In-situ construction method of aluminum alloy surface three-level structure anticorrosive coating

A dense three-level structural anti-corrosion layer is constructed through the synergistic and complementary technology of NiAl-LDHs and ZnAl-LDHs, which solves the problem that traditional aluminum alloy surface anti-corrosion coatings are prone to corrosion in saline-alkali environments, achieves self-healing and intelligent anti-corrosion functions, and significantly improves Corrosion resistance and service life.

CN118773607APending Publication Date: 2024-10-15YULIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410756836.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional aluminum alloy surface anti-corrosion coatings are prone to corrosion in saline-alkali environments and lack self-healing and intelligent slow-release functions, resulting in reduced service life.

Method used

Using the synergistic and complementary technology of NiAl-LDHs film and ZnAl-LDHs, a dense three-level anti-corrosion layer is constructed through in-situ growth, combined with hydrophobic modification and anionic surfactant, to form a ZnAl-LDHs base layer@NiAl-LDHs dense layer@ Anti-corrosion coating in the hydrophobic zone of the interface.

Benefits of technology

It significantly enhances the corrosion resistance of the aluminum alloy surface, realizes self-healing and intelligent anti-corrosion functions, improves the density and hydrophobicity of the coating, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773607A_ABST
    Figure CN118773607A_ABST
Patent Text Reader

Abstract

The invention discloses an in-situ construction method of a three-level structure anticorrosive coating on an aluminum alloy surface, belongs to the technical field of surface coating preparation, and aims to solve the problem that a traditional anticorrosive coating is easy to damage and crack in a long-term use process. The construction method comprises the following steps: step 1, constructing a ZnAl-LDHs (at) Al first anticorrosive coating by taking an aluminum alloy as a substrate; 2, the ZnAl-LDHs anti-corrosion layer serves as a supporting point, and a NiAl-LDHs outer anti-corrosion coating grows on the surface of the ZnAl-LDHs in situ; and 3, an anti-corrosion inhibitor is stored in an LDHs nanometer storage device through the ion exchange performance of the ZnAl-LDHs and the NiAl-LDHs, meanwhile, hydrophobic modification and hydrophobic regulation are conducted on the surfaces of the NiAl-LDHs, and a three-level structure anti-corrosion layer of a ZnAl-LDHs substrate layer, a NiAl-LDHs compact layer and an interface hydrophobic area is obtained. The NiAl-SLS-LDHs (at) ZnAl-LDHs (at) Al film prepared by the method has the characteristics that (1) the film has a hydrophobic surface; (2) self-repairing capability; and (3) the two different types of LDHs coatings can be used as anion micro-nano containers to carry out intelligent anti-corrosion adsorption and storage on chloride ions, so that the device effectively adapts to environments with different corrosion ion concentrations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface coating preparation, and in particular relates to an in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy. Background Art

[0002] Aluminum alloy is an important structural material, among which 6061 aluminum alloy is widely used in industrial production. However, in saline-alkali environment, acid rain conditions or environment containing chloride ions, the surface of aluminum alloy is easily corroded and damaged. Traditional anti-corrosion coatings are prone to damage and cracking during long-term use. If they are not repaired in time and accurately, the substrate will be directly exposed to the corrosive environment. These defects will reduce the protective effect of the coating on the metal. In addition, these coatings fail to exert the slow-release and intelligent anti-corrosion effects of the coating, reducing the service life of the coating. Therefore, it is of great significance for the anti-corrosion protection and application of aluminum alloys to formulate effective corrosion protection strategies and construct suitable anti-corrosion coatings to achieve a high degree of integration with the 6061 aluminum alloy substrate and have both self-repairing and intelligent slow-release anti-corrosion effects.

[0003] The new two-dimensional LDHs material has a stable layered structure, special regeneration function and anion exchangeability. On the one hand, these characteristics can provide a physical barrier to the matrix, hindering the corrosion of the corrosive ions on its substrate. On the other hand, its special interlayer channel structure absorbs the corrosive ions in the environment to provide slow release and intelligent protection for the matrix. More importantly, hydrotalcite-like materials can also serve as the best nanocontainer for corrosion inhibitors and hydrophobic groups (surfactants). These functional characteristics have laid the foundation for the potential application of such layered materials as salt-alkali corrosion-resistant coating materials.

[0004] In the LDHs material family, ZnAl-LDHs layer stacking thickness is relatively thick, and it can directly establish contact with the metal substrate through in-situ growth technology, forming a chemical bond, ensuring the strong adhesion between the LDHs film and the substrate, and the strong bonding ability with the substrate. The interlayer channel structure can also absorb a large amount of corrosive ions to provide intelligent protection for the substrate. However, the growth orientation of ZnAl-LDHs crystals is arranged perpendicular to the substrate, and the gaps between the layers are large, resulting in holes and structural defects in the film that are penetrated by corrosive ions. Summary of the invention

[0005] In view of the above problems, since the NiAl-LDHs layer is small and thin, due to the steric hindrance effect, the nano-layers on the NiAl-LDHs film can grow continuously, and by in-situ growth into a very dense film, it can more effectively prevent the penetration of corrosive ions, which is very suitable for the construction of an anti-corrosion outer coating. Based on the ZnAl-LDHs thick coating, the present invention in-situ grows a NiAl-LDHs thin layer coating with good density, and realizes a uniform, dense, and defect-free anti-corrosion coating through the synergistic and complementary effects of two different types of LDHs. In addition, the NiAl-LDHs surface is hydrophobically modified and hydrophobically regulated, and a repair zone is established at the LDHs and hydrophobic interface to obtain a three-level structure anti-corrosion layer with self-repairing function of ZnAl-LDHs base layer @ NiAl-LDHs dense layer @ interface hydrophobic zone.

[0006] The purpose of the present invention is to provide an application of a reagent for detecting the expression level of the molecular marker IRAK1 in the preparation of a glioma diagnosis kit.

[0007] Another object of the present invention is to provide an in-situ construction method for a three-level structure anti-corrosion layer on an aluminum alloy surface, the construction method comprising the following steps:

[0008] Step 1: Using 6061 aluminum alloy as substrate, construct the first anti-corrosion coating of ZnAl-LDHs@Al;

[0009] Step 2: Using the ZnAl-LDHs anti-corrosion layer as a support point, in-situ grow the NiAl-LDHs outer anti-corrosion coating on the surface of ZnAl-LDHs;

[0010] Step 3: Use the ion exchange properties of ZnAl-LDHs and NiAl-LDHs to store corrosion inhibitors in LDHs nanoreservoirs, and at the same time perform hydrophobic modification and hydrophobic regulation on the surface of NiAl-LDHs to obtain a tertiary structure corrosion protection layer of ZnAl-LDHs base layer @NiAl-LDHs dense layer @interface hydrophobic area.

[0011] Furthermore, the construction process of step 1 includes:

[0012] Step 101: preparing a ZnAl-LDHs thin film growth solution;

[0013] Step 102: vertically suspending the pretreated 6061 aluminum sheet in a ZnAl-LDHs thin film growth solution for a water bath reflux reaction;

[0014] Step 103: After the reaction is completed, take out the 6061 aluminum sheet, wash it with deionized water, then wash it with ethanol, and finally dry it at room temperature to obtain Zn 2+ -Al 3+ -LDHs film aluminum sheet;

[0015] Step 104: washing the precipitate in the reaction ZnAl-LDHs film growth solution by centrifugation until the deionized water is clear after washing, then washing it three times with anhydrous ethanol, drying it at room temperature, and finally obtaining ZnAl-LDHs powder for subsequent detection;

[0016] Step 105: Prepare Zn 2+ -Al 3+ -LDHs thin film aluminum sheet is expressed by concentration and ratio as ZnAl-LDHs-xA / B, where x is Zn 2+ The proportion of total ions in the solution is: A is 22.5mmol / L; B is 50mmol / L.

[0017] Furthermore, the specific preparation process of step 101 includes:

[0018] According to Zn 2+ :Al 3+ The molar ratio is 2-4:1. Weigh Zn(NO3)2·6H2O and Al(NO3)3·9H2O respectively and add them into the flask. Then add deionized water and a small magnet into the flask. Put the round-bottom flask into an ultrasonicator and ultrasonicate for 15 minutes. Then add H2NCONH2 and ultrasonicate for another 15 minutes to make it fully dissolved in water and set aside.

[0019] Furthermore, the specific process of step 2 includes:

[0020] Step 201: preparing a NiAl-LDHs thin film growth solution;

[0021] Step 202: Select a suitable aluminum sheet from the ZnAl-LDHs-xA / B obtained in step 104 and place it in a NiAl-LDHs thin film growth solution to perform a water bath reflux reaction;

[0022] Step 203: Take out the aluminum sheet after the reaction, wash it with deionized water, then wash it with ethanol, and finally dry it at room temperature to obtain Ni 2+ -Al 3+ -LDHs@ZnAl-LDHs thin film aluminum sheet;

[0023] Step 204: The precipitate obtained after the reaction is centrifuged and washed until the deionized water is clear, then washed three times with anhydrous ethanol, and dried at room temperature to obtain NiAl-LDHs-zC / D@ZnAl-LDHs powder;

[0024] Step 205: Prepare Ni 2+ -Al 3+-LDHs@ZnAl-LDHs thin film aluminum sheet is expressed by concentration and ratio as NiAl-LDHs-zC / D@ZnAl-LDHs@Al, where z is the proportion of Ni2+; C is the total ions of the solution, which is 50mmol / L; and D is the total ions of the solution, which is 90mmol / L.

[0025] Furthermore, the preparation process of step 201 includes:

[0026] According to Ni 2+ :Al 3+ The molar ratio is 2-4:1. Weigh Ni(NO3)2·6H2O and Al(NO3)3·9H2O respectively and add them into a flask. Then add deionized water and a small magnet. Put the flask into an ultrasonic instrument and sonicate for 15 minutes. Then add urea and sonicate again for 15 minutes to make it fully dissolved in water and set aside.

[0027] Furthermore, the reaction temperature of the water bath reflux reaction in step 101 and step 102 is 97° C., and the constant temperature reaction is performed for 8 hours.

[0028] Furthermore, the specific process of step 3 includes:

[0029] Step 301: Select a suitable aluminum sheet from the NiAl-LDHs-zC / D@ZnAl-LDHs@Al prepared in step 204, and place it in a muffle furnace for calcination to prepare for intercalation modification;

[0030] Step 302: Weigh the surfactant solid powder to prepare a surfactant solution of a certain concentration, suspend the calcined NiAl-LDHs-zC / D@ZnAl-LDHs@Al in a flask with a copper wire, then pour the prepared surfactant solution into the flask to completely immerse the sample, pass nitrogen to expel the air in the system, seal the system, and connect the experimental device to start the reaction;

[0031] Step 303: After the reaction is completed, turn off the power supply, wait until the temperature of the solution in the beaker drops to room temperature, take out the prepared aluminum sheet and name it NiAl-SLS / SL / SPT / SAS-LDHs@ZnAl-LDHs@Al.

[0032] Furthermore, in step 301, the calcination temperature is 400°C and the calcination time is 4 hours.

[0033] Furthermore, the surfactant solution prepared in step 302 is a SLS negative surfactant solution, and the aluminum sheet finally obtained is NiAl-SLS-LDHs@ZnAl-LDHs@Al.

[0034] Furthermore, the corrosion potential of the NiAl-SLS-LDHs@ZnAl-LDHs@Al anti-corrosion layer is 0.582 V, and the corrosion current density is 1.657E-4 A / cm 2 .

[0035] Compared with the prior art, the present invention has the following advantages:

[0036] 1. The present invention constructs a double-layer NiAl-LDHs@ZnAl-LDHs anti-corrosion coating with complementary properties on the surface of 6061 aluminum alloy for the first time, and analyzes the effects of different synthesis concentrations and different metal salt ratios on metal corrosion through various tests, and obtains the sample NiAl-4-D-LDHs@ZnAl-2-BLDHs@Al with the best corrosion resistance.

[0037] 2. The present invention makes full use of the anion exchangeable properties of the LDHs layer in the NiAl-4-D-LDHs@ZnAl-2-BLDHs@Al structure, introduces anionic surfactants (SLS, SL, SPT), and finds that the surface structure of the NiAl-SLS-LDHs@ZnAl-LDHs@Al coating is denser and has a lower porosity than that of NiAl-LDHs@ZnAl-LDHs@Al, and the hydrophobicity (contact angle of 138.6°) is greatly increased. EIS and polarization curve test data show that in a 3.5% NaCl solution, the LDHs coating containing SLS significantly increases the corrosion potential of the aluminum alloy (reaching 0.582V) and significantly reduces the corrosion current (reaching 1.657E-4A / cm 2 ). This indicates that the anti-corrosion performance of LDHs is significantly enhanced.

[0038] 3. The NiAl-SLS-LDHs@ZnAl-LDHs@Al film prepared by the present invention has the following characteristics: ① a hydrophobic surface; ② self-healing ability; ③ two different types of LDHs coatings can be used as anion micro-nano containers to perform intelligent anti-corrosion adsorption and storage of chloride ions, effectively adapting to environments with different corrosive ion concentrations. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1SEM images of NiAl-LDHs@ZnAl-LDHs@Al prepared with different surfactants; (a) and (a') are SEM images of NiAl-LDHs@ZnAl-LDHs@Al coatings; (b) and (b') are SEM images of NiAl-SL-LDHs@ZnAl-LDHs@Al coatings; (c) and (c') are SEM images of NiAl-SPT-LDHs@ZnAl-LDHs@Al coatings; (d) and (d') are SEM images of NiAl-SLS-LDHs@ZnAl-LDHs@Al coatings;

[0040] Figure 2 XPS high-resolution spectra of NiAl-SL-LDHs@ZnAl-LDHs@Al (a) Al 2p, (b) Zn 2p, (c) Ni 2p (d) C 1s, (e) O 1s and (f) S2p;

[0041] Figure 3 XPS high-resolution spectra of NiAl-SPT-LDHs@ZnAl-LDHs@Al (a) Al 2p, (b) Ni 2p (c) C1s, (d) O 1s and (e) S2p;

[0042] Figure 4 XPS high-resolution spectra of NiAl-SLS-LDHs@ZnAl-LDHs@Al (a) Al 2p, (b) Zn2p, (c) Ni2p (d) C 1s, (e) O 1s and (f) S2p;

[0043] Figure 5 is the droplet shape and corresponding contact angle on the surface of different samples;

[0044] Figure 6 (a) Nyquist curves, (b) Bode plots, (c) phase diagrams and;

[0045] Figure 7 is the equivalent circuit used to fit the EIS data of NiAl-SLS-LDHs@ZnAl-LDHs;

[0046] Figure 8 Polarization curves of LDHs layers prepared with different surfactants;

[0047] Fig. 9XRD spectra of aluminum alloy substrate and different LDH films on the surface (a) Al-Substrate (b) ZnAl-LDHs@Al (c) NiAl-LDHs-@ZnAl-LDHs@Al (d) NiAl-SLS-LDHs@ZnAl-LDHs@Al

[0048] Fig.10 FT-IR spectra of aluminum alloy substrate and different LDH films on the surface (a) aluminum alloy substrate (b) ZnAl-LDHs@Al (c) NiAl-LDHs@ZnAl-LDHs@Al (d) NiAl-SLS-LDHs@ZnAl-LDHs@Al

[0049] Fig.11 (a) ZnAl-LDHs@Al (b) prepared at different concentrations and metal ratios

[0050] SEM spectra of NiAl-LDHs-@ZnAl-LDHs@Al (c) NiAl-SLS-LDHs@ZnAl-LDHs@Al;

[0051] Fig.12 Mapping images of different LDHs coatings;

[0052] Fig.13 XPS high-resolution spectra of NiAl-SLS-LDHs@ZnAl-LDHs@Al (a) Al 2p, (b) Zn 2p, (c) Ni2p (d) C 1s, (e) O 1s and (f) S2p;

[0053] Fig.14 AFM images of ZnAl-LDHs@Al thin films;

[0054] Fig.15 AFM images of NiAl-LDHs@ZnAl-LDHs@Al thin films;

[0055] Fig.16 is the droplet shape and corresponding contact angle on different sample surfaces;

[0056] Fig.17 (a) Nyquist curves, (b) Bode diagrams, and (c) phase diagrams of aluminum alloy substrate and different LDHs layers.

[0057] Fig.18 is the equivalent circuit diagram for fitting the EIS data of aluminum alloy matrix;

[0058] Fig.19is the equivalent circuit used to fit the EIS data of ZnAl-LDHs@Al and NiAl-LDHs@ZnAl-LDHs@Al;

[0059] Fig. 20 is the equivalent circuit used to fit the EIS data of NiAl-SLS-LDHs@ZnAl-LDHs@Al;

[0060] Fig.21 5-13. Polarization curves of aluminum alloy substrate and LDHs layer of different coatings;

[0061] Fig. 22 SEM micrographs of different samples after being immersed in 3.5% sodium chloride aqueous solution at room temperature for different time periods (a) Al-substrate (b) ZnAl-LDHs@Al (c) NiAl-LDHs@ZnAl-LDHs@Al (d)

[0062] NiAl-SLS-LDHs@ZnAl-LDHs@Al;

[0063] Fig.23 Schematic diagram of the corrosion protection mechanism of NiAl-SLS-LDHs@ZnAl-LDHs@Al film;

[0064] Fig.24 SEM micrographs of (a) scratched-NiAl-SLS-LDHs@ZnAl-LDHs@Al (b) and (c) self-healed-NiAl-SLS-LDHs@ZnAl-LDHs@A;

[0065] Fig.25 The spectrum results of scratched-NiAl-SLS-LDHs@ZnAl-LDHs@Al (left) and regenerated-NiAl-SLS-LDHs@ZnAl-LDHs@Al (right);

[0066] Fig.26 NiAl-SLS-LDHs@ZnAl-LDHs@Al after scratching and self-recovery; (a) Nyquist diagram, (b) Bode diagram, (c) phase diagram, and (d) polarization curve. DETAILED DESCRIPTION

[0067] The present invention is further described below with reference to specific examples.

[0068] 1. Preparation of LDHs layer

[0069] 1.1 Experimental instruments and reagents

[0070] The equipment used for the analysis method of the samples obtained during the experiment are shown in Table 1-1: contact angle meter (OCA), field emission scanning electron microscope (SEM), atomic force microscope (AFM), X-ray diffractometer (XRD), electrochemical workstation, X-ray photoelectron spectroscopy (XPS), and Fourier transform infrared spectrometer (FTIR).

[0071] Table 1-1 Experimental equipment and characterization instruments

[0072]

[0073]

[0074] This experiment used 6061 aluminum alloy. All chemical reagents used in all LDHs preparation and electrochemical performance testing processes are listed in detail in Table 1-2.

[0075] Table 1-2 Experimental reagents

[0076]

[0077] The 6061 aluminum alloy was cut into 10×10×2mm specimens using a wire cutting machine. 500, 800, 1200 and 1500# sandpapers were used to polish the specimens until there were no obvious scratches on the surface. Then, H2O2 was used to make the oxide film on the surface of the aluminum sheet evenly distributed and dense. After fully oxidizing for 30 minutes, the aluminum sheet was immersed in deionized water and ultrasonically washed to remove surface impurities. After the aluminum sheet was dried, it was wrapped in tin foil for later use.

[0078] 1.2 Preparation of LDHs layer

[0079] 1.2.1 Preparation of ZnAl-LDHs@Al

[0080] Zn 2+ :Al 3+ The molar ratio was 2:1, 3:1 and 4:1, and the mixed solution with the total ion concentration of 22.5mmol / L and 50mmol / L was prepared to generate ZnAl-LDHs film. After comparing the six groups of results, it can be seen that when the total ion concentration of the solution is 50mmol / L, Zn 2+ :Al 3+ When the molar ratio is 2:1, Zn is most suitable 2+ -Al 3+ -LDHs thin film growth.

[0081] Weigh 2.4791 g of Zn(NO3)2·6H2O and 1.5631 g of Al(NO3)3·9H2O and add them into a flask. Then add 250 ml of deionized water and a small magnet into the round-bottom flask. After the round-bottom flask is placed in an ultrasonicator and ultrasonicated for 15 minutes, weigh 1.8769 g of H2NCONH2 and add it into the round-bottom flask and ultrasonicate it again for 15 minutes to make it fully dissolved in water. Set aside for later use.

[0082] The pretreated aluminum sheet was suspended vertically in the above solution for water bath reflux reaction. The reaction temperature was set, and the timing was started when the temperature rose to 97°C. After the constant temperature reaction for 8 hours, the reaction device was closed. The aluminum sheet after the reaction was taken out, first washed with deionized water, then washed with ethanol, and finally dried at room temperature to obtain Zn 2+ -Al 3+ -LDHs thin film aluminum sheet. The precipitate obtained after the reaction is then centrifuged and washed until the deionized water is clear, then washed three times with anhydrous ethanol, and dried at room temperature to obtain ZnAl-LDHs powder.

[0083] For simplicity, the prepared LDHs membranes are expressed in terms of concentration and ratio as ZnAl-LDHs-xA / B (where x is Zn 2+ The proportion of total ions in the solution is: A is 22.5mmol / L; B is 50mmol / L).

[0084] 1.2.2 Preparation of NiAl-LDHs@ZnAl-LDHs@Al

[0085] Ni 2+ :Al 3+ The molar ratio was 2:1, 3:1 and 4:1, and the total ion concentration was 50mmol / L and 90mmol / L. The mixed solution was prepared to generate NiAl-LDHs film. After comparing the six groups of results, it can be seen that when the total ion concentration of the solution is 90mmol / L, Ni 2+ :Al 3+ When the molar ratio is 4:1, Ni is most suitable 2+ -Al 3+ -LDHs film growth. Weigh 5.2344g of Ni(NO3)2·6H2O and 1.6881g of Al(NO3)3·9H2O and add them to the flask, then add 250ml of deionized water and a small magnet to the round-bottom flask, put the round-bottom flask into the ultrasonicator for 15 minutes, weigh 3.3784g of urea and add it to the round-bottom flask for another 15 minutes to make it fully soluble in water, and set aside for later use.

[0086] Select the aluminum sheet with the best corrosion resistance from ZnAl-LDHs-xA / B and place it in the above solution for water bath reflux reaction. Set the reaction temperature, start timing when the temperature rises to 97°C, and close the reaction device after constant temperature reaction for 8 hours. Take out the aluminum sheet after the reaction, wash it with deionized water first, then with ethanol, and finally dry it at room temperature to obtain Ni 2+ -Al 3+ -LDHs@ZnAl-LDHs thin film aluminum sheet. The precipitate obtained after the reaction was then centrifuged and washed until the deionized water was clear, then washed three times with anhydrous ethanol, and dried at room temperature to obtain NiAl-LDHs-zC / D@ZnAl-LDHs powder. For simplicity, the prepared LDH s film is expressed in terms of concentration and ratio as NiAl-LDHs-zC / D@ZnAl-LDHs @Al (where z is Ni 2+ The proportion of total ions in the solution is C: 50mmol / L; D: 90mmol / L).

[0087] 1.2.3 Preparation of NiAl-x(surfactant)-LDHs@ZnAl-LDHs@Al

[0088] The aluminum sheet with the best corrosion resistance was selected from NiAl-LDHs-zC / D@ZnAl-LDHs and calcined at 400 °C for 4 hours in a muffle furnace in preparation for intercalation modification.

[0089] Weigh the surfactant solid powder to prepare a surfactant solution with a certain concentration, where SPT: 0.1 mol / L; SAS: 0.1 mol / L; SLS: 0.1 mol / L; SL: 0.05 mol / L [58,59] , respectively, to prepare 250mL solution. The calcined NiAl-LDHs-zC / D@ZnAl-LDHs sample was suspended in a round-bottom three-necked flask with a copper wire, and then the prepared surfactant solution was poured in to completely immerse the sample. After nitrogen was passed to exhaust the air in the system, the system was sealed and the experimental device was connected to start the reaction. When the temperature reached the boiling temperature of 98°C, the timing began. After eight hours of reaction, the power was turned off. The condensation device was turned off after the reaction solution was slightly cooled. After the solution temperature in the beaker dropped to room temperature, the prepared sample was taken out and named NiAl-SLS / SL / SPT / SAS-LDHs@ZnAl-LDHs.

[0090] 2. Study on the anti-corrosion properties of NiAl-LDHs@ZnAl-LDHs films prepared by in-situ growth on aluminum alloy surface

[0091] A ZnAl-LDHs film was in-situ grown on the surface of 6061 aluminum alloy using a hydrothermal synthesis method, and using it as the base layer, a NiAl-LDHs-@ZnAl-LDHs coating was in-situ constructed for dense filling. Through various test characterizations, it was found that the microstructure and corrosion resistance of the ZnAl-LDHs@Al and NiAl-LDHs-@ZnAl-LDHs@Al films prepared at different concentrations and metal ratios were significantly different. Although both ZnAl-LDHs@Al and NiAl-LDHs-@ZnAl-LDHs@Al films grow vertically to the substrate and completely cover the aluminum substrate, there are obvious differences in their morphological characteristics and corrosion resistance behaviors. When the total ion concentration is 50mmol / L and Zn 2+ :Al 3+ The ZnAl-LDHs-2-B synthesized under the conditions of a molar ratio of 2:1, and the total ion concentration of 90mmol / L, Ni 2+ :Al 3+ NiAl-LDHs-4-D@ZnAl-LDHs synthesized under a molar ratio of 4:1 has a smaller interlayer spacing and a stronger bonding force between its layers, resulting in a greater interlayer density. Therefore, ZnAl-LDHs-2-B and NiAl-LDHs-4-D@ZnAl-LDHs are given priority in subsequent modification research. LDHs have a significant enhancement effect on the corrosion resistance of 6061 aluminum alloy, and the corrosion resistance of LDHs also changes significantly with the change of its number of layers. Therefore, in the subsequent modification process, NiAl-LDHs-4-D@ZnAl-LDHs with the best effect was also selected for specific development.

[0092] 3. Effect of different anionic surfactants on intercalated NiAl-LDHs@ZnAl-LDHs coatings

[0093] 3.1 Characterization of LDHs

[0094] 3.1.1 Characterization of the tissue structure of LDHs

[0095] The crystal structure of NiAl-x(surfactant)-LDHs@ZnAl-LDHs@Al was studied by XRD, 10° / min, 3-80°; the functional group structure of NiAl-x(surfactant)-LDHs@ZnAl-LDHs@Al was studied by FT-IR, 4000-600cm -1 SEM was used to observe the morphology of the LDHs coating surface, and mapping was used to study the uniformity of the coating element distribution. XPS was also used to study the chemical composition of the LDHs coating surface, and the obtained data were fitted (avantage software), using carbon C1s (284.8eV binding energy) as the reference peak for calibration.

[0096] 3.1.2 Corrosion resistance test of LDHs coating

[0097] The corrosion resistance of the synthesized LDHs coating was evaluated by PDP and EIS electrochemical methods.

[0098] 3.3 Experimental Results and Discussion

[0099] 3.3.1 Micromorphology analysis of LDHs coating

[0100] like Figure 1 As shown, the SEM images of aluminum alloy plates covered with LDHs coatings prepared by different surfactants. Figure 1 It can be seen from (a) and (a') that the NiAl-LDHs@ZnAl-LDHs@Al coating grows well and has a uniform and dense lamellar structure. However, there are still small gaps on the surface, and these gaps have a certain depth. These gaps cause the structure of the prepared NiAl-LDHs@ZnAl-LDHs@Al coating to be not dense from bottom to top, but composed of a dense inner layer and a porous outer layer. Although the dense inner layer can hinder the penetration of corrosive media, the porous outer layer can provide space for corrosive media such as water, oxygen and chloride ions, which will increase the possibility of corrosive media penetration and coating failure. Therefore, it is necessary to prepare a dense LDHs coating from the outside to the inside. Figure 1 (b), (b'), (c), (c'), (d), (d') are the surface morphologies of NiAl-LDHs@ZnAl-LDHs@Al coatings after hydrothermal coprecipitation with the introduction of three surfactants. Compared with NiAl-LDHs@ZnAl-LDHs@Al coatings, the surface morphologies of LDHs coatings modified with different types and concentrations of surfactants have changed significantly. Figure 1 (b) and (b') are SEM images of NiAl-SL-LDHs@ZnAl-LDHs@Al coatings. It can be clearly seen that the original LDHs structure is more compact and its surface is slightly thickened compared to NiAl-LDHs@ZnAl-LDHs@Al, which further indicates that its surface is covered with laurate ions. Figure 1 (c) and (c') are SEM images of NiAl-SPT-LDHs@ZnAl-LDHs@Al coatings. It can be seen from the images that the pores on the surface are smaller and fewer, and these pores are filled with interwoven LDHs sheets. Figure 1From the pores in (d) and (d'), we can see that the LDHs sheets in the LDHs coating modified by anionic surfactants have obvious lamellar structures and the LDHs sheets are obviously bent. These bent LDHs sheets are interwoven to form a flower-like structure, which is consistent with previous reports. The above results show that the surface of the LDHs coating can be modified by anionic surfactants to regulate the morphology of the LDHs coating and prepare a dense coating structure.

[0101] 3.3.2 Composition and hydrophobic properties of LDHs coating

[0102] (1) Composition analysis of LDHs coating

[0103] Figure 2 , 3 Figures 4 and 5 are the XPS narrow spectra of several main components of NiAl-SL-LDHs@ZnAl-LDHs@Al, NiAl-SPT-LDHs@ZnAl-LDHs@Al and NiAl-SLS-LDHs@ZnAl-LDHs@Al coatings on the surface of 6061 aluminum alloy. In these LDHs coatings, the peak at 74.6 eV of the Al 2p spectrum indicates that the Al in the NiAl-LDH film mainly exists in the form of Al-O with a chemical state of +3. Another peak at 68.8 eV can be attributed to Ni 3p. The narrow spectra of Zn elements on the surfaces of NiAl-SL-LDHs@ZnAl-LDHs@Al and NiAl-SLS-LDHs@ZnAl-LDHs@Al are shown in Figure 5. Figure 2 b and 4b. According to the XPS database and literature, the peaks of ZnO and LDHs appear at 1021.2 and 1022.7 eV, respectively, and the Zn signal is weak. The absence of Zn signal in NiAl-SPT-LDHs@ZnAl-LDHs@Al means that the NiAl-LDH film completely covers the substrate. The narrow spectra of Ni element on the surface of NiAl-SL-LDHs@ZnAl-LDHs@Al and NiAl-SLS-LDHs@ZnAl-LDHs@Al are shown in Figure 4. Figure 2 c and 4c. Ni matches Ni 2p3 / 2 and Ni 2p1 / 2 at 857.0eV and 874.8eV, respectively. A satellite peak was detected for each main peak. These results indicate that Ni exists in the form of Ni-O with a chemical state of +2. For the NiAl-SL-LDHs@ZnAl-LDHs@Al coating, the C 1s spectrum ( Figure 2 d) 284.8eV represents the binding energy of CC / CH, 288.3eV represents the binding energy of -COO-; O1s( Figure 2e) The binding energies near 530.65 eV, 531.55 eV and 532.25 eV in the spectrum can be attributed to O=M, HO and -COO-, respectively. For the NiAl-SPT-LDHs@ZnAl-LDHs@Al coating, the C 1s spectrum ( Figure 3 c) 284.8eV represents CH and CC(sp3) and CC(sp2) from benzene ring, 288.75eV represents the binding energy of CS; O1s spectrum ( Figure 3 The binding energies at 530.2 eV, 531.85 eV and 533.3 eV in d) can be attributed to O=M, OH and -SO3, respectively; the S2p spectrum ( Figure 3 e) 167.28eV and 168.65eV represent S2p1 / 2 and S2p3 / 2 in the sulfonic acid group, respectively. For the NiAl-SLS-LDHs@ZnAl-LDHs@Al coating, the C 1s spectrum ( Figure 4 c) 284.8eV represents the binding energy of CC / CH, and 286.3eV represents the binding energy of CS; O1s spectrum ( Figure 4 The binding energies at 530.2 eV, 531.08 eV, 531.6 eV and 532.9 eV in d) can be attributed to O=M, HO and -OSO3, respectively. The S2p spectrum ( Figure 4 e) 167.3eV represents S2p3 / 2 in the sulfonic acid group. The above results show that the surfactants SL, SPT and SLS are involved in the formation of LDHS. Comparing the distribution of the peaks of the same element in different coatings, it can be found that the bonding in different coatings is not exactly the same, so the peaks of binding energy are not exactly the same.

[0104] (2) Contact angle of LDHs coating

[0105] The static contact angle (CA) of all LDHs coatings synthesized in this chapter was tested using a contact angle tester. The results are as follows: Figure 5As shown. In order to ensure the certainty of the test results, each sample was tested at five different positions, the values ​​with large deviations were removed, and the other data were averaged to obtain the final data results. On this basis, the static contact angles of different film materials were obtained. Since the surface of the NiAl-LDHs@ZnAl-LDHs@Al coating contains abundant hydroxyl groups, the coating is hydrophilic, and the CA is only 27.3°. For the LDHs coating based on surfactant modification, it can be seen from the figure that the contact angles of NiAl-LDHs@ZnAl-LDHs@Al, NiAl-SL-LDHs@ZnAl-LDHs@Al, NiAl-SPT-LDHs@ZnAl-LDHs@Al and NiAl-SLS-LDHs@ZnAl-LDHs@Al coatings are 71°, 111°, 75° and 138.6°, respectively, which shows that these anionic surfactants can modify the surface of LDHs to make the LDHs coating change from hydrophilic to hydrophobic, especially SL and SLS. Therefore, the preparation method in this chapter can greatly enhance the hydrophobic properties of the double-layer NiAl-LDHs@ZnAl-LDHs@Al coating.

[0106] 3.3.3 Corrosion resistance analysis of LDHs coating

[0107] like Figure 6 The EIS spectra and polarization curves of the aluminum alloy coated with NiAl-LDHs@ZnAl-LDHs without anionic surfactant and the NiAl-x(surfactant)-LDHs@ZnAl-LDHs coating prepared by surface covering anionic surfactant in 3.5% NaCl solution. Figure 6From the Nyquist plot of (a), it can be clearly seen that among these surfactant-based LDHs coatings, only the semicircle radius of the low-frequency capacitance arc of NiAl-SLS-LDHs@ZnAl-LDHs@Al is significantly larger than that of the low-frequency capacitance arc of NiAl-LDHs@ZnAl-LDHs@Al coating. In the Bode plot, the low-frequency impedance value of the coating is also only that of NiAl-SLS-LDHs@ZnAl-LDHs@Al is significantly larger than that of NiAl-LDHs@ZnAl-LDHs@Al coating. This is mainly because the dodecyl sulfonate ions can be fully intercalated into NiAl-LDHs@ZnAl-LDHs, while the corresponding laurate ions and p-toluene sulfonate ions of NiAl-SL-LDHs@ZnAl-LDHs@Al and NiAl-SPT-LDHs@ZnAl-LDHs@Al do not enter the NiAl-LDHs@ZnAl-LDHs interlayers, but only act on their surfaces. The results show that, combined with the large phase angle exhibited by NiAl-SLS-LDHs@ZnAl-LDHs@Al at lower frequencies, the sample has good capacitive and dielectric properties.

[0108] Figure 7 It is an equivalent circuit model diagram used to simulate the EIS data of ZnAl-LDHs and NiAl-LDHs@ZnAl-LDHs. sol is the solution resistance of the electrolyte; CEP LDHs With R LDHs is the time constant associated with the LDHs coating, where R LDHs represents the resistance of the LDHs coating; using CEP S and R S The second time constant in the mid-frequency region is represented in parallel, corresponding to the capacitance and resistance of the Al2O3 film respectively; CPE dl and R CT Charge transfer resistance is the double layer capacitance. In order to better fit the experimental data, CPE is used instead of capacitors to compensate for the inhomogeneity in the system. The impedance of CPE is given by ZCPE = [Y(jω)n] -1 Calculated as follows, where Y is the CPE constant, ω is the frequency, and n is a dimensionless index (0≤n≤1). When n is 0 and 1, CPE is pure resistance and pure capacitance, respectively. Since the electrochemical situation of the NiAl-x (surfactant)-LDHs@ZnAl-LDHs sample is more complicated, immersing the sample in the solution will form an absolutely hydrophobic "air film" on its surface, so CPEair is introduced to represent the trapped air.

[0109] like Figure 8The polarization curves of the aluminum alloy covered with the NiAl-LDHs@ZnAl-LDHs coating without the addition of anionic surfactant and the NiAl-x(surfactant)-LDHs@ZnAl-LDHs coating prepared by the surface covering anionic surfactant in 3.5% NaCl solution are shown in Table 3-1. The specific corrosion potential (Ecorr) and corrosion current (Icorr) values ​​are shown in Table 3-1. Generally speaking, the higher the corrosion potential (Ecorr), the lower the corrosion current (Icorr), and the greater the corrosion resistance.

[0110] The Icorr value of NiAl-LDHs@ZnAl-LDHs is (2.164E-5A / cm-2), while the lowest Ecorr reaches (-0.727V), indicating that the corrosion resistance of NiAl-LDHs@ZnAl-LDHs is average. As different surfactants are inserted between the LDHs layers on the surface of aluminum alloy, the corresponding corrosion properties of different coatings change significantly. Among the three types of surfactant-intercalated LDHs coatings, NiAl-SLS-LDHs@ZnAl-LDHs@Al exhibits the highest Ecorr (-0.582V) and a lower Icorr (1.657E-4A / cm2) than NiAl-LDHs@ZnAl-LDHs. Although the corrosion voltages of NiAl-SL-LDHs@ZnAl-LDHs (-0.718V) and NiAl-SPT-LDHs@ZnAl-LDHs@Al (-0.712V) are greater than

[0111] The Icorr of NiAl-LDHs@ZnAl-LDHs@Al (-0.727V), but NiAl-SL-LDHs@ZnAl-LDHs@Al (5.818E-5A / cm-2) is significantly greater than that of NiAl-LDHs@ZnAl-LDHs@Al. This indicates that the hydrophobic properties of NiAl-SPT-LDHs@ZnAl-LDHs and NiAl-SLS-LDHs@ZnAl-LDHs@Al are helpful to inhibit the corrosion reaction.

[0112] NiAl-SL-LDHs@ZnAl-LDHs@Al has a certain promoting effect on the corrosion voltage, but has a certain effect on I corr There is a certain inhibitory effect. The higher the Icorr, the weaker the corrosion resistance and the higher the ion adsorption capacity. According to the test data obtained, among the three different LDHs layers, the NiAl-SLS-LDHs@ZnAl-LDHs@Al layer exhibits the best corrosion resistance.

[0113] Table 3-1. Electrochemical parameters of LDH layers prepared with different surfactants in 3.5% NaCl solution NaCl solution

[0114]

[0115]

[0116] 3.4 Summary

[0117] Different anionic surfactants (including SLS, SPT and SL) were introduced on the surface of aluminum alloy with in situ growth of double-layer LDHs (NiAl-LDHs@ZnAl-LDHs), and different NiAl-x (surfactant)-LDHs@ZnAl-LDHs@Al coatings were prepared on the surface of 6061 aluminum alloy. The crystal structure and composition of the synthesized LDHs were analyzed by XRD and FTIR. The composition, structure and morphology of the LDHs coating were studied by XPS, SEM, etc. The corrosion resistance of the coating was studied by electrochemical test. The research results are as follows:

[0118] (1) After the anionic surfactant modification process of NiAl-LDHs@ZnAl-LDHs, the anionic surfactant containing a long carbon chain can be modified on the LDHs and play a hydrophobic modification role on the LDHs coating;

[0119] (3) The LDHs coating prepared based on anionic surfactants has a denser and more hydrophobic coating structure than the NiAl-LDHs@ZnAl-LDHs coating, and the coating has good bonding performance with the metal substrate; therefore, the LDHs coating prepared based on anionic surfactants has better corrosion resistance than the NiAl-LDHs@ZnAl-LDHs coating;

[0120] (4) The addition of anionic surfactants has a great influence on the morphology of the synthesized NiAl-LDHs@ZnAl-LDHs coating. The coating surface changes differently with the addition of different anionic surfactants, and its surface density and hydrophobic properties are also different. From the experimental results, the addition of sodium dodecyl sulfate also greatly enhances the corrosion resistance of the sample.

[0121] 4. Study on the corrosion resistance and self-healing properties of SLS intercalated NiAl-LDHs@ZnAl-LDHs coating

[0122] 4.1 Characterization of LDHs

[0123] 4.1.1 Characterization of the organizational structure of LDHs

[0124] XRD studies the crystal structure of aluminum alloy substrate and different LDHs coatings on the surface, 10° / min, 3-80°; FTIR studies the functional group structure of aluminum alloy substrate and different LDHs coatings on the surface, 4000-600cm -1 . SEM was used to observe the morphology of the surface of different LDHs coatings, and mapping was used to study the uniformity of the element distribution of the coatings. XPS was also used to study the surface chemical composition of NiAl-SLS-LDHs@ZnAl-LDHs@Al coatings. All XPS data were fitted using XPS peak4.1 software, using the Tougaard background fitting method, and using carbon C1s (284.8 eV binding energy) as the reference peak for calibration.

[0125] 4.1.2 Corrosion resistance test of LDHs coating

[0126] The corrosion resistance of the synthesized LDHs coating was evaluated by PDP and EIS electrochemical methods.

[0127] The chemical stability of aluminum alloy substrate and different LDHs coatings on the surface was studied. The coating NiAl-SLS-LDHs@ZnAl-LDHs@Al was immersed in 3.5wt% NaCl solution, and the morphology and electrochemical detection were carried out when the morphology changed. The surface morphology of the sample was observed to evaluate the corrosion resistance of the sample. The NiAl-SLS-LDHs@ZnAl-LDHs@Al was artificially scratched, and the self-healing performance was studied under certain conditions.

[0128] 4.2 Experimental Results and Discussion

[0129] 4.2.1 XRD and FTIR of LDHs

[0130] XRD spectra of aluminum alloy and different LDHs layers on the surface Fig. 9 After growing ZnAl-LDHs on aluminum alloy, the characteristic diffraction peaks of 003 and 006 of LDHs were observed. The diffraction peaks are narrow and strong, indicating that the ZnAl-LDHs film material on the outer layer of aluminum alloy has high crystallinity and a layered structure ( Fig. 9 ab). In addition, no other crystal diffraction peaks of ZnAl-LDHs@Al were detected, indicating that ZnAl-LDHs are single-phase LDHs. In addition, the diffraction peaks of the aluminum matrix metal aluminum phase were detected in NiAl-LDHs@ZnAl-LDHs@Al.

[0131] NiAl-LDHs further grows on the outer layer of ZnAl-LDHs to form a NiAl-LDHs@ZnAl-LDHs composite film, and the 003 diffraction peak of the product is enhanced, indicating that the surface of ZnAl-LDHs@Al is loaded with NiAl-LDHs. In contrast, the diffraction peak of the aluminum phase of the aluminum-based metal decreases. This is because the presence of two layers of Zn-Al-LDHs and Ni-Al-LDHs materials leads to an increase in the film thickness, which shields the detection of the aluminum substrate. The (003) base spacings of Zn-Al-LDHs@Al and Ni-Al-LDHs@Zn-Al-LDHs@Al are 0.725nm and 0.760nm, respectively. In order to enhance the hydrophobic properties of the composite material, Ni-Al-LDHs@Zn-Al-LDHs@Al was hydrophobically modified, and the XRD spectrum of the product is shown in the figure. Fig. 9 As shown in Figure d, the interlayer distance of the product increased from 0.760nm to 0.945nm, which was mainly due to the insertion of SLS hydrophobic groups with large molecular radius between the LDHs layers.

[0132] Fourier transform infrared spectroscopy was used to analyze the structural changes of various LDHs materials on the aluminum substrate and the changes in interlayer anions ( Fig.10 Since the aluminum alloy substrate has no supporting film material, it does not show any absorption peak in the infrared spectrum ( Fig.10 After ZnAl-LDHs and NiAl-LDHs were formed on pure aluminum substrate, multiple absorption peaks appeared ( Fig.10 bc), the absorption peak is located at 3650-3350cm -1 Between, the center is located at 3450cm -1 , attributed to the OH stretching vibrations of interstitial H2O molecules and hydroxyl-OH groups. 1299cm -1 The infrared peak at 100 nm is attributed to the characteristic vibration mode of carbonate ions, indicating the presence of this anion in the LDHs layer. Other peaks found at lower wavenumbers are related to the Al-O and Ni-O vibrations in the LDHs lattice, respectively.

[0133] It should be emphasized that after hydrophobic modification, the product of NiAl-LDHs@ZnAl-LDHs@Al is at 2928 cm -1 and 2870cm -1 There are two absorption vibration peaks at ( Fig.10 d), mainly due to the CH 2- and CH 3- absorption vibration peak. At the same time, at 1139cm -1 There is an absorption peak at the dodecylsulfonate ion structure. 3-The results show that the dodecyl sulfonate was successfully inserted into the LDHs layer prepared on the aluminum alloy by calcination and composite. Fig. 9 The XRD results shown are consistent. The analysis further shows that the two LDHs were successfully grown on the aluminum substrate and successfully assembled through SLS intercalation, achieving the purpose of hydrophobic modification.

[0134] 4.2.2 Morphology analysis of LDHs coating

[0135] Fig.11 , 12 SEM and EDS images of different LDHs coatings are shown. Fig.11 It can be seen from the a and 12ZnAl-LDHs@Al images that the lamellar structure in the ZnAl-LDHsl coating structure is large and thick, and there are large gaps in the lamellar structure. The ZnAl-LDHs coating structure grows vertically to the aluminum substrate, which is mainly attributed to the spatial domain effect, and also shows that the binding of ZnAl-LDHs to the aluminum substrate is stronger. In order to compensate for the shortcomings of the uneven surface structure and large lamellar structure of ZnAl-LDHs@Al, NiAl-LDHs with a smaller lamellar structure are grown on the surface of the ZnAl-LDHs film for filling ( Fig.11 b) From Fig.12 It can be seen from the EDS spectrum of NiAl-LDHs that Ni and Al elements are evenly covered on the surface of ZnAl-LDHs@Al film, and the lamellar structure of NiAl-LDHs is finer, denser, and more complete, which improves the overall density and uniformity of the coating. Fig.11 c is the SEM image of the NiAl-SLS-LDHs@ZnAl-LDHs@Al coating. As can be seen from the figure, the NiAl-SLS-LDHs@ZnAl-LDHs@Al film material after SLS hydrophobic modification is dense and has almost no pores. Combined with the distribution of elements such as S and C, after three stages of treatment (ZnAl-LDHs, NiAl-LDHs and NiAl-SLS-LDHs), the entire aluminum alloy substrate surface is covered with the modified LDHs film, which further improves the material's anti-corrosion performance on the substrate.

[0136] Fig.12 These are mapping images of different LDHs coatings. The distribution of elements in the coating can be studied through the coating element mapping images. From the element map of ZnAl-LDHs@Al ( Fig.12) It can be seen that Al and Zn elements are uniformly distributed on the surface of the aluminum matrix, which further indicates that ZnAl-LDHs is in situ grown on the surface of the Al matrix, which is consistent with the results of SEM observation. It is worth noting that we found that the nickel distributed on the surface of NiAl-LDHs@ZnAl-LDHs@Al is attributed to the growth of Ni-Al-LDHs (second layer) on Zn-Al-LDHs@Al. Ni element ( Fig.12 The uniform distribution of NiAl-LDHs@ZnAl-LDHs@Al also proves that Ni-Al-LDHs are evenly and densely distributed on the surface of ZnAl-LDHs@Al. The S element in SLS ( Fig.12 NiAl-SLS-LDHs@ZnAl-LDHs@Al), which further proves that SLS is successfully inserted into the outer Ni-Al-LDHs interlayer, corresponding to the results of FT-IR and XRD analysis.

[0137] XPS (such as Fig.13 ) further confirmed the distribution of elements in NiAl-SLS-LDHs@ZnAl-LDHs@Al. Al 2p( Fig.13 a) The spectrum shows a peak at 74.2 eV. Zn2p1 / 2 and Zn 2p3 / 2 ( Fig.13 b) are located at 1045.0 and 1022.1 eV, suggesting the existence of ZnAl-LDHs, which is consistent with the literature reports. Fig.13 c) There is a Ni(OH)2 peak at 855.6 eV, and two satellite peaks at 879.4 and 861.6 eV. Fig.13 d is the spectrum of C1s, where the fitted peaks at 284.8 and 288.5 eV are due to -CH2 and CO3, respectively. 2- The presence of these -CH2 groups. The reason for detecting these -CH2 is that some CH3(CH2) 11 SO3 - (SLS - ) were adsorbed and inserted into the NiAl-LDHs membrane.

[0138] The O1s spectrum is mainly composed of three peaks ( Fig.13 e). The presence of oxygen in the metal hydroxide results in a peak at 531.6 eV, the presence of a C=O bond results in a peak at 531.6 eV, and in addition, a peak at 532.4 eV ( Fig.13 e) corresponds exactly to the water molecules adsorbed on the film. Combined with the XPS results of S ( Fig.13f) It can be seen that the peak at 168.4 eV is related to oxygen-containing sulfur (thiosulfate, sulfate). The appearance of these two peaks proves the presence of CH3(CH2) on the surface of NiAl-SLS-LDHs@ZnAl-LDHs@Al 11 SO3 - .

[0139] The morphology and roughness of ZnAl-LDHs films were measured by AFM. Fig.14 The surface structure is thick and flake-like, about 3um in length and 1um in thickness, and the surface is very rough. The surface average roughness Ra is about 400nm, and the surface root mean square roughness Rq is about 350nm. Select a layer structure, make a force curve on it, select the Herz model, and automatically fit the modulus to be about 12.6GPa. The mechanical properties are good, which is mainly because LDHs belongs to the hexagonal crystal system and there is Al in the layer structure unit. 3+ and OH - The octahedral unit can provide important growth points for LDHs by sharing O, ensuring strong adhesion between the LDHs film and the substrate. This shows that the ZnAl-LDHs film has good bonding with the metal substrate.

[0140] like Fig.15 This is an atomic force microscope image of NiAl-LDHs@ZnAl-LDHs. The surface structure is petal-shaped, with each cluster of about 5um. The fine structure above is flaky, and the surface roughness is lower than that of ZnAl-LDHs. The average surface roughness Ra is about 230nm, and the surface root mean square roughness Rq is about 200nm. Select a flat area, make a force curve on it, select the Herz model, and automatically fit the modulus to about 6.56GPa. The bonding force is less than that of the ZnAl-LDHs film. This is mainly due to the problem of in-situ growth of the bonding layer of NiAl-LDHs.

[0141] Contact angle measurements can be used to demonstrate the hydrophobic properties of a sample surface. The contact angle between a material and a water droplet is a standard method for determining the hydrophobicity of a material. Materials with large contact angles are highly hydrophobic, which provides them with good corrosion protection. In order to ensure the certainty of the test results, we tested each sample at five different locations, removed the values ​​with large deviations, averaged the other data, and obtained the final data results. On this basis, the static contact angles of different thin film materials were obtained. The contact angle of the aluminum substrate surface is 59.6° ( Fig.16). Since the surface of the LDHs coating contains abundant hydroxyl groups, the coating is hydrophilic. The overall test showed that the CA value of ZnAl-LDHs@Al was 71°. NiAl-LDHs@ZnAl-LDHs@Al contains more hydroxyl groups under the same area conditions than ZnAl-LDHs with larger and thicker structures due to the filling and coverage of the smaller and thinner NiAl-LDHs. Therefore, its CA value dropped to 28.2°, which also shows that the filling effect of NiAl-LDHs on the surface of ZnAl-LDHs@Al is obvious. The shape of the water droplet on the surface of the NiAl-SLS-LDHs@ZnAl-LDHs@Al material obtained by surfactant intercalation in the later stage remained completely unchanged, and the contact angle increased to 138.6°( Fig.16 ). This indicates that NiAl-SLS-LDHs@ZnAl-LDHs@Al has high hydrophobicity and increases the anti-corrosion performance of the coated aluminum substrate material.

[0142] 4.2.3 Corrosion resistance analysis of LDHs coating

[0143] In order to further explore the corrosion resistance of aluminum substrates with different coatings, electrochemical tests were carried out. Fig.17 The polarization curves and EIS spectra of different LDHs coatings on aluminum alloy surfaces in 3.5% wt. NaCl solution are shown in Figure 2. The results show that the impedance of the bare aluminum alloy substrate is extremely low, and the capacitance radius reactance arc is very small at high frequencies (e.g. Fig.17 a). It was observed that all four samples showed obvious loops, and the order of curvature radius was

[0144] NiAl-SLS-LDHs@ZnAl-LDHs@Al>NiAl-LDHs@ZnAl-LDHs@Al>Zn-Al-LDHs>aluminum alloy matrix. The NiAl-SLS-LDHs@ZnAl-LDHs@Al material exhibits the largest curvature, indicating that it has better corrosion resistance. At lower frequencies, especially at 0.01Hz, the higher the impedance value, the greater the corrosion resistance of the material. Fig.17 b shows the frequency-impedance plot of these materials, where the four curves are widely spaced, especially in the low-frequency range, demonstrating the large differences in the material impedances. Fig.17 c is Fig.17 The Nyquist plot in a is combined with a phase-frequency plot showing two time constants. The first time constant in the mid-frequency range (100-10 4 Hz) can be attributed to the oxide film between the aluminum substrate surface and the LDHs layer; the second time constant (>10 4 Hz) corresponds to the response of the LDHs film.

[0145] Since the coatings on the aluminum alloys studied in this chapter are different, three different equivalent circuit diagrams ( Fig.18 , 19 and 20) to simulate the EIS data of different coatings on 6061 aluminum alloy. Fig.18 The representative is the equivalent circuit diagram of the EIS data obtained for bare aluminum alloy in 3.5%wtNaCl solution, where the inductor component (L) and the inductor impedance (R L ) indicates the inductance loop that appears in the low-frequency region; CPE dl is a constant phase element; R s Represents the resistance of the electrolyte solution; R CT represents the charge transfer resistance, which corresponds to the process of charge transfer from the substrate to the surface.

[0146] Fig.19 This is an equivalent circuit diagram used to simulate the EIS data of ZnAl-LDHs@Al and NiAl-LDHs@ZnAl-LDHs@Al. NiAl-SLS-LDHs@ZnAl-LDHs@Al is compared with ZnAl-LDHs@Al and

[0147] The electrochemical reaction of the NiAl-LDHs@ZnAl-LDHs@Al sample is more complicated. Considering the absolute hydrophobicity of its surface, when it is immersed in the solution, a layer of "air film" will automatically form between its surface and the atmosphere. CPEair is introduced to represent the captured air. The corresponding equivalent circuit diagram is shown in Fig. 20 .

[0148] like Fig.21 The polarization curves of aluminum alloy and different LDHs coatings on its surface in 3.5% NaCl solution are shown in Table 4-1. The specific corrosion potential and corrosion current values ​​are shown in Table 4-1. Generally speaking, the higher the Ecorr, the lower the Icorr, and the better the corrosion resistance. The bare aluminum substrate has the highest Icorr value (1.854E-3A / cm 2 ), while Ecorr reaches (-0.686V), indicating that the corrosion resistance of bare aluminum alloy is poor. As LDHs grow on the aluminum substrate, the corrosion properties of different coatings change significantly. Among the three types of LDHs layers, NiAl-SLS-LDHs@ZnAl-LDHs@Al exhibits the highest Ecorr (-0.582V) and lower Icorr (1.657E-4A / cm2) than the bare aluminum substrate. 2 ). A higher corrosion current means weaker corrosion resistance and higher ion adsorption capacity. According to the test data obtained, among the three different LDHs layers, the NiAl-SLS-LDHs@ZnAl-LDHs@Al coating showed the best corrosion resistance. This means that its hydrophobic properties seem to help inhibit corrosion.

[0149] Table 4-1. Electrochemical parameters of aluminum alloy matrix and its different LDHs layers in 3.5% NaCl solution

[0150]

[0151] Due to Cl - It is easily adsorbed by metals, so metals are - The test sample was immersed in 3.5% NaCl solution for a certain period of time, and then the corrosion of the sample was observed by SEM. Fig. 22 The SEM micrographs of the samples after being immersed in 3.5% NaCl solution for different time periods at room temperature. Fig. 22 a It can be seen that the aluminum substrate has corrosion pinholes after immersion for 15 days, and its corrosion resistance is poor. Fig. 22 b) After 15 days of immersion, it shows slight changes and some corrosion pinholes can be seen on the film surface. Fig. 22 c shows the morphology of NiAl-LDHs@ZnAl-LDHs@Al after immersion in the solution for 15 days, and no obvious collapse or corrosion pinholes are observed. In contrast, the hydrophobically modified NiAl-SLS-LDHs@ZnAl-LDHs@Al film ( Fig. 22 d) There was no obvious change in the surface and no corrosion was detected after immersion for 15 days.

[0152] After ZnAl-LDHs@Al film was immersed in NaCl solution for 27 days, the surface crystal structure ( Fig. 22 b) collapsed and became loose, indicating that the corrosion resistance of the Zn-Al-LDHs film was damaged due to long-term immersion. After immersion for 27 days, many corrosion pinholes appeared on the surface of the NiAl-LDHs@ZnAl-LDHs@Al film ( Fig. 22 c), the corrosion resistance decreased. However, after immersion for 27 days, the surface of NiAl-SLS-LDHs@ZnAl-LDHs@Al film ( Fig. 22 d) remains unchanged, indicating that the superhydrophobic NiAl-SLS-LDHs@ZnAl-LDHs@Al film has good long-term corrosion resistance.

[0153] Fig.23Schematic diagram of the anticorrosion structure of NiAl-SLS-LDHs@ZnAl-LDHs@Al in NaCl solution. First, the relative coating thickness of ZnAl-LDHs@Al and the dense filling of NiAl-LDHs produce a composite film of two LDHs, thus forming a uniform, dense, continuous and complete film on the surface of the aluminum alloy. This can more effectively prevent the penetration of corrosive ions and improve the survivability of the substrate in a corrosive environment ( Fig.23 a).

[0154] Secondly, SLS was introduced into the interlayer of NiAl-LDHs@ZnAl-LDHs@Al to form a monomolecular hydrophobic layer on the surface of LDHs, in which the hydrophilic groups faced the substrate and the hydrophobic groups faced the medium ( Fig.23 b) When NiAl-SLS-LDHs@ZnAl-LDHs@Al is in the presence of H2O molecules and corrosive Cl - When in an ion environment, the long carbon chain of SLS extends outward to generate spatial repulsion and forms an air film layer on the hydrophobic surface of the outermost LDHs to prevent the penetration of water molecules and chlorides, thereby protecting the metal substrate. On the other hand, we believe that the large radius SLS in the LDHs layer can increase the interlayer spacing, thereby effectively enhancing the capture and storage capacity of chloride ions. To prove this point, the ability of these two coatings (NiAl-LDHs@ZnAl-LDHs@Al and NiAl-SLS-LDHs@ZnAl-LDHs@Al) to capture chloride ions was studied. The results show that the ability of the NiAl-SLS-LDHs@ZnAl-LDHs@Al coating to capture and adsorb chloride ions is more than twice that of the coating without SLS inserted (0.68% / 0.30% in Table 4-2).

[0155] Table 4-2 EDS element content results of aluminum alloy matrix and different LDHs layers after immersion in 3.5% NaCl solution for 27 days

[0156]

[0157] More importantly, the two different types of LDHs coatings can act as anion micro-nano containers to intelligently adsorb and store chloride ions and effectively adapt to environments with different chloride ion concentrations. - When the concentration reaches a certain value, SLS begins to be displaced into the solution and the following reaction occurs ( Fig.23 c):

[0158] NiAl-SLS - -LDHs+2Cl - →NiAl-2Cl - -LDHs+SLS - (1)

[0159] Only when the hydrophobic air film is destroyed to a certain extent and the Cl - As the concentration continues to increase, a large amount of Cl - In order to enter the interlayer of NiAl-LDHs, water can enter. At this stage, the NiAl-LDHs on the top of the coating act as the first layer storage container for corrosive anions, while the next layer of ZnAl-LDHs coating will not be activated as a reserve corrosive anion container. Even if the substrate continues to be in high Cl - solution, resulting in Cl between NiAl-LDHs layers - The concentration reaches the saturation value, and the excess Cl - It will also enter the interlayer of ZnAl-LDHs coating, ( Fig.23 d). The replacement process is as follows:

[0160] ZnAl-CO3 2- -LDHs+2Cl - →ZnAl-2Cl - -LDHs+CO3 2- (2)

[0161] It is worth noting that once part of the Cl - Entering into the ZnAl-LDHs layer, Cl in the NiAl-LDHs layer - The concentration will decrease, which is due to the ZnAl-LDHs - As we all know, the anion priority order is: CO3 2- >SO4 2- >OH - >F - >Cl - >Br - >NO3 - , so the most preferred anion will lead to a more stable LDHs structure. In addition, due to CO3 2- The strong affinity between the NiAl-LDHs layer and the Cl - By ambient CO3 2- exchanged into the corrosive solution, resulting in some Cl - Reverse direction away from the aluminum substrate ( Fig.23 e). In this case, it is difficult for a large amount of chloride ions to penetrate into the aluminum substrate through the thicker ZnAl-LDHs coating. Therefore, both different types of LDHs composite structure coatings have the ability to intelligently store and distribute chloride ions, can adapt to different concentrations of chloride ions in the environment, and enhance the corrosion resistance of the composite coating material.

[0162] In addition, the self-healing property of this NiAl-SLS-LDHs@ZnAl-LDHs@Al coating material is also an important advantage. In order to verify the self-healing ability of the coating, a knife was used to physically damage the surface in the diagonal direction ( Fig.24 a). From the element distribution diagram ( Fig.25 The C, O, Ni, and Zn in the left image can also be clearly seen. The NiAl-SLS-LDHs@ZnAl-LDHs on the aluminum substrate surface after damage is obviously cracked. The material is then immersed in an alkaline environment containing aluminum ion salt and nickel ion salt. After 10 days, the scratches are self-covered and regenerated. Fig.24 b and Fig.24 c. The elemental mapping of the self-healing NiAl-SLS-LDHs@ZnAl-LDHs@Al also shows that C, O, Ni, Zn, and Al are evenly distributed after self-healing ( Fig.25 Right), no scratch marks appear in the diagonal direction, indicating that the composite coating material self-repairs again at the scratch, proving the self-repairing performance of NiAl-SLS-LDHs@ZnAl-LDHs@Al. This self-repairing may be attributed to the dissolution and recrystallization process of the film material in a saline-alkali environment. In addition, the amorphous phase and part of the film edge in the aluminum plate anodic / micro-arc oxidation film at the scratch will dissolve under alkaline conditions, providing an ion source for the reconstruction of the LDHs film. LDHs can be grown in situ using the aluminum alloy anodic / micro-arc oxidation film to self-repair the sealing coating.

[0163] Fig.26 The EIS and PDP spectra of regenerated and scratched NiAl-SLS-LDHs@ZnAl-LDHs@Al are shown. The results show that the scratched NiAl-SLS-LDHs@ZnAl-LDHs@Al has extremely low impedance and a very small capacitance radius reactance arc at high frequencies (e.g. Fig.26 a). It is observed that both samples exhibit obvious loops, and the curvature radius of the regenerated NiAl-SLS-LDHs@ZnAl-LDHs@Al is much larger than that of the scratched NiAl-SLS-LDHs@ZnAl-LDHs@Al, indicating that it has better corrosion resistance. Fig.26 (b) shows the frequency-impedance plot for the two materials, where the two curves are widely spaced, especially in the low-frequency range, demonstrating the large difference in material impedance. Fig.26 (c) is related to Fig.26 The Nyquist plot in (a) is combined with the phase-frequency plot, where two time constants are observed. The first time constant at the intermediate frequency (10-10 4 Hz) is caused by the oxide film between the aluminum substrate surface and the LDHs layer; the second time constant (>10 4Hz) corresponds to the response of LDHs film. Fig.26 (d) shows the polarization curves and EIS spectra of regenerated and scratched NiAl-SLS-LDHs@ZnAl-LDHs@Al. The specific parameters of corrosion current and corrosion potential are shown in Table 4-3. It can be seen from Table 4-3 that the Icorr (1.528E-4A / cm2) of the regenerated NiAl-SLS-LDHs@ZnAl-LDHs@Al is significantly lower than that of the scratched NiAl-SLS-LDHs@ZnAl-LDHs@Al (7.966E-4A / cm2). At the same time, the Ecorr of the regenerated NiAl-SLS-LDHs@ZnAl-LDHs@Al is significantly improved to -0.623V. Compared with the Ecorr (-0.678V) of the scratched NiAl-SLS-LDHs@ZnAl-LDHs@Al, the regenerated

[0164] The Ecorr value of NiAl-SLS-LDHs@ZnAl-LDHs@Al increased significantly. This may be attributed to the regeneration

[0165] The self-healing effect of NiAl-SLS-LDHs@ZnAl-LDHs@Al repaired the corroded parts to a certain extent. The results showed that the regeneration by immersion method could repair the damaged NiAl-SLS-LDHs@ZnAl-LDHs@Al and restore its anti-corrosion ability to a certain extent.

[0166] Table 4-3 Electrochemical parameters of regenerated and scratched NiAl-SLS-LDHs@ZnAl-LDHs@Al

[0167]

[0168] 4.3 Summary

[0169] Various types of LDHs thin film materials (ZnAl-LDHs@Al, NiAl-LDHs@ZnAl-LDHs@Al and NiAl-SLS-LDHs@ZnAl-LDHs@Al) were successfully prepared by in-situ growth technique. Compared with ZnAl-LDHs@Al, NiAl-LDHs@ZnAl-LDHs@Al coatings are very dense and have much fewer pores. SLS-modified NiAl-LDHs@ZnAl-LDHs@Al thin film (NiAl-SLS-LDHs@ZnAl-LDHs@Al) materials have high contact angles, showing their better hydrophobic properties. The anti-corrosion properties of ZnAl-LDHs@Al, NiAl-LDHs@ZnAl-LDHs@Al and NiAl-SLS-LDHs@ZnAl-LDHs@Al composite coatings were investigated using potentiodynamic polarization curves and EIS analysis. The results of this work show that the corrosion resistance of LDHs coatings is significantly enhanced compared with that of bare aluminum alloys. Among the three LDHs films, the hydrophobic NiAl-SLS-LDHs@ZnAl-LDHs film exhibited the highest Ecorr (-0.582 V) and the lowest Icorr (1.657E-4 A / cm 2 ), with the best corrosion resistance. The two different types of LDHs coatings can be used as anion micro-nano containers to intelligently adsorb and store chloride ions for corrosion protection, effectively adapting to environments with different concentrations of corrosive ions. This NiAl-SLS-LDHs@ZnAl-LDHs@Al coating also exhibits self-healing properties, further enhancing corrosion resistance and durability.

[0170] Through research, it was found that the superior corrosion resistance of NiAl-SLS-LDHs@ZnAl-LDHs@Al film is mainly due to three important factors. First, the use of surfactants makes the coating have a hydrophobic surface, which can effectively isolate corrosive ions from the film surface; second, the microstructure of LDHs enables it to self-repair the film through dissolution-recrystallization; third, the use of two different types of LDHs coatings can be used as anion micro-nano containers to intelligently adsorb and store chloride ions for corrosion resistance, effectively adapting to environments with different corrosive ion concentrations, and further improving corrosion resistance and durability.

[0171] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An in-situ construction method for a three-level structure anti-corrosion layer on an aluminum alloy surface, characterized in that: The construction method includes the following steps: Step 1: Using aluminum alloy as substrate, construct the first anti-corrosion coating of ZnAl-LDHs@Al; Step 2: Using the ZnAl-LDHs anti-corrosion layer as a support point, in-situ grow the NiAl-LDHs outer anti-corrosion coating on the surface of ZnAl-LDHs; Step 3: Use the ion exchange properties of ZnAl-LDHs and NiAl-LDHs to store corrosion inhibitors in LDHs nanoreservoirs, and at the same time perform hydrophobic modification and hydrophobic regulation on the surface of NiAl-LDHs to obtain a tertiary structure corrosion protection layer of ZnAl-LDHs base layer @NiAl-LDHs dense layer @interface hydrophobic area.

2. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 1, characterized in that: The construction process of step 1 includes: Step 101: preparing a ZnAl-LDHs thin film growth solution; Step 102: vertically suspending the pretreated aluminum sheet in a ZnAl-LDHs thin film growth solution for a water bath reflux reaction; Step 103: After the reaction is completed, the aluminum sheet is taken out and washed with deionized water, then washed with ethanol, and finally dried at room temperature to obtain Zn 2+ -Al 3+ -LDHs film aluminum sheet; Step 104: washing the precipitate in the ZnAl-LDHs film growth solution after the reaction by centrifugation until the deionized water is clear after washing, then washing it three times with anhydrous ethanol, drying it at room temperature, and finally obtaining ZnAl-LDHs powder for subsequent detection; Step 105: Prepare Zn 2+ -Al 3+ -LDHs thin film aluminum sheet is expressed by concentration and ratio as ZnAl-LDHs-xA / B, where x is Zn 2+ The proportion of total ions in the solution is: A is 22.5mmol / L; B is 50mmol / L.

3. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 2, characterized in that: The specific preparation process of step 101 includes: According to Zn 2+ :Al 3+ The molar ratio is 2-4:

1. Weigh Zn(NO3)2·6H2O and Al(NO3)3·9H2O respectively and add them into the flask. Then add deionized water and a small magnet into the flask. Put the round-bottom flask into an ultrasonicator and ultrasonicate for 15 minutes. Then add H2NCONH2 and ultrasonicate for another 15 minutes to make it fully dissolved in water and set aside.

4. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 3, characterized in that: The specific process of step 2 includes: Step 201: preparing a NiAl-LDHs thin film growth solution; Step 202: Select a suitable aluminum sheet from the ZnAl-LDHs-xA / B obtained in step 104 and place it in a NiAl-LDHs thin film growth solution to perform a water bath reflux reaction; Step 203: Take out the aluminum sheet after the reaction, wash it with deionized water, then wash it with ethanol, and finally dry it at room temperature to obtain Ni 2+ -Al 3+ -LDHs@ZnAl-LDHs thin film aluminum sheet; Step 204: The precipitate obtained after the reaction is centrifuged and washed until the deionized water is clear, then washed three times with anhydrous ethanol, and dried at room temperature to obtain NiAl-LDHs-zC / D@ZnAl-LDHs powder; Step 205: Prepare Ni 2+ -Al 3+ -LDHs@ZnAl-LDHs thin film aluminum film is expressed by concentration and ratio as NiAl-LDHs-zC / D@ZnAl-LDHs@Al, where z is the proportion of Ni2+; C is the total ions of the solution, which is 50mmol / L; and D is the total ions of the solution, which is 90mmol / L.

5. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 4, characterized in that: The preparation process of step 201 includes: According to Ni 2+ :Al 3+ The molar ratio is 2-4:

1. Weigh Ni(NO3)2·6H2O and Al(NO3)3·9H2O respectively and add them into a flask. Then add deionized water and a small magnet. Put the flask into an ultrasonic instrument and sonicate for 15 minutes. Then add urea and sonicate again for 15 minutes to make it fully dissolved in water and set aside.

6. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 5, characterized in that: The reaction temperature of the water bath reflux reaction in step 101 and step 102 is 97° C., and the reaction is carried out at a constant temperature for 8 hours.

7. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 6, characterized in that: The specific process of step 3 includes: Step 301: Select a suitable aluminum sheet from the NiAl-LDHs-zC / D@ZnAl-LDHs@Al prepared in step 204, and place it in a muffle furnace for calcination to prepare for intercalation modification; Step 302: Weigh the surfactant solid powder to prepare a surfactant solution of a certain concentration, suspend the calcined NiAl-LDHs-zC / D@ZnAl-LDHs@Al in a flask with a copper wire, then pour the prepared surfactant solution into the flask to completely immerse the sample, pass nitrogen to expel the air in the system, seal the system, and connect the experimental device to start the reaction; Step 303: After the reaction is completed, turn off the power supply, wait until the temperature of the solution in the beaker drops to room temperature, take out the prepared aluminum sheet and name it NiAl-SLS / SL / SPT / SAS-LDHs@ZnAl-LDHs@Al.

8. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 7, characterized in that: In step 301, the calcination temperature is 400° C. and the calcination time is 4 hours.

9. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 8, characterized in that: The surfactant solution prepared in step 302 is a SLS negative surfactant solution, and the aluminum sheet finally obtained is NiAl-SLS-LDHs@ZnAl-LDHs@Al.

10. The in-situ construction method of a three-level structure anti-corrosion layer on the surface of an aluminum alloy according to claim 9, characterized in that: The corrosion potential of the NiAl-SLS-LDHs@ZnAl-LDHs@Al anti-corrosion layer is 0.582V, and the corrosion current density is 1.657E-4A / cm 2 .