 600 W, the rotating frame speed was 0.5 r / min, and the deposition time was 80 min.

3. (4) Top coating deposition After the bottom layer deposition is completed, the argon flow rate is maintained at 70 sccm, nitrogen is introduced, the nitrogen flow rate is 5-15 sccm, the sputtering power of the MoS2 target is maintained at 600 W, a DC power supply is applied to the pure C target, the deposition current is adjusted to 0.5-1.5 A, the rotating frame speed is 0.5r / min, the deposition time is 50 min, and the Mo-SCN coating is deposited.

4. The preparation method according to claim 2, characterized in that: The pre-sputtering cleaning conditions of step (2) are: vacuum degree less than 0.001 Pa, argon gas is introduced, the argon gas flow rate is 30 sccm, the etching pressure is 0.2 Pa, the rotation speed is 5 r / min, and the substrate bias is -400 V.

5. The preparation method according to claim 2, characterized in that: The nitrogen flow rate in step (4) is 15 sccm.

6. The preparation method according to claim 4, characterized in that: The deposition current of step (4) is 1.5 A.

7. The preparation method according to claim 2, characterized in that: The substrate in step (1) is a 9Cr18 alloy steel substrate.