Yttrium-gadolinium alloy oxide modified metal-based composite coating as well as preparation method and application thereof
Through the preparation of yttrium-gadolinium alloy oxide modified metal-based composite coating, the problem of insufficient anti-corrosion performance of laser cladding anti-corrosion coating is solved by mixing (Y1-xGdx)2O3 powder with tungsten carbide powder and nickel-based metal powder. Obtained better corrosion resistance and simple preparation process on offshore steel structures.
Patent Information
- Application Number
- CN202410793926.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-15
AI Technical Summary
Existing laser cladding anti-corrosion coatings have limited anti-corrosion performance on offshore steel structural materials, resulting in poor durability of the coating, easy failure, and complicated preparation process, which may have adverse effects on the environment.
The preparation method of the yttrium-gadolinium alloy oxide modified metal-based composite coating is adopted. (Y1-xGdx)2O3 powder, tungsten carbide powder and nickel-based metal powder are mixed to form a preset layer, and laser melting is performed under inert gas protection. coating to prepare a composite coating with better corrosion resistance.
It realizes that the coating in the field of marine anti-corrosion has better corrosion resistance, and the preparation method has low cost and simple process, and is suitable for industrial production.
Smart Images

Figure CN118773603A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laser cladding coatings, and in particular to a yttrium-gadolinium alloy oxide modified metal-based composite coating and a preparation method and application thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Offshore steel structural materials have long been exposed to seawater corrosion and the working environment is very harsh. Most of their corrosion failures are concentrated on the surface of the workpiece. Therefore, it is particularly important to use processing methods to improve their corrosion resistance. At present, the corrosion resistance of offshore steel structural materials is mainly improved by applying anti-corrosion coatings. However, the anti-corrosion coating applied on the surface of the steel substrate by brushing or spraying often has poor durability. The coating is prone to gloss loss, discoloration, powdering, bulging, cracking and swelling due to the corrosion of the marine atmospheric environment. If defects occur in part of the coating, the entire coating loses its protective effect and needs to be completely removed and re-coated. Therefore, there is a problem of high frequency of coating replacement. In addition, in order to make the anti-corrosion coating have good adhesion, leveling, anti-corrosion performance, etc., the materials in the coating are complex and the preparation process is cumbersome, which may have adverse effects on the marine environment.
[0004] Laser cladding technology is simpler to prepare anti-corrosion coatings than brushing or spraying anti-corrosion coatings. It can effectively improve the corrosion resistance and other properties of the surface of the alloy material without changing the internal structure of the substrate, thereby effectively protecting the steel structure. However, there are few studies on laser cladding anti-corrosion coatings, and the existing laser cladding coatings have limited anti-corrosion properties. Therefore, providing a laser cladding anti-corrosion coating with good corrosion resistance is an urgent problem to be solved. Summary of the invention
[0005] In view of this, the present invention provides a yttrium-gadolinium alloy oxide modified metal-based composite coating and a preparation method and application thereof, which solves the problem of poor anti-corrosion performance of existing laser cladding anti-corrosion coatings.
[0006] In a first aspect, the present invention provides a method for preparing a yttrium-gadolinium alloy oxide modified metal-based composite coating, comprising the following steps:
[0007] (Y 1-x G x )2O3 powder, tungsten carbide powder and nickel-based metal powder are mixed to obtain a mixed powder;
[0008] The mixed powder is formed into a pre-deposited layer on the surface of a metal substrate, and laser cladding is performed under the protection of an inert gas to obtain;
[0009] Among them, 0 <x<1。
[0010] Preferably, in the mixed powder, (Y 1-x G x )The mass content of 2O3 powder is 1-3wt%, the mass content of tungsten carbide powder is 20-30wt%, and the balance is nickel-based metal powder.
[0011] Preferably, x is 0.1 to 0.9.
[0012] Preferably, the nickel-based metal powder is selected from one or more of Ni60A, Ni60 or Ni45A.
[0013] Preferably, the (Y 1-x G x )2O3 powder is prepared as follows: yttrium nitrate and gadolinium nitrate are used as raw materials, a yttrium-gadolinium precursor is prepared by a homogeneous precipitation method, and then the yttrium-gadolinium precursor is calcined at a high temperature to obtain the powder.
[0014] Furthermore, the steps of preparing the yttrium-gadolinium precursor by homogeneous precipitation method using yttrium nitrate and gadolinium nitrate as raw materials are specifically as follows: yttrium nitrate, gadolinium nitrate and urea are fully dispersed in water, heated and stirred at 80-100° C. and precipitated to obtain a mixed rare earth powder, which is washed with water and ethanol in turn, and dried to obtain the yttrium-gadolinium precursor.
[0015] Further, in the step of fully dispersing yttrium nitrate, gadolinium nitrate and urea in water, Gd 3+ With Y 3+ The sum of ion concentrations is 0.01-0.03 mol / L, and the urea concentration is 0.3-0.7 mol / L.
[0016] Furthermore, the high temperature calcination temperature is 900-1100° C., and the calcination time is 3-5 hours.
[0017] Preferably, the inert gas is selected from one or both of argon and nitrogen.
[0018] Preferably, the thickness of the preset layer is 1 to 2 mm; the parameters of the laser cladding are as follows: laser power is 1100 to 1500 W, spot size is 1.5 to 3 mm, scanning speed is 4 to 8 mm / s, and overlap rate is 30 to 50%.
[0019] In a second aspect, the present invention provides a yttrium-gadolinium alloy oxide modified metal-based composite coating prepared by the above preparation method.
[0020] In a third aspect, the present invention provides the application of the above-mentioned yttrium-gadolinium alloy oxide modified metal-based composite coating in the field of marine corrosion protection.
[0021] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0022] The present invention will (Y 1-x G x )2O3 powder is blended with tungsten carbide powder and nickel-based metal powder as coating powder for laser cladding, which can make the obtained composite coating have more excellent corrosion resistance and has potential application prospects in the field of marine corrosion protection. Moreover, the method for preparing the composite coating of the present invention has low cost and simple process, and can be realized in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 is the yttrium-gadolinium alloy oxide (Y 1-x G x ) Flow chart of the preparation method of 2O3 modified metal-based composite coating;
[0025] Figure 2 The preparation of Example 1 of the present invention (Y 0.8 G 0.2 ) SEM images (a, b), SEM-EDS images (c, d) and TEM and TEM-EDS images (e) of 2O3 powder;
[0026] Figure 3 is the polarization curve of the laser cladding composite coating molded parts in Examples 1 to 4 and Comparative Examples 1 to 3 of the present invention;
[0027] Figure 4 It is the Nyquist diagram of the laser cladding composite coating molded parts in Examples 1 to 4 and Comparative Examples 1 to 3 of the present invention. DETAILED DESCRIPTION
[0028] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0029] The present invention provides a method for preparing a yttrium-gadolinium alloy oxide modified metal-based composite coating, comprising the following steps:
[0030] (Y 1-x G x )2O3 powder, tungsten carbide powder and nickel-based metal powder are mixed to obtain a mixed powder;
[0031] The mixed powder is formed into a pre-deposited layer on the surface of a metal substrate, and laser cladding is performed under the protection of an inert gas to obtain;
[0032] Among them, 0 <x<1。
[0033] In the present invention, tungsten carbide powder and nickel-based metal powder have high corrosion resistance and wear resistance, and have good wettability on the surface of the metal matrix. The present invention introduces binary rare earth oxide (Y 1-x G x )2O3, the two rare earth elements have different atomic radii, and their single content is not large, which can avoid the aggregation phenomenon caused by excessive content of a single element and increase the nucleation points. (Y 1-x G x )2O3 in the composite coating can give the coating a higher density and promote the formation of a passivation film, thereby effectively slowing down the corrosion rate. It can also change the properties of inclusions, reduce the electrode potential difference between inclusions and the matrix, and avoid pitting corrosion. Compared with adding Y2O3 or Gd2O3 alone, binary rare earth oxides (Y 1-x G x )2O3 can make the coating have better anti-corrosion performance. 1-x G x )2O3 has good bonding performance with tungsten carbide powder and nickel-based metal powder, which can ensure the formation of a uniform laser cladding composite coating.
[0034] In the mixed powder of the present invention, (Y 1-x G x )The mass content of 2O3 powder is 1-3wt%, the mass content of tungsten carbide powder is 20-30wt%, and the balance is nickel-based metal powder.
[0035] The present invention is for (Y 1-x G x There is no special restriction on the mixing method of )2O3 powder, tungsten carbide powder and nickel-based metal powder, for example, grinding, stirring or ball milling can be used, and ball milling is preferred in the present invention. There is no special restriction on the ball milling mixing step in the present invention, and the ball milling mixing means well known to those skilled in the art can be used.
[0036] In the present invention, x is 0.1 to 0.9, and more preferably, x is 0.2 to 0.6. In the present invention, x = Gd 3+ / (Y 3++Gd 3+ ), the value of x will affect the anti-corrosion performance of the final coating.
[0037] In the present invention, the nickel-based metal powder is selected from one or more of Ni60A, Ni60 or Ni45A.
[0038] In the present invention, the (Y 1-x G x )2O3 powder is prepared as follows: yttrium nitrate and gadolinium nitrate are used as raw materials, a yttrium-gadolinium precursor is prepared by a homogeneous precipitation method, and then the yttrium-gadolinium precursor is calcined at a high temperature to obtain the powder.
[0039] In the present invention, the steps of preparing the yttrium-gadolinium precursor by homogeneous precipitation method using yttrium nitrate and gadolinium nitrate as raw materials are specifically as follows: yttrium nitrate, gadolinium nitrate and urea are fully dispersed in water, heated and stirred at 80-100°C and precipitated to obtain a mixed rare earth powder, which is washed with water and ethanol in turn, and dried to obtain the yttrium-gadolinium precursor. The present invention uses homogeneous precipitation method to prepare binary rare earth oxides to form spherical particles, which have a large specific surface area, strong adsorption capacity, and are easy to mix with tungsten carbide powder and nickel-based metal powder.
[0040] The yttrium nitrate and gadolinium nitrate of the present invention may also be used as hydrates thereof, and the present invention does not impose any particular limitation thereto.
[0041] In the present invention, in the step of fully dispersing yttrium nitrate, gadolinium nitrate and urea in water, Gd 3+ With Y 3+ The sum of the ion concentrations is 0.01-0.03 mol / L, and urea is used as a precipitant with a concentration of 0.3-0.7 mol / L. In the solution system, the hydrolysis of gadolinium nitrate and yttrium nitrate causes the presence of Gd in the mixed solution. 3+ With Y 3+ As urea is added and the reaction temperature increases, urea hydrolyzes to generate precipitating groups OH - ,CO3 2- and HCO3 - When the supersaturation exceeds the critical saturation, homogeneous precipitation slowly occurs.
[0042] The present invention does not impose any particular limitation on the number of times of washing with water and ethanol in sequence, as long as the urea and byproducts on the surface of the precipitate are washed clean. The present invention preferably uses water and ethanol for washing 2 to 5 times each in sequence.
[0043] In the present invention, the high temperature calcination temperature is 900-1100°C, and the calcination time is 3-5h. 1-x G x )2O3 powder. The high temperature calcination of the present invention is carried out in an air atmosphere.
[0044] In the present invention, the inert gas in laser cladding is selected from one or both of argon and nitrogen to avoid adverse effects of air on the coating.
[0045] In the present invention, the thickness of the pre-deposited layer is 1-2 mm. The present invention does not impose any special restrictions on the steps of forming the pre-deposited layer, and any method known in the art may be used.
[0046] In the present invention, the parameters of the laser cladding are as follows: laser power is 1100-1500W, spot size is 1.5-3mm, scanning speed is 4-8mm / s, and overlap rate is 30-50%. The present invention does not impose any special restrictions on the specific laser cladding equipment and operation process, and the laser cladding means well known to those skilled in the art can be used.
[0047] The present invention also includes a step of pre-treating the metal substrate. The present invention does not impose any special limitation on this process, and the common means used by technicians in this field to pre-treat the metal substrate before laser cladding can be used.
[0048] The present invention also provides a yttrium-gadolinium alloy oxide modified metal-based composite coating prepared by the above preparation method. The composite coating of the present invention has good corrosion resistance.
[0049] The present invention also provides the application of the above-mentioned yttrium-gadolinium alloy oxide modified metal-based composite coating in the field of marine corrosion protection. The present invention does not impose any special restrictions on the specific application field, and those skilled in the art can apply it according to the corrosion protection requirements.
[0050] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0051] Figure 1 is the yttrium-gadolinium alloy oxide (Y 1-x G x )Flow chart of the preparation method of 2O3 modified metal-based composite coating.
[0052] Example 1
[0053] This embodiment provides a yttrium-gadolinium alloy oxide (Y 0.8 G 0.2 )2O3 modified metal-based composite coating preparation method.
[0054] (1) Pre-treat the surface of H13 steel, the substrate to be clad, to remove surface rust and oxide layer.
[0055] (2) Disperse yttrium nitrate hexahydrate and gadolinium nitrate hexahydrate in deionized water so that x=Gd 3+ / (Y 3+ +Gd 3+)=0.2, the mixed solution maintains Y 3+ With Gd 3+ The total ion concentration was 0.015 mol / L, urea was added as a precipitant with a concentration of 0.5 mol / L, heated and stirred at 90°C in a water bath heating stirrer for 3 h, the composite rare earth powder was washed three times with deionized water and anhydrous ethanol in turn, dried at 85°C for 12 h, and finally calcined at 1000°C for 4 h to obtain (Y 0.8 G 0.2 )2O3 powder.
[0056] Figure 2 The (Y 0.8 G 0.2 )2O3 powder SEM images (a, b), SEM-EDS analysis images (c, d) and TEM-EDS analysis image (e); it can be seen from the figure that the distribution of Y and Gd elements overlaps, (Y 0.8 G 0.2 )2O3 powder particles are similar in shape and uniform in size, and are not doped with other impurity elements.
[0057] (3) Wet ball milling preparation (Y 0.8 G 0.2 )2O3 / Ni60A / WC mixed powder: 2wt% treated (Y 0.8 G 0.2 )2O3 powder was mixed with 25wt% WC powder and 73wt% Ni60A, and a small amount of anhydrous ethanol was added for ball milling. The ball milling equipment was a GNS3-8 pot mill with a ball-to-powder ratio of 50:3 and a rotation speed of 20rpm for 24h. The ball-milled solution was then dried in a vacuum drying oven at a set temperature of 85°C for 12h.
[0058] (4) Laser cladding: The mixed powder was pre-deposited on the substrate surface to form a 1.5 mm pre-deposited layer, and laser cladding was performed under argon protection to successfully obtain a composite coating with uniform structure. The specific cladding process parameters are as follows: laser power of 1300 W, spot size of 2 mm, scanning speed of 6 mm / s, and overlap rate of 40%.
[0059] Example 2
[0060] This embodiment provides a yttrium-gadolinium alloy oxide (Y 0.6 G 0.4 )2O3 modified metal-based composite coating preparation method.
[0061] Compared with Example 1, the difference is that in this example, x=Gd in the mixed solution of step (2) 3+ / (Y 3+ +Gd 3+ )=0.4.
[0062] Example 3
[0063] This embodiment provides a yttrium-gadolinium alloy oxide (Y 0.4 G 0.6 )2O3 modified metal-based composite coating preparation method.
[0064] Compared with Example 1, the difference is that in this example, x=Gd in the mixed solution of step (2) 3+ / (Y 3+ +Gd 3+ )=0.6.
[0065] Example 4
[0066] This embodiment provides a yttrium-gadolinium alloy oxide (Y 0.2 G 0.8 )2O3 modified metal-based composite coating preparation method.
[0067] Compared with Example 1, the difference is that in this example, x=Gd in the mixed solution of step (2) 3+ / (Y 3+ +Gd 3+ )=0.8.
[0068] Comparative Example 1
[0069] This comparative example is different from Example 1 in that no (Y 0.8 G 0.2 )The mass ratio of 2O3 powder, WC powder and Ni60A is 25:75.
[0070] Comparative Example 2
[0071] This comparative example provides a method for preparing a Y2O3 modified metal-based composite coating.
[0072] Compared with Example 1, the difference is that gadolinium nitrate hexahydrate is not added in step (2) of this comparative example.
[0073] Comparative Example 3
[0074] This comparative example provides a method for preparing a Gd2O3 modified metal-based composite coating.
[0075] Compared with Example 1, the difference is that yttrium nitrate hexahydrate is not added in step (2) of this comparative example.
[0076] Test example
[0077] The corrosion resistance of the laser cladding composite coating molded parts in Examples 1 to 4 and Comparative Examples 1 to 3 was tested. Figure 3is the polarization curve of each laser cladding composite coating molded part, Figure 4 It is the Nyquist diagram of each laser cladding composite coating molded part.
[0078] from Figure 3 It can be seen that compared with the Ni60A / WC composite coating of Comparative Example 1, the corrosion resistance of the composite coating with rare earth oxide added is improved, and the self-corrosion potential (E coor ) moves in the positive direction, and the self-corrosion current density (I coor ) becomes smaller, and the specific data are shown in the following Table 1, among which the composite coating of Example 1 has the best corrosion resistance.
[0079] Table 1 Electrochemical corrosion parameters of each composite coating
[0080]
[0081] Depend on Figure 4 It can be found that compared with the Ni60A / WC composite coating of comparative example 1, the radius of the capacitive reactance arc in the Nyquist plot of the composite coating with rare earth oxide added is increased, and the composite coating of example 1 has the best corrosion resistance.
[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a yttrium-gadolinium alloy oxide modified metal-based composite coating, characterized in that: The steps include: (Y 1-x G x )2O3 powder, tungsten carbide powder and nickel-based metal powder are mixed to obtain a mixed powder; The mixed powder is formed into a pre-deposited layer on the surface of a metal substrate, and laser cladding is performed under the protection of an inert gas to obtain; Among them, 0 <x<1。 2. The preparation method according to claim 1, characterized in that In the mixed powder, (Y 1-x G x )The mass content of 2O3 powder is 1-3wt%, the mass content of tungsten carbide powder is 20-30wt%, and the balance is nickel-based metal powder.
3. The preparation method according to claim 1, characterized in that: x is 0.1 to 0.9; the nickel-based metal powder is selected from one or more of Ni60A, Ni60 or Ni45A.
4. The preparation method according to claim 1, characterized in that: The 1-x G x )2O3 powder is prepared as follows: yttrium nitrate and gadolinium nitrate are used as raw materials, a yttrium-gadolinium precursor is prepared by a homogeneous precipitation method, and then the yttrium-gadolinium precursor is calcined at a high temperature to obtain the powder.
5. The preparation method according to claim 4, characterized in that: The steps of preparing the yttrium-gadolinium precursor by homogeneous precipitation method using yttrium nitrate and gadolinium nitrate as raw materials are specifically as follows: yttrium nitrate, gadolinium nitrate and urea are fully dispersed in water, heated and stirred at 80-100° C. and precipitated to obtain a mixed rare earth powder, which is washed with water and ethanol in turn, and dried to obtain the yttrium-gadolinium precursor.
6. The preparation method according to claim 5, characterized in that: In the step of fully dispersing yttrium nitrate, gadolinium nitrate and urea in water, Gd 3+ With Y 3+ The sum of ion concentrations is 0.01-0.03 mol / L, and the urea concentration is 0.3-0.7 mol / L.
7. The preparation method according to claim 4, characterized in that: The high temperature calcination temperature is 900-1100° C., and the calcination time is 3-5 hours.
8. The preparation method according to claim 1, characterized in that: The inert gas is selected from one or both of argon and nitrogen; the thickness of the preset layer is 1 to 2 mm; the parameters of the laser cladding are as follows: the laser power is 1100 to 1500 W, the spot size is 1.5 to 3 mm, the scanning speed is 4 to 8 mm / s, and the overlap rate is 30 to 50%.
9. The yttrium-gadolinium alloy oxide modified metal-based composite coating prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the yttrium-gadolinium alloy oxide modified metal-based composite coating as claimed in claim 9 in the field of marine corrosion protection.