Beta-chitin fiber material, preparation method thereof and ligament / tendon repair material based on beta-chitin fiber material

By extracting and processing β-chitin fibers from squid parietal bones to retain their natural multi-level orientation structure, the problem of insufficient β-chitin fiber material performance in the existing technology is solved, and mechanical properties similar to natural ligaments/tendons are achieved. Biocompatibility, used for ligament/tendon repair, significantly improves the repair effect and industrialization potential.

CN118773775APending Publication Date: 2024-10-15JINAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410777097.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to reconstruct the multi-level orientation structure and performance of natural β-chitin with existing technology, and artificial scaffolds have limited mechanical properties, poor cytocompatibility, poor biological activity, and high immunogenicity in ligament/tendon repair, making it difficult to achieve effective tissue repair. regeneration.

Method used

By extracting mineralized β-chitin fibers from squid parietal bones and treating them with alkali and ethanol solutions to retain the natural multi-level orientation and mineralized structure, β-chitin fiber materials with excellent mechanical properties and biocompatibility were prepared. , and combined with active substances to prepare ligament/tendon repair materials.

Benefits of technology

It has achieved a fiber structure skeleton similar to natural ligaments/tendons, with good mechanical properties, hydrophilicity and biocompatibility, overcoming the shortcomings of artificial scaffolds, and significantly improving the effect of ligament/tendon repair and industrialization prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773775A_ABST
    Figure CN118773775A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of biological materials, and discloses a beta-chitin fiber material, a preparation method thereof and a ligament / tendon repair material based on the beta-chitin fiber material. The beta-chitin fiber material retains the natural orientation structure and trace calcium component of chitin in the squid parietal bone, is white and semitransparent, and has the acetylation degree of 85-97%. The squid top bone is directly used as a raw material, the beta-chitin fiber material is obtained through reaction treatment of alkali liquor and an ethanol solution containing polysorbate 80, the structural framework of beta-chitin in the squid bone is reserved, and the beta-chitin fiber material has an anisotropic fiber orientation structure and a fine multi-scale layered structure; the structure is similar to the orientation structure of the ligament / tendon, has low immunogenicity, excellent mechanical property, hydrophilicity and good mechanical property and pore structure, and can be applied to repair and regeneration of the ligament / tendon as a high-added-value product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomaterials, and particularly relates to a beta-chitin fiber material and a preparation method thereof, and a ligament / tendon repair material based thereon. Background Art

[0002] In recent years, with the rapid development of tissue engineering scaffold materials, artificial scaffolds for ligament / tendon injury repair have shown extremely broad application prospects. Artificial scaffolds can overcome the problems of limited donors and immune rejection, and can maintain their strength during a certain period of implantation, provide mechanical support for human movement, and promote tissue ingrowth and regeneration, thereby restoring the structure and function of ligaments / tendons. At present, commonly used materials such as decellularized extracellular matrix have structures and active substances similar to those of tissues, but there is a risk of immunogenicity; synthetic polymer materials have excellent mechanical properties, but are prone to stress shielding effects and are difficult to integrate with surrounding tissues; natural polymers have good biological activity, but poor mechanical properties and are difficult to provide mechanical support for tissues.

[0003] As a natural polysaccharide material, chitin has a unique chemical structure and composition that endows it with good biological activities, such as antibacterial, immunomodulatory and osteogenic activity. These biological activities make chitin widely used in the biomedical field, such as tissue engineering scaffolds, wound dressings, drug delivery carriers, biosensors, etc. β-Chitin is a long-chain polymer of (1,4)-β-N-acetylglucosamine, whose molecular chains are arranged in parallel, the intermolecular hydrogen bonds are relatively weak, and the chain segments are arranged loosely. β-Chitin is commonly found in squid cartilage, and the mineral content of squid parietal bones is low, and the degree of contamination is low, which makes it suitable for extracting high-purity β-chitin fibers, which can be used in high-value-added medical device products.

[0004] At present, the preparation of chitosan fiber usually involves purifying raw materials such as shrimp shells, crab shells, and squid bones to obtain chitosan, then dissolving chitosan in a limited solvent to obtain chitosan solution, and then assembling and regenerating chitosan fibers with target morphology and structure, or preparing chitosan films by hot pressing, etc. This preparation method can design and control the structure of fibers and films, but it is difficult to reconstruct the multi-level orientation structure and properties of natural β-chitosan.

[0005] Therefore, there is an urgent need to provide a new β-chitin fiber material that not only retains the natural multi-level orientation and mineralized structure of β-chitin in squid bones, but also has good mechanical properties and excellent biocompatibility, and can be used to prepare ligament / tendon repair materials to achieve structural advantages and practical application value. Summary of the invention

[0006] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a β-chitosan fiber material.

[0007] The β-chitin fiber material of the present invention has a fiber structural skeleton similar to that of natural ligaments / tendons (anisotropic fiber orientation structure and fine multi-scale layered structure), and also has the advantages of mechanical properties matching tissues, good pore structure, excellent hydrophilicity and biocompatibility.

[0008] Another object of the present invention is to provide a method for preparing the above-mentioned β-chitin fiber material.

[0009] The invention provides a method for extracting mineralized beta-chitin fibers from squid parietal bones, which retains the natural multi-level orientation and mineralized structure of beta-chitin in the squid bones and can be used for preparing ligament / tendon repair materials.

[0010] Another object of the present invention is to provide application of the above-mentioned β-chitin fiber material in the preparation of ligament / tendon repair materials.

[0011] The β-chitin fiber material of the present invention overcomes the shortcomings of artificial scaffolds, such as limited mechanical properties, poor cell compatibility, poor biological activity, and immunogenicity. It can be directly used or modified in structure and functionality, and can be used in ligament / tendon repair and regeneration after being combined with other active substances. It has obvious advantages and good industrial prospects.

[0012] Another object of the present invention is to provide a ligament / tendon repair material based on the above-mentioned β-chitin fiber material.

[0013] The purpose of the present invention is achieved through the following solutions:

[0014] The first aspect is a method for preparing a β-chitin fiber material, which is obtained by treating squid cartilage with an alkali solution and an ethanol solution in sequence.

[0015] Furthermore, the alkali solution may be sodium hydroxide or potassium hydroxide solution.

[0016] Furthermore, the concentration of the alkali solution may be 4-20wt%.

[0017] Furthermore, the alkali solution treatment refers to soaking the squid top bones in alkali solution; the soaking can be carried out at 60-95°C.

[0018] Furthermore, the mass ratio of the squid cartilage to the alkali solution may be 1:5 to 1:40.

[0019] Furthermore, the alkali solution treatment time may be 6-24 hours.

[0020] Furthermore, the alkali solution can be replaced during the alkali solution treatment, such as replacing the alkali solution every 2 hours; the reaction solution changes from orange-yellow to colorless and transparent, and the reactants appear in a white and translucent state.

[0021] Furthermore, after the alkaline solution treatment, the product is washed to neutrality and then treated with an ethanol solution.

[0022] Furthermore, the concentration of the ethanol solution is greater than or equal to 85%.

[0023] Furthermore, the ethanol solution may also contain polysorbate 80 at a concentration of 0-10 wt %.

[0024] Furthermore, the reaction temperature of the ethanol solution treatment is 50-65°C.

[0025] Furthermore, the ethanol solution treatment time is 1-10 hours.

[0026] Furthermore, when the ethanol solution is used for treatment, the mass ratio of the reactant to the ethanol solution may be 1:10 to 1:30.

[0027] Furthermore, after being treated with the ethanol solution, the cellulose fiber can be washed with water to obtain a high-purity β-chitin fiber material.

[0028] Furthermore, the raw material is squid cartilage, preferably squid parietal bone; the squid cartilage can be cleaned, the flanks can be trimmed and removed, and the squid parietal bone can be retained for later use.

[0029] The present invention provides for the first time a method of directly using squid parietal bones as raw materials, and obtaining high-purity β-chitin fibers through reaction treatment with alkali solution and ethanol solution, and retaining the structural skeleton of β-chitin in squid bones, which can be directly used to prepare ligament / tendon repair materials. The preparation method of the present invention has a simple reaction process, is easy to operate, and is suitable for industrialization.

[0030] In the second aspect, a β-chitosan fiber material is prepared by the above method. The β-chitosan fiber material of the present invention retains the natural orientation structure and trace calcium components of chitosan in the squid parietal bone, is white and translucent, and has an acetylation degree of 85-97%.

[0031] The β-chitin fiber material of the present invention retains the structural skeleton of β-chitin in squid bones, has an anisotropic fiber orientation structure and a fine multi-scale layered structure, which is similar to the orientation structure of ligaments / tendons, and has low immunogenicity, excellent mechanical properties, hydrophilicity, good mechanical properties and pore structure, and can be used as a high value-added product in the repair and regeneration of ligaments / tendons.

[0032] The third aspect is the application of the above-mentioned β-chitin fiber material in the preparation of ligament / tendon repair materials.

[0033] The β-chitin fiber material of the present invention overcomes the shortcomings of artificial scaffolds, such as limited mechanical properties, poor cell compatibility, poor biological activity, and immunogenicity. It can be directly used or subjected to structural and functional modifications, and can be prepared into ligament / tendon repair materials after being compounded with other active substances. It is applied to the repair and regeneration of ligaments / tendons, and has obvious advantages and good industrialization prospects.

[0034] Furthermore, the ligament / tendon repair material is specifically a tissue engineering ligament / tendon repair material, and the application sites include but are not limited to the knee joint, shoulder joint, ankle joint, lumbar vertebrae and cervical vertebrae.

[0035] Furthermore, the structural and functional modifications include, but are not limited to, modification strategies such as layer-by-layer self-assembly of active factors, in-situ deposition of minerals, and chemical grafting. These modification methods can enrich the functions and applications of β-chitin fibers.

[0036] In a fourth aspect, a ligament / tendon repair material comprises the above-mentioned β-chitin fiber material.

[0037] Furthermore, the ligament / tendon repair material also contains active substances.

[0038] Furthermore, the active substances may include but are not limited to hydroxyapatite, calcium carbonate, cell growth factors, polypeptides, platelet lysate, hyaluronan, chondroitin sulfate and collagen, etc. Active substances can not only provide good biological functions to promote the regeneration of cells and tissues, but also can be used to regulate cell proliferation and differentiation.

[0039] In a fifth aspect, a ligament / tendon repair material comprises the above-mentioned β-chitin fiber material and hydroxyapatite crystals mineralized on the fiber matrix.

[0040] The hydroxyapatite crystals are formed by mineralization in the above-mentioned β-chitin fiber material through a conventional biomimetic mineralization strategy.

[0041] Specifically, the preparation method of the above ligament / tendon repair material is to immerse the β-chitin fiber material in a mineralizing liquid for mineralization.

[0042] Furthermore, the mineralization liquid can be a conventional mineralization liquid, such as a mineralization liquid containing a mineralization inducer, a calcium salt solution and a phosphate solution.

[0043] Further, the mineralization inducer includes but is not limited to at least one of polyacrylic acid, polyaspartic acid, etc. The calcium salt may include but is not limited to at least one of water-soluble calcium salts such as calcium chloride, calcium nitrate, and calcium acetate. The phosphate includes but is not limited to at least one of disodium hydrogen phosphate, sodium phosphate, and sodium monohydrogen phosphate.

[0044] In a sixth aspect, a ligament / tendon repair material comprises the above-mentioned β-chitin fiber, polydopamine and chondroitin sulfate.

[0045] The present invention provides a β-chitin fiber material, which uses natural squid parietal bones as raw materials, and is treated with alkaline solution and ethanol solution to obtain β-chitin fibers that retain natural fiber structure skeletons and trace calcium. The β-chitin fibers present an anisotropic orientation structure and a multi-scale layered structure, and have mechanical behaviors (mechanical strength, fatigue resistance, and viscoelasticity) similar to natural ligaments, and have the advantages of high hydrophilicity, good pore structure, biodegradability, low immune rejection, and excellent cell compatibility. Ligament / tendon repair materials are prepared directly or after compounding and modification, and are applied to ligament / tendon repair, which can overcome the shortcomings of mismatch between the mechanical properties of the graft and the tissue, low biological activity, and inability to degrade and absorb, and have obvious advantages and good industrialization prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0047] Figure 1 The figures are the results of scanning electron microscope (SEM) observation of the transverse (A) and longitudinal (B) cross sections of the β-chitin fiber of the present invention, and the results of polarizing microscope observation of the surface (C).

[0048] Figure 2 These are the transmission electron microscopy observation results of β-chitin nanofibers prepared by the existing conventional method.

[0049] Figure 3 The figures show the proliferation status (A) and live / dead staining results (B) of the co-culture of β-chitin fiber and bone marrow mesenchymal stem cells of the present invention.

[0050] Figure 4 This is a SEM observation image of the β-chitosan fiber mineralized scaffold material of the present invention.

[0051] Figure 5 The results of co-culture of β-chitin fiber mineralized scaffold material and bone marrow mesenchymal stem cells show the promotion of alkaline phosphatase secretion and quantification results (A), and the formation of calcium nodules and quantification results (B).

[0052] Figure 6The results of histological staining sections of the repair of completely injured anterior cruciate ligament in rats with β-chitin fiber mineralized scaffold materials. "L" in the figure represents the reconstructed ligament; "B" represents the bone end; and "M" represents the bone marrow.

[0053] Figure 7 The immunohistochemical staining results of the section of the rat anterior cruciate ligament repaired with β-chitin fiber mineralized scaffold material. "L" in the figure indicates the reconstructed ligament; "B" indicates the bone end; "M" indicates the bone marrow; and the arrow indicates the antibody staining site.

[0054] Figure 8 Micro-CT scanning analysis and observation results of β-chitin fiber mineralized scaffold material in repairing completely injured anterior cruciate ligament in rats.

[0055] Fig. 9 These are the test results of the fracture load (A) and stiffness (B) of the reconstructed ligament after the β-chitosan fiber mineralized scaffold material of the present invention was implanted in vivo. DETAILED DESCRIPTION

[0056] The present invention is further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto. The materials involved in the following examples can be obtained from commercial channels unless otherwise specified. The methods described are conventional methods unless otherwise specified. The amounts of each component are measured in parts by mass and parts by volume, g, mL.

[0057] Example 1

[0058] A β-chitin fiber material for preparing ligament / tendon repair materials, which is directly extracted from the squid parietal bone. Specifically comprising the following steps:

[0059] (1) 200 parts by mass of squid parietal bones were added to 1000 parts by volume of a 4 wt % sodium hydroxide solution, and reacted at 90° C. for 6 h (the sodium hydroxide solution was replaced every 2 h), and the obtained product was washed until neutral.

[0060] (2) Take 10 parts by mass of the product after the alkali solution treatment, add 300 parts by volume of anhydrous ethanol solution, soak at 65° C. for 2 hours, and wash; repeat the soaking treatment 3 times to obtain high-purity β-chitin fibers with a layered structure and a multi-level oriented structure.

[0061] Figure 1 The SEM observation results of the transverse (A) and longitudinal (B) sections of β-chitin fibers show the macroscopic layered structure of the fibers. Figure 1(C) is the polarizing microscope observation result of the β-chitin fiber surface, which shows that the fiber has an oriented structure (multi-level oriented structure) both microscopically and macroscopically. This structure is similar to natural ligaments / tendons and gives the fiber good mechanical properties. Compared with other existing β-chitin fiber repair materials, the structure and performance of the β-chitin fiber of the present invention are advantageous.

[0062] This is because the existing preparation methods of β-chitosan fibers cannot preserve the macroscopic layered structure and multi-level oriented structure of β-chitosan in squid bones. The existing preparation methods generally grind the squid parietal bones, use acid, ethanol, alkali solution and other multi-step treatments, and then grind and crush to obtain β-chitosan nanofibers. During the treatment process, the multi-level oriented structure of β-chitosan is destroyed. Therefore, chitosan fibers with target morphology and structure can only be formed by assembly and regeneration, or chitosan films can be prepared by hot pressing, solvent evaporation and other methods. Figure 2 This is a transmission electron microscope image of β-chitin nanofibers prepared by conventional methods. The chitin polymer chain still has alternating nanocrystalline and amorphous regions, but the multi-level oriented structure of β-chitin in squid bones has been destroyed and is difficult to rebuild through reassembly methods such as hot pressing film forming and spinning.

[0063] Example 2: Effect of β-chitin fiber on the proliferation of bone marrow mesenchymal stem cells

[0064] The β-chitin fibers prepared in Example 1 are co-cultured with bone marrow mesenchymal stem cells, specifically comprising the following steps:

[0065] (1) Cell culture: Mouse bone marrow mesenchymal stem cells were used as seed cells to evaluate the cell compatibility of the material in vitro. The cells were cultured in a high-glucose culture medium containing 10% fetal bovine serum and 1% double antibody; the culture conditions were 37°C, 95% relative humidity, and 5% CO 2 concentration; the culture medium was changed every two days.

[0066] (2) Extract preparation: To simulate the conditions of co-culture of β-chitin fiber and cells, the material extract was prepared according to the following steps. First, 30 mg of β-chitin fiber was placed in a clean bench for UV sterilization for 24 h, and then 3 mL of high-sugar culture medium was added and placed in an incubator overnight to obtain an extract (10 mg / mL).

[0067] (3) Cell plate: Digest and count the cells, then plate at 2×10 4The cells / well were inoculated at a density of 1.54 × 10 cells / well in a 24-well plate (three replicate wells per group) and placed in a cell culture incubator overnight. After the cells adhered to the wall, the high-sugar culture medium was replaced with the material extract (1 mL per well), which was used as the β-chitin fiber group and recorded as day 0. Repeat step (3), but replace the material extract with high-sugar culture medium, which was used as the culture plate group and recorded as day 0. In addition, in the β-chitin group, after replacing the high-sugar culture medium in the well plate with the material extract, 3 mL of fresh high-sugar culture medium was added to continue the extraction with the material to prepare the extract required for the next liquid change.

[0068] (4) Cell viability test: On days 1, 3, and 5, the cell viability of the two groups was detected using a CCK-8 kit. Then, the live and dead cells were stained with calcein-AM / PI staining solution. The fluorescent images of live / dead cells were observed and photographed using an inverted fluorescence microscope. The results are shown in Table 1. Figure 3 shown.

[0069] As can be seen from the figure, the fiber of the present invention has good cell compatibility and can promote cell adhesion, spreading and proliferation. Cell proliferation and live / dead staining.

[0070] Example 3

[0071] A ligament / tendon repair material, specifically a β-chitin fiber mineralized scaffold material for promoting ligament / tendon and bone integration, the components of which include the above-mentioned β-chitin fiber material and hydroxyapatite crystals mineralized on the fiber matrix. The preparation method can be firstly to extract β-chitin fiber from the squid parietal bone, and then to mineralize hydroxyapatite crystals with osteogenic activity on the fiber using a bionic mineralization strategy, specifically comprising the following steps:

[0072] (1) 100 parts by mass of squid parietal bones were added to 500 parts by volume of a 4 wt% sodium hydroxide solution, reacted at 90°C for 6 hours (the sodium hydroxide solution was changed every 2 hours), and the obtained product was washed to neutrality. (2) 10 parts by mass of the product was added to 300 parts by volume of anhydrous ethanol solution, and immersed at 65°C for 2 hours; the immersion treatment was repeated 3 times to obtain high-purity β-chitin fibers with a layered structure and a multi-level oriented structure.

[0073] The molecular chain amino groups and hydroxyl groups of the beta-chitin fiber of the present invention can aggregate ions, and the fiber has a suitable internal space and a multi-scale layered structure, and can be used as an organic template in a bionic mineralization strategy.

[0074] (3) Preparation of Tris buffer: Dissolve Tris buffer in 1 L of deionized water, adjust the pH to 7.4 with 36% concentrated hydrochloric acid, and finally adjust the volume to 2 L. Seal and store. This solution is used as a solvent for preparing disodium hydrogen phosphate and calcium chloride solutions.

[0075] (4) Preparation of mineralization solution: Prepare 100 mL of 5.34 mmol / L disodium hydrogen phosphate solution and place it in a beaker, add 5 mg of polyacrylic acid, stir at room temperature for 5 hours until it is completely dissolved, then add 100 mL of 9 mmol / L calcium chloride solution and mix thoroughly.

[0076] (5) Preparation of scaffold material: 0.1 parts by mass of β-chitin fiber was added to 50 parts by volume of mineralization solution and placed in a 37°C incubator for mineralization (e.g., 5 days) to obtain a scaffold material of β-chitin fiber mineralized hydroxyapatite. The SEM observation image of the mineralized scaffold is shown in FIG. Figure 4 shown.

[0077] (6) Cell osteogenic activity test: The β-chitin fiber mineralized scaffold material was co-cultured with bone marrow mesenchymal stem cells. The specific steps are as follows:

[0078] a. Cell culture: Mouse bone marrow mesenchymal stem cells were used as seed cells to evaluate the cell compatibility of the material in vitro. The cells were cultured in a high-glucose culture medium containing 10% fetal bovine serum and 1% double antibody; the culture conditions were 37°C, 95% relative humidity, and 5% CO 2 concentration; the culture medium was changed every two days.

[0079] b. Prepare osteogenic induction medium: Add three osteogenic induction agents, L-ascorbic acid (50 μg / mL), b-sodium glycerophosphate (10 mmol / L), and dexamethasone (10 nmol / L) in the high glucose medium in the following proportions, and mix thoroughly to ensure that each component is evenly dispersed. The concentration in brackets refers to the concentration of the osteogenic induction agent in the high glucose medium.

[0080] c. Extract preparation: To simulate the conditions of co-culture of β-chitin mineralized scaffold material and cells, the material extract was prepared according to the following steps. First, 30 mg of β-chitin mineralized scaffold material was placed in a clean bench for UV sterilization for 24 hours, and then 3 mL of osteogenic induction culture medium was added, and placed in an incubator overnight to obtain an extract (10 mg / mL).

[0081] d. Cell seeding: BMSCs were plated at 1×10 5The cells / well were inoculated in a 24-well plate and placed in an incubator for incubation. When the cell adhesion and fusion reached 80%, the high-glucose culture medium was replaced with a material extract containing an osteogenic induction agent (1 mL per well), which was used as the β-chitin mineralized scaffold group and recorded as day 0. Repeat step d, but replace the material extract with an osteogenic induction culture medium, as the culture plate group, recorded as day 0. In addition, in the β-chitin mineralized scaffold group, after replacing the high-glucose culture medium in the well plate with the material extract, 3 mL of fresh osteogenic induction culture medium should be added again to continue the material extraction to prepare the extract required for the next liquid change.

[0082] e. Determination of cell osteogenic markers: After 7 and 14 days of culture, alkaline phosphatase was qualitatively analyzed using an alkaline phosphatase colorimetric kit, and AKP kit and BCA protein content detection kit were used for quantitative analysis. After 14 and 21 days of culture, calcium nodules were qualitatively analyzed using Alizarin Red dye, and quantitatively analyzed using cetylpyridinium chloride (10wt%) working solution. The test results of alkaline phosphatase and calcium nodules are shown in Figure 2. Figure 5 The results showed that β-chitin mineralized scaffold material can induce cell mineralization and has good osteogenic activity.

[0083] (7) Animal experiment of scaffold materials: The two ends of the β-chitin fiber were mineralized (the lengths were 1.6 cm and 1 cm respectively), and the original state of the β-chitin fiber was maintained in the middle (the length was 1 cm), to obtain a composite scaffold material, which was then implanted into the complete defect site of the anterior cruciate ligament of rats. The tissue healing and regeneration were evaluated by histological analysis, the effect of bone integration was analyzed by Micro-CT scanning, and the mechanical recovery of the reconstructed ligament was tested by biomechanical testing, indicating the promoting effect of the mineralized scaffold on ligament repair and regeneration in rats. The experiment was divided into three groups (each group had 3 parallel samples): autologous flexor digitorum longus tendon transplantation group (Control), composite scaffold material group (CH) and composite scaffold material combined with autologous flexor digitorum longus tendon group (CHA). The experimental animals were 8-week-old male SD rats. The experimental steps are as follows:

[0084] a. Modeling and implantation: An experimental animal model of complete anterior cruciate ligament injury in rats was established and the graft was implanted.

[0085] b. Histological analysis: The animals were sacrificed at 4, 8, and 12 weeks after surgery to evaluate their tissue characteristics. The specimens were placed in a 10% EDTA solution for decalcification. After complete decalcification, they were dehydrated, embedded, and cut into tissue sections, followed by staining with safranin fast green, Masson, and toluidine blue. For immunohistochemical analysis, endogenous peroxidase was blocked with a 3% hydrogen peroxide solution for 25 minutes, blocked with 3% BSA and rabbit serum for 30 minutes, and incubated overnight at 4°C with type I collagen antibody (5 μg / mL), collagen III antibody (1:100), and TNMD (1:2000). The sections were observed and imaged using an optical microscope.

[0086] c. Micro-CT technology and three-dimensional model reconstruction technology were used to evaluate the specimens at 4, 8, and 12 weeks after surgery to analyze the integration of the graft in the bone tunnel. After the scan was completed, the image was reconstructed in three dimensions using mimics software along the long axis of the tibial tunnel, and the bone volume ratio of the new bone around the medullary canal to that inside was calculated.

[0087] d. Biomechanical testing of the specimens was performed 12 weeks after surgery to evaluate the biomechanical recovery of the grafts. The soft tissue surrounding the grafts was carefully dissected and removed, and the femur-graft-tibia complex was then fixed to the fixture of a universal testing machine, with a preload applied to correct the clamping position of the specimen. Next, the graft was stretched at a constant loading rate of 5 mm / min until it broke or was pulled out of the bone tunnel, and the ultimate failure load and stiffness were recorded.

[0088] Figure 6 The histological staining section observation results of the repair of completely injured anterior cruciate ligament in rats with β-chitin fiber mineralized scaffold material, including safranin fast green staining, Masson staining and toluidine blue staining. Figure 7 The results of immunohistochemical staining of the sections of the rat anterior cruciate ligament completely injured by β-chitin fiber mineralized scaffold material were observed, including the staining analysis of type I collagen, type III collagen, and tendon regeneration-related proteins (SCX and TNMD). Figure 8 Micro-CT scanning analysis and observation results of the repair of completely injured anterior cruciate ligament in rats with β-chitin fiber mineralized scaffold material, including the scan image of the new bone in the bone tunnel (A), and the bone volume ratio analysis of the new bone inside (B) and around (C) the bone tunnel. Fig. 9 These are the test results of the fracture load (A) and stiffness (B) of the reconstructed ligament after the β-chitosan fiber mineralized scaffold material of the present invention was implanted in vivo.

[0089] As can be seen from the figure, the composite scaffold of the present invention can not only promote collagen deposition and trabecular regeneration (such as Figure 6), promoting the expression of type I collagen, type III collagen, SCX and TNMD proteins (as shown in Figure 7 It can also promote the regeneration of bone trabeculae inside and around the bone marrow duct and promote the integration of the complex with bone (as shown in Figure 8 As shown in Figure 2 ); and, as the tissue grows in, the ligament repaired by the composite scaffold has better biomechanical properties (as shown in Figure 2 ). Fig. 9 shown).

[0090] Example 4

[0091] A ligament / tendon repair material, specifically a β-chitin fiber functionalized composite scaffold for promoting ligament / tendon repair, comprising β-chitin fiber, polydopamine and chondroitin sulfate. The preparation method is as follows:

[0092] (1) 100 parts by mass of squid parietal bones were added to 1000 parts by volume of a 5 wt % potassium hydroxide solution, and reacted at 80° C. for 8 h (the potassium hydroxide solution was changed every 2 h), and the obtained product was washed until neutral.

[0093] (2) 10 parts by mass of the product were added to 200 parts by volume of an anhydrous ethanol solution containing 4 wt% polysorbate 80, and the mixture was immersed in water at 50°C for 2 h, washed, and the immersion and washing were repeated 3 times to obtain high-purity β-chitin fibers with a layered structure and a multi-level oriented structure, which were freeze-dried for storage.

[0094] (3) Prepare a 2 mg / mL dopamine solution by dissolving 20 mg of dopamine powder in 10 mL of deionized water and stirring evenly in the dark.

[0095] (4) Preparation of scaffold materials:

[0096] a. Take 10 parts by mass of β-chitin fiber and put it into 40 parts by volume of the above dopamine solution, and react for 1 hour in the dark. Take out the product and wash it with deionized water to remove free dopamine;

[0097] b. The above product was immersed in 10 parts by volume of a chondroitin sulfate solution with a concentration of 5 mg / mL, reacted for 5 hours, and then washed with deionized water three times to obtain a polydopamine and chondroitin sulfate functionalized β-chitin fiber composite scaffold.

[0098] (5) Cell activity test: The β-chitin fiber functionalized scaffold material was co-cultured with bone marrow mesenchymal stem cells. The cells could proliferate and differentiate normally on the scaffold, showing good cell compatibility and ideal biocompatibility. The results were similar to those in Example 3 and are not described in detail here.

[0099] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing β-chitin fiber material, characterized in that The squid cartilage is processed with alkali solution and ethanol solution in sequence; the alkali solution is sodium hydroxide or potassium hydroxide solution; the concentration of the alkali solution is 4-20wt%; the concentration of the ethanol solution is greater than or equal to 85%.

2. The preparation method according to claim 1, characterized in that: The mass ratio of squid cartilage to alkali solution is 1:5-1:40; when using ethanol solution for treatment, the mass ratio of reactant to ethanol solution is 1:10-1:30; the time of alkali solution treatment is 6-24h; the time of ethanol solution treatment is 1-10h.

3. The preparation method according to claim 1, characterized in that: The ethanol solution also contains polysorbate 80 in a concentration of 0-10 wt%.

4. A β-chitin fiber material, characterized in that The method is prepared by any one of claims 1 to 3.

5. Use of the β-chitin fiber material according to claim 4 in the preparation of ligament / tendon repair materials.

6. A ligament / tendon repair material, characterized in that: The component comprises the β-chitosan fiber material according to claim 4.

7. The ligament / tendon repair material according to claim 6, characterized in that: The components also contain active substances; the active substances include at least one of hydroxyapatite, calcium carbonate, cell growth factor, polypeptide, platelet lysate, hyaluronan, chondroitin sulfate and collagen.

8. A ligament / tendon repair material, characterized in that: The components include the β-chitin fiber material as claimed in claim 4 and hydroxyapatite crystals mineralized on the fiber matrix.

9. A method for preparing the ligament / tendon repair material according to claim 8, characterized in that The β-chitosan fiber material according to claim 4 is immersed in a mineralizing liquid for mineralization.

10. A ligament / tendon repair material, characterized in that: The components include the β-chitin fiber material according to claim 4, polydopamine and chondroitin sulfate.