Porous nickel electrode and preparation method and application thereof
Through plasma spraying and multi-step activation treatment, the catalytic activity and coating adhesion of porous nickel electrodes are improved, the problems of high hydrogen evolution overpotential and performance degradation of water electrolysis electrode materials are solved, and more efficient hydrogen production by electrolysis of water is achieved. .
Patent Information
- Application Number
- CN202410957034.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-15
AI Technical Summary
Existing electrode materials for water electrolysis have problems such as high hydrogen evolution overpotential, high power consumption, high price, small specific surface area, and poor electrocatalytic activity, which limits the development of hydrogen production technology through electrolysis of water, and the coating is susceptible to chemical corrosion and mechanical corrosion. wear and tear, resulting in reduced performance.
Aluminum powder, nickel powder, TiB2 powder and TiC powder are mixed and sprayed on the substrate electrode using plasma spraying method, and through multi-step activation treatment, including erosion and pickling, the uniformity, adhesion and catalytic activity of the coating are improved , increase the specific surface area.
A porous nickel electrode with higher catalytic activity, better coating uniformity and adhesion was realized, which reduced the hydrogen evolution overpotential, extended the service life of the electrode and improved the efficiency of hydrogen production by electrolysis of water.
Smart Images

Figure CN118773640A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode preparation, and in particular to a porous nickel electrode and a preparation method and application thereof. Background Art
[0002] Hydrogen production by alkaline water electrolysis is currently the most mature green hydrogen production method. It has a long life, simple structure, good stability and electrocatalytic activity. The biggest problem with this technology is the high energy consumption, which makes the production cost high. The main reason for the high energy consumption is that the hydrogen evolution overpotential of the electrolysis electrode is too high. Therefore, it is particularly important to study how to reduce the hydrogen evolution overpotential to reduce the energy consumption of electrolysis. In addition, the electrode materials currently used for water electrolysis have the disadvantages of being expensive, small specific surface area, and low electrocatalytic activity, which leads to excessively high hydrogen evolution potential and energy consumption of the electrolysis electrode, which seriously restricts the development of water electrolysis hydrogen production technology.
[0003] With the gradual recovery of the global economy and the optimization and upgrading of the industrial structure, porous nickel electrodes, as a material with excellent electrochemical properties, have a wide range of application value in the fields of energy, environment and electrochemistry. In the preparation process, how to further improve the uniformity, adhesion and activation specific surface area of the coating are all issues that need to be solved urgently.
[0004] Judging from the relevant domestic and foreign patents, a variety of processes have been developed and adopted at home and abroad for the preparation of water electrolysis electrodes, such as electroplating, chemical plating, cold pressing, magnetron sputtering and thermal spraying. Compared with other preparation processes, plasma spraying is an efficient surface modification process. During the spraying process, the substrate is not charged and does not melt. The substrate and the spray gun move at a high speed relative to each other, so that the substrate structure does not change, the coating has few impurities, and the coating is flat and smooth, with high density and high bonding strength. It is very suitable for electrode surface treatment and rapid preparation of catalytic coatings.
[0005] In the prior art, the preparation of water electrolysis electrodes mainly adopts electroplating, chemical plating, cold pressing, magnetron spraying and thermal spraying. For example, patent application CN117661018A adopts plasma spraying to spray aluminum yttrium-coated nickel-molybdenum powder onto the pretreated nickel mesh, and then prepares a porous nickel electrode through activation and pore formation; patent application CN117512640A adds nickel powder, aluminum powder and molybdenum powder to nickel sulfate, and then prepares a porous nickel electrode through deposition, rolling, heat treatment, electroplating and sintering processes. The electrode wire mesh prepared by plasma spraying has the advantages of stable process, high quality, environmental protection, and fast spraying speed, and is a very potential means of optimizing the performance of hydrogen evolution electrodes.
[0006] Electrodes currently on the market are very susceptible to chemical corrosion, mechanical wear or structural changes during use, causing the coating to fall off, leading to a gradual decline in performance. How to further improve the bonding strength of the electrode coating, the specific surface area of the activation layer, and improve the erosion pore-forming process are the key and difficult issues in the current work of water electrolysis electrodes. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a porous nickel electrode and a preparation method and application thereof, so as to realize a porous nickel electrode with higher catalytic activity, higher uniformity of coating and higher adhesion.
[0008] In a first aspect, the present invention first provides a method for preparing a porous nickel electrode, comprising: S1: mixing raw material powder and additives to obtain spray powder; the raw material powder includes aluminum powder, nickel powder, titanium diboride powder and titanium carbide powder; S2: depositing the spray powder onto a substrate electrode to obtain a catalytic electrode; S3: activating the catalytic electrode to obtain the porous nickel electrode.
[0009] According to a method for preparing a porous nickel electrode provided by the present invention, the particle size of the nickel powder is 10 to 50 microns; and / or the particle size of the aluminum powder is 70 to 150 microns; and / or the particle sizes of the TiB2 powder and the TiC powder are independently, identically or differently, 10 to 100 microns.
[0010] According to a method for preparing a porous nickel electrode provided by the present invention, the raw material powder includes the following components: 15-25wt% aluminum powder, 0.5-3wt% titanium diboride powder, 0.5-3wt% titanium carbide powder and the remainder nickel powder.
[0011] According to a method for preparing a porous nickel electrode provided by the present invention, the additive includes one or more of alkyd varnish, polyenol, polyimide and dimethyl sulfoxide; preferably, the amount of the additive is 1-5wt% of the mass of the spray powder.
[0012] According to a method for preparing a porous nickel electrode provided by the present invention, the deposition includes spraying the spray powder on the surface of the substrate electrode by plasma spraying; preferably, the sprayed coating thickness is 10 to 5000 microns.
[0013] According to a method for preparing a porous nickel electrode provided by the present invention, the spraying conditions of the plasma spraying method include: a spraying current of 500~800A, a spraying voltage of 20~60V, a powder feeding amount of 150~300g / min, an argon flow rate of 40~80L / min, a hydrogen flow rate of 1~2L / min, a spraying distance of 100~200mm, and a spray gun moving speed of 500~1000mm / sec.
[0014] According to a method for preparing a porous nickel electrode provided by the present invention, the activation treatment in S3 comprises: S31: corroding the catalytic electrode in a first alkaline solution at 20-30 degrees Celsius, and then washing with water; S32: continuing to erode in a mixed solution at 20-30 degrees Celsius, and then washing with water; the mixed solution includes a sulfuric acid aqueous solution, an ammonium citrate aqueous solution and a hydrogen peroxide aqueous solution; S33: Soaking in a second alkaline solution at 40-60 degrees Celsius, and then washing with water.
[0015] Preferably, the concentration of the first alkaline solution is 3-10wt%; the concentration of the aqueous sulfuric acid solution is 20-30wt%, the concentration of the aqueous ammonium citrate solution is 15-25wt%, the concentration of the aqueous hydrogen peroxide solution is 2-5wt%; the concentration of the first alkaline solution is 25-30wt%.
[0016] Preferably, the aqueous ammonium citrate solution accounts for 10-20 wt % of the solution after mixing with the aqueous sulfuric acid solution, and the aqueous hydrogen peroxide solution accounts for 8-15 wt % of the mixed solution of ammonium citrate and sulfuric acid.
[0017] According to a method for preparing a porous nickel electrode provided by the present invention, the method further comprises pre-treating the substrate electrode before deposition, and the pre-treatment comprises: sandblasting and washing the substrate electrode.
[0018] In a second aspect, the present invention provides a porous nickel electrode, which is prepared by the method for preparing the porous nickel electrode.
[0019] In a third aspect, the present invention provides application of the porous nickel electrode in hydrogen evolution reaction.
[0020] The porous nickel electrode and its preparation method and application provided by the present invention can change the size of aluminum grains in the coating by adding TiB2 powder and TiC powder, thereby changing the specific surface area of the coating after activation, thereby increasing the catalytic activity. At the same time, by adjusting the grain size, the uniformity and adhesion of the coating can also be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is a flow chart for preparing the porous nickel electrode in Example 1 provided by the present invention. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solutions and advantages of the present invention clearer, the following will be combined with Figure 1 The technical solutions in the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] At present, there are many formulas for nickel-based alloy hydrogen evolution electrodes in the prior art, especially alloy elements such as Ni-Mo, Ni-Co, Ni-Mn, Ni-Al, precious metals and rare earths, but there is still room for further improvement in catalytic activity and coating adhesion.
[0025] Based on the above problems, the present invention finds that adding TiB2 and TiC to Ni powder and Al powder can change the specific surface area of the coating after activation by changing the coating grain size, thereby increasing the catalytic activity of the electrode. At the same time, by adjusting the grain size, the uniformity and adhesion of the coating can be further improved.
[0026] To this end, the present invention has the following technical solutions: In a first aspect, the present invention first provides a method for preparing a porous nickel electrode, comprising: S1: mixing raw material powder and additives to obtain spray powder; the raw material powder includes aluminum powder, nickel powder, titanium diboride powder and titanium carbide powder; S2: depositing the spray powder onto a substrate electrode to obtain a catalytic electrode; S3: activating the catalytic electrode to obtain the porous nickel electrode.
[0027] In the present invention, the raw material powder and the additive can be mixed by stirring or ball milling, including wet or dry methods, to perform agglomeration granulation at a speed of 200 to 400 rpm for 60 to 160 minutes to obtain agglomerated particles (i.e., the spray powder).
[0028] Furthermore, if wet stirring or ball milling is used, the solvent can be removed by vacuum drying as needed.
[0029] According to a preferred embodiment provided by the present invention, the particle size of the nickel powder is 10~50 microns; and / or, the particle size of the aluminum powder is 70~150 microns; and / or, the particle sizes of the TiB2 powder and the TiC powder are independently, identically or differently, 10~100 microns.
[0030] According to a preferred embodiment provided by the present invention, the raw material powder includes the following components: 15-25wt% aluminum powder, 0.5-3wt% titanium diboride powder, 0.5-3wt% titanium carbide powder and the balance nickel powder.
[0031] In the present invention, by controlling the particle size of the raw material powders, especially the particle size of the TiB2 powder and the TiC powder, the uniformity, density and adhesion between the coating and the substrate can be increased, the bonding strength of the coating can be improved, and the durability and service life of the coating can be extended.
[0032] According to a preferred embodiment provided by the present invention, the additive includes one or more of alkyd varnish, polyenol, polyimide and dimethyl sulfoxide.
[0033] According to a preferred embodiment provided by the present invention, the amount of the additive is 1-5wt% of the mass of the spray powder.
[0034] According to a preferred embodiment provided by the present invention, the deposition includes spraying the spray powder onto the surface of the substrate electrode by a plasma spraying method.
[0035] According to a preferred embodiment provided by the present invention, the thickness of the sprayed coating is 10 to 5000 microns.
[0036] According to a preferred embodiment provided by the present invention, the spraying conditions of the plasma spraying method include: spraying current 500~800A, spraying voltage 20~60V, powder feeding amount 150~300g / min, argon flow rate 40~80L / min, hydrogen flow rate 1~2L / min, spraying distance 100~200mm, and spray gun moving speed 500~1000mm / sec.
[0037] According to a preferred embodiment provided by the present invention, the activation process in S3 includes: S31: corroding the catalytic electrode in a first alkaline solution at 20-30 degrees Celsius, and then washing with water; S32: continuing to erode in a mixed solution at 20-30 degrees Celsius, and then washing with water; the mixed solution includes a sulfuric acid aqueous solution, an ammonium citrate aqueous solution and a hydrogen peroxide aqueous solution; S33: Soaking in a second alkaline solution at 40-60 degrees Celsius, and then washing with water.
[0038] The present invention adds a step of acid washing activation method, which can minimize the aluminum content in the coating while maintaining sufficient activity of the electrode, so that the electrode can avoid the negative impact of coating shedding caused by the reaction between aluminum and alkali during subsequent electrolysis work, which leads to a decrease in electrode activity.
[0039] According to a preferred embodiment provided by the present invention, the concentration of the first alkaline solution is 3-10wt%; the concentration of the aqueous sulfuric acid solution is 20-30wt%, the concentration of the aqueous ammonium citrate solution is 15-25wt%, the concentration of the aqueous hydrogen peroxide solution is 2-5wt%; the concentration of the first alkaline solution is 25-30wt%.
[0040] According to a preferred embodiment provided by the present invention, the aqueous solution of ammonium citrate accounts for 10-20wt% of the solution after mixing with the aqueous solution of sulfuric acid, and the aqueous solution of hydrogen peroxide accounts for 8-15wt% of the mixed solution of ammonium citrate and sulfuric acid.
[0041] According to a preferred embodiment provided by the present invention, the erosion time in S31 is 20 to 40 minutes; the erosion time in S31 is 10 to 30 minutes; the erosion time in S31 is 1.5 to 2.5 hours.
[0042] According to a preferred embodiment provided by the present invention, the preparation method further comprises pre-treating the substrate electrode before deposition, and the pre-treatment comprises: sandblasting and washing the substrate electrode.
[0043] According to a preferred embodiment provided by the present invention, the aqueous hydrogen peroxide solution is added in multiple times; further preferably, the aqueous hydrogen peroxide solution is added in two times.
[0044] According to a preferred embodiment provided by the present invention, the substrate electrode can be a woven mesh, stretched mesh, punched mesh or foam mesh made of nickel, iron or copper; when the substrate is a nickel mesh, the number of nickel meshes is generally 30 to 150 meshes, and the pretreatment method includes sandblasting and washing.
[0045] Further preferably, the sandblasting uses 70-90 mesh white corundum sand, a spraying pressure of 0.2-0.4 MPa, and a nozzle tilted at an angle of 60-80 degrees.
[0046] Further preferably, the washing is sequentially performed by alkaline washing to remove oil, deionized water washing to remove alkali, and then ultrasonic cleaning with ethanol before waiting for spraying.
[0047] In a second aspect, the present invention provides a porous nickel electrode, which is prepared by the method for preparing the porous nickel electrode.
[0048] In a third aspect, the present invention provides application of the porous nickel electrode in hydrogen evolution reaction.
[0049] Unless otherwise specified, all raw materials used in the examples are commercially available conventional raw materials, and the technical means used are conventional means well known to those skilled in the art.
[0050] Example 1
[0051] This embodiment provides a porous nickel electrode (see the preparation flow chart for details) Figure 1 ), the preparation method of which comprises the following steps: A. Powder mixing: nickel powder, aluminum powder, TiB2 powder, and TiC powder are mixed in a mass ratio of 7:2.7:0.1:0.2 to obtain a mixed powder; 2 wt% polyenol and 1 wt% alkyd varnish (based on the mass of the mixed powder) are added, the rotation speed is 350 rpm, the time is 160 minutes, and the obtained agglomerated particles are dried in a drying oven at 100°C for 8 hours to obtain sprayable particles.
[0052] B. Pretreatment of the base electrode: Sandblast and wash the nickel mesh. Use 80-mesh white corundum sand, spray pressure 0.3 MPa, and the nozzle is tilted at 70 degrees. Wash by alkali washing to remove oil, deionized water washing to remove alkali, and then use ethanol ultrasonic cleaning to clean and wait for spraying.
[0053] C. Plasma spraying: The process parameters for spraying the transition layer are: current 600A, voltage 45V, powder feeding rate 150g / min, argon flow 40L / min, hydrogen flow 2L / min, spray gun moving speed 550mm / s, spray distance 100mm, spray thickness between 70 and 120μm. Finally, a coated nickel electrode is obtained; D. Electrode activation: The sprayed electrode is first corroded in a 5wt% sodium hydroxide solution at room temperature for 30 minutes, washed with deionized water, and then corroded in a mixed solution of a certain proportion of dilute sulfuric acid, ammonium citrate aqueous solution and hydrogen peroxide aqueous solution at room temperature for 10 to 30 minutes. After washing with deionized water, it is immersed in a 50°C, 30wt% sodium hydroxide solution for 2 hours, and then rinsed with deionized water to complete the etching and pore-forming work to obtain a porous nickel electrode.
[0054] The selected concentration of dilute sulfuric acid is 30wt%, the selected concentration of ammonium citrate aqueous solution is 20wt%, and the concentration of hydrogen peroxide aqueous solution is 3wt%; the mass ratio of dilute sulfuric acid: ammonium citrate is 8:2, the activation time is 10 minutes, and hydrogen peroxide is added to 5% of the total solution at the initial stage, and another 5% is added after 5 minutes.
[0055] Example 2
[0056] This embodiment provides a porous nickel electrode, and the preparation method thereof is different from that of Embodiment 1 only in that: in A, the mass ratio of nickel powder, aluminum powder, TiB2 powder, and TiC powder is 7:2.7:0.2:0.1.
[0057] Example 3
[0058] This embodiment provides a porous nickel electrode, and the preparation method thereof is different from that of Embodiment 1 only in that: in D, the selected concentration of dilute sulfuric acid is 20 wt %, and the selected concentration of ammonium citrate solution is 15 wt %.
[0059] Example 4
[0060] This embodiment provides a porous nickel electrode, and the preparation method thereof is different from that of Embodiment 1 only in that: D uses a 30 wt % sodium hydroxide solution for activation dealumination and then dries.
[0061] Comparative Example 1
[0062] This embodiment provides a porous nickel electrode, and the preparation method thereof is different from that of Embodiment 1 only in that the TiC powder is replaced with an equal amount of TiB2 powder.
[0063] Comparative Example 2
[0064] This embodiment provides a porous nickel electrode, and the preparation method thereof is different from that of Embodiment 1 only in that TiC powder and TiB2 powder are replaced with an equal amount of boron powder.
[0065] Experimental example
[0066] The present invention further tests the effects of the porous nickel electrodes prepared in the examples and comparative examples (including the bonding strength between the substrate electrode and the coating, electrode performance, etc.), and the test results are shown in Table 1: Table 1
[0067] Among them, the electrode weight loss test method includes the following steps: 1. Weigh the weight of the electrode to be tested before the test; 2. Soak the electrode to be tested in a beaker filled with water, place the beaker in an ultrasonic machine, continue ultrasonication for 3 hours, and weigh the weight of the electrode after cleaning and drying; 3. Calculate the difference in electrode weight before and after the test, and further calculate to obtain the electrode weight loss percentage.
[0068] Potential test method: A three-electrode electrochemical test system is used, the reference electrode is a saturated calomel electrode, at 3kA / m 2 The potential of the working electrode was tested under electrical density, and the working electrode was used as cathode and anode to test the hydrogen evolution overpotential and oxygen evolution overpotential of the electrode.
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a porous nickel electrode, It is characterized in that include: S1: mixing raw material powder and additives to obtain spray powder; the raw material powder includes aluminum powder, nickel powder, titanium diboride powder and titanium carbide powder; S2: depositing the spray powder onto a substrate electrode to obtain a catalytic electrode; S3: activating the catalytic electrode to obtain the porous nickel electrode.
2. The method for preparing the porous nickel electrode according to claim 1, It is characterized in that The particle size of the nickel powder is 10 to 50 microns; and / or the particle size of the aluminum powder is 70 to 150 microns; and / or the TiB 2 The particle sizes of the powder and the TiC powder are independently, identically or differently, 10 to 100 microns.
3. The method for preparing the porous nickel electrode according to claim 1, It is characterized in that The raw material powder comprises the following components: 15-25wt% aluminum powder, 0.5-3wt% titanium diboride powder, 0.5-3wt% titanium carbide powder and the balance nickel powder.
4. The method for preparing the porous nickel electrode according to any one of claims 1 to 3, It is characterized in that The additive includes one or more of alkyd varnish, polyenol, polyimide and dimethyl sulfoxide; preferably, the amount of the additive is 1-5wt% of the mass of the spray powder.
5. The method for preparing the porous nickel electrode according to any one of claims 1 to 3, It is characterized in that The deposition includes spraying the spray powder onto the surface of the substrate electrode by plasma spraying; preferably, the spray coating thickness is 10 to 5000 microns.
6. The method for preparing the porous nickel electrode according to claim 4, It is characterized in that The spraying conditions of the plasma spraying method include: spraying current 500~800A, spraying voltage 20~60V, powder feeding amount 150~300g / min, argon flow rate 40~80L / min, hydrogen flow rate 1~2L / min, spraying distance 100~200mm, and spray gun moving speed 500~1000mm / sec.
7. The method for preparing the porous nickel electrode according to any one of claims 1 to 3, It is characterized in that The activation process in S3 includes: S31: corroding the catalytic electrode in a first alkaline solution at 20-30 degrees Celsius, and then washing with water; S32: continuing to erode in a mixed solution at 20-30 degrees Celsius, and then washing with water; the mixed solution includes a sulfuric acid aqueous solution, an ammonium citrate aqueous solution and a hydrogen peroxide aqueous solution; S33: soaking in a second alkaline solution at 40-60 degrees Celsius, and then washing with water; Preferably, the concentration of the first alkaline solution is 3-10wt%; the concentration of the aqueous sulfuric acid solution is 20-30wt%, the concentration of the aqueous ammonium citrate solution is 15-25wt%, the concentration of the aqueous hydrogen peroxide solution is 2-5wt%; the concentration of the first alkaline solution is 25-30wt%; Preferably, the aqueous ammonium citrate solution accounts for 10-20 wt % of the solution after mixing with the aqueous sulfuric acid solution, and the aqueous hydrogen peroxide solution accounts for 8-15 wt % of the mixed solution of ammonium citrate and sulfuric acid.
8. The method for preparing the porous nickel electrode according to any one of claims 1 to 3, It is characterized in that The preparation method further comprises pre-treating the substrate electrode before deposition, wherein the pre-treatment comprises: sandblasting and washing the substrate electrode.
9. A porous nickel electrode, It is characterized in that The porous nickel electrode is prepared by the method for preparing the porous nickel electrode according to any one of claims 1 to 8.
10. Use of the porous nickel electrode according to claim 9 in hydrogen evolution reaction.