TiCoNb-based sliding bearing and preparation method thereof

Sliding bearings with self-healing function are manufactured using TiCoNb-based materials and laser fused deposition technology, which solves the problem of lubrication failure of sliding bearings under extreme working conditions, achieves high lubrication performance and low friction coefficient, and is suitable for aviation aircraft.

CN118775432APending Publication Date: 2024-10-15ANYANG INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410824089.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing sliding bearings experience high friction heat and lubrication failure under extreme working conditions such as sudden load changes and high temperatures and heavy loads, resulting in increased friction and wear and affecting the safety and stability of aerospace vehicles.

Method used

TiCoNb-based materials are used to prepare sliding bearings, and vacuum air atomization technology and laser fused deposition technology are used to manufacture sliding bearings with sinusoidal hole structures and self-healing functions. Friction reducing agents and anti-friction agents are used to form a lubricating film on the friction surface, and Vacuum hot pressure infiltration is carried out in the annular cavity to achieve self-regulation of lubrication and self-healing of the friction surface.

Benefits of technology

It achieves high lubrication performance and low friction coefficient under extreme working conditions, reduces friction and wear, improves the stability and self-healing ability of sliding bearings, and is suitable for key lubrication components such as aviation aircraft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118775432A_ABST
    Figure CN118775432A_ABST
Patent Text Reader

Abstract

The invention discloses a TiCoNb-based sliding bearing and a preparation method thereof, and relates to the technical field of composite material preparation of sliding bearings, the TiCoNb-based sliding bearing comprises elastic elements and an outer ring, an annular cavity is arranged between the outer ring and an outer ring lining, a plurality of groups of elastic elements are arranged in the annular cavity in the vertical direction, the outer ring lining communicates with the annular cavity through the elastic elements, and the outer ring lining communicates with the annular cavity through the elastic elements. A plurality of groups of inner side channels are uniformly distributed on the inner surface of the outer ring lining along the vertical direction, the shape of each group of inner side channels is two tracks of which the sine function is y = A * sin (x / T), the difference between the initial phases of the two sine functions is pi, and materials for manufacturing the TiCoNb-based sliding bearing outer ring lining comprise an antifriction agent, an antifriction agent, a self-healing material and a TiCoNb matrix, the TiCoNb-based sliding bearing has the advantages of lubrication self-regulation function, interface self-healing capability, excellent lubrication stability, corrosion resistance, fatigue resistance and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a TiCoNb-based sliding bearing and a preparation method thereof, and relates to the technical field of composite structure bearing component preparation and lubrication. Background Art

[0002] Improving the friction reduction of key components is of great engineering wear resistance significance for energy conservation and consumption reduction, environmental protection, and the promotion of healthy development of the social economy and environment. Sliding bearings, as key components of mechanical equipment, are currently mainly made of bearing materials such as M50 and M50NiL. However, their high density and poor friction reduction and wear resistance can no longer meet the lightweight structural applications of modern aircraft. In particular, the high friction heat caused by sudden load changes and high temperature and heavy loads is the main factor leading to the increased friction and wear of sliding bearings and the failure of surface lubrication. This directly affects the safety and stability of aviation flight and restricts the layout and technological development of my country's aviation industry. TiCoNb-based sliding bearings have low density, high specific strength, corrosion resistance and high temperature resistance, and are the preferred structural materials for sliding bearings. In order to solve the important engineering problem of lubrication of sliding bearing interface, the present invention provides a TiCoNb-based sliding bearing with lubrication self-regulation function and surface self-healing ability. It still has high load-bearing capacity, good thermodynamic properties, excellent lubrication stability, lubrication self-regulation and friction surface self-healing function under extreme working conditions such as load mutation and high temperature and heavy load, and overcomes the engineering problem that grease is difficult to achieve excellent lubrication under extreme working conditions. The specific preparation process of a TiCoNb-based sliding bearing disclosed by the present invention is: firstly weigh the friction reducer, anti-friction agent, self-healing powder and TiCoNb matrix according to a certain proportion; mechanically ball mill the anti-friction agent, self-healing material and TiCoNb matrix powder; then mechanically vibrate and mix the self-healing material, TiCoNb matrix powder, friction reducer, anti-friction agent, etc. to obtain the ingredients that are mixed evenly. Spherical self-healing powder and TiCoNb matrix powder are prepared by vacuum gas atomization technology, and the two are mechanically vibrated and mixed to obtain a uniformly mixed laser additive manufacturing ingredient; a sliding bearing with a sinusoidal hole structure, a friction-reducing and anti-friction agent annular cavity and a self-healing function is deposited by laser melting. Then, the friction-reducing agent and the anti-friction agent are mechanically vibrated to obtain a uniformly mixed friction-reducing and anti-friction agent mixed powder. On this basis, the friction-reducing and anti-friction agent mixed powder is melt-infiltrated into the sinusoidal / cosine hole structure and the annular cavity by vacuum hot pressing equipment to obtain a TiCoNb-based sliding bearing with surface self-healing and lubrication self-regulation function. This sliding bearing has a short preparation cycle, simple operation and easy control, good self-healing ability of the friction surface, high lubrication self-regulation function, stable tribological performance, etc. It has high application value and development potential for key lubrication components such as aviation aircraft. Summary of the invention

[0003] The purpose of the present invention is to provide a sliding bearing having an outer ring with a cavity, and a plurality of elastic elements are arranged in the cavity, the outer ring lining is provided with two sinusoidal function channels with different phases, the outer ring of the sliding bearing is printed by additive manufacturing technology, and friction reducers and wear resistant agents are added to the cavity and the channel by vacuum infiltration technology, so as to provide a sliding bearing with self-healing ability, stable lubrication, corrosion resistance and fatigue resistance.

[0004] The technical solution adopted by the present invention to solve the above-mentioned engineering problems is: a TiCoNb-based sliding bearing, comprising an elastic element 1, an outer ring liner 2, an inner ring 3, an inner channel 4, and an outer ring 6. An annular cavity 5 is arranged between the outer ring 6 and the outer ring liner 2. Multiple groups of elastic elements 1 are arranged in the annular cavity 5 along the up and down directions. Each group of elastic elements consists of elastic elements 1 uniformly distributed along the circumferential direction of the outer cylindrical surface of the outer ring 6. The elastic element 1 is a butterfly spring structure with two large ends arranged opposite to each other. The outer ring liner 2 is connected to the annular cavity 5 through the elastic element 1. The inner surface of the outer ring liner 2 is uniformly provided with multiple groups of inner channels 4 along the up and down directions. The shape of each group of inner channels 4 is the trajectory of two sinusoidal functions y=A×sin(x / T). The two sinusoidal functions have the same period and amplitude of y=A×sin(x / T), but the initial phase difference is π. Each sinusoidal function is connected end to end. The inner surface of the outer ring liner 2 is a porous structure, and the pores are used to accommodate and store lubricating materials.

[0005] Preferably, the structure in which the outer ring lining 2 is connected to the annular cavity 5 through the elastic element 1 is as follows: the outer small end of the elastic element 1 is fixed on the inner wall of the outer ring 6, the inner small end of the elastic element 1 is fixed on the outer ring lining 2, and the inner cavity of the elastic element 1 and the elastic element 1 are provided with a plurality of axially penetrating connecting holes 101 evenly distributed along the circumferential direction of the elastic element 1, which are used to connect the inner cavity of the elastic element 1 with the annular cavity 5, and the inner cavity of the elastic element 1 is also connected with the connecting holes 203 provided on the outer ring lining 2, and a plurality of groups of connecting holes 203 are provided on the outer ring lining 2 along the upper and lower sides, and each group of connecting holes 203 is provided with a plurality of connecting holes 203 evenly distributed along the circumferential direction of the outer cylindrical surface of the outer ring 6, and the number of groups of connecting holes 203 is the same as the number of groups of elastic element 1.

[0006] Preferably, in the y=A×sin(x / T), A is 2000 μm, T is 10 μs, the channel hole diameter of the inner channel 4 is 800 μm, the channel hole cross-section is semicircular, x is the central angle of the outer ring lining 2 along the vertical center, the unit is radian, y is the vertical displacement, and the connecting hole 203 is located in the middle position of the two sinusoidal function trajectories.

[0007] Preferably, the elastic element has a large end diameter of 2000 μm, a small end diameter of 800 μm, a wall thickness of 100 μm, a height of 600 μm, and a connecting hole 101 with a diameter of 50 μm.

[0008] Preferably, the material for making the TiCoNb-based sliding bearing outer ring lining 2 includes a friction reducer composed of AuCuZn, AuCd and AgCd, an anti-friction agent composed of ZrO and TiSiC, a self-healing material, and a TiCoNb matrix.

[0009] Preferably, the mass ratio of the friction reducer to the anti-friction agent is 5:1, the mass ratio of AuCuZn:AuCd:AgCd in the friction reducer is 3:2:1, wherein the atomic ratio of AuCuZn is 4:3:1, the atomic ratio of AuCd is 2:1, and the atomic ratio of AgCd is 4:1; the mass ratio of ZrO:TiSiC in the anti-friction agent is 2:1, wherein the atomic ratio of ZrO is 1:1, and the atomic ratio of TiSiC is 2:1:2; the mass ratio of TiCoNb matrix to self-healing material is 7:1; the self-healing material includes NiAl and MoCu, wherein the mass ratio of NiAl:MoCu is 3:1, the atomic ratio of NiAl is 1:1, and the atomic ratio of MoCu is 10:7; the atomic ratio of Ti, Co, Nb, B and Cr in the TiCoNb matrix is ​​6:5:4:3:1; the bearing outer ring lining 2 is made of the same material as the elastic element 1 and the inner channel 4.

[0010] Preferably, the method for preparing the TiCoNb-based sliding bearing comprises the following steps:

[0011] (1) weighing a friction reducer, an anti-friction agent, a self-healing material and a TiCoNb matrix powder according to a proportion, mechanically ball-milling the anti-friction agent into a 500 nm mixed powder, mechanically ball-milling the self-healing material into a 700 nm powder, mechanically ball-milling the Ti, Co, Nb, B and Cr powders of the TiCoNb matrix into a 300 nm mixed powder, and mechanically vibrating and mixing the self-healing mixed powder, the TiCoNb matrix powder, the friction reducer powder and the anti-friction agent powder respectively;

[0012] (2) preparing the self-healing material into spherical self-healing powder by vacuum gas atomization technology, and preparing the TiCoNb matrix powder into TiCoNb matrix spherical powder;

[0013] (3) mechanically vibrating and mixing the spherical self-healing powder and the TiCoNb matrix spherical powder to obtain a laser additive manufacturing material, and laser melting and depositing the laser additive manufacturing material layer by layer from bottom to top to form a structure of an elastic element 1, an outer ring lining 2, an inner channel 4, an annular cavity 5, and an outer ring 6;

[0014] (4) Laser additive manufacturing materials are subjected to laser melting deposition, and a mixed powder of the friction reducer and the anti-friction agent is placed in the inner channel 4 and the annular cavity 5 by using vacuum hot pressing and infiltration technology;

[0015] (5) The inner surface of the outer ring liner 2 and the outer surface of the outer ring 6 are processed and then pressed into the bearing inner ring 3 to obtain a TiCoNb-based sliding bearing.

[0016] Preferably, the mechanical ball milling speed of the self-healing material is 1000 rpm, the ball-to-material mass ratio is 9:2, and the ball milling time is 15 hours. The mechanical ball milling speed of the TiCoNb matrix powder is 11000 rpm, the ball-to-material mass ratio is 9:2, and the ball milling time is 16 hours. The mechanical vibration mixing frequency of the spherical self-healing powder is 60 Hz, and the vibration time is 140 min. The mechanical vibration mixing frequency of the TiCoNb matrix spherical powder is 65 Hz, and the vibration time is 150 min. The mechanical vibration mixing frequency of the friction reducer is 55 Hz, and the vibration time is 110 min. The mechanical vibration mixing frequency of the anti-friction agent is 57 Hz, and the vibration time is 120 min.

[0017] Preferably, the vacuum gas atomization melting temperature of the spherical self-healing powder is 1250°C, the melting time is 120 min, the cooling liquid is ultrapure water, and the vacuum degree is 5.4×10 -2 Pa, TiCoNb matrix spherical powder vacuum gas atomization melting temperature is 1300 ℃, melting time is 125min, cooling liquid is ultrapure water, vacuum degree is 5.7×10 -2 Pa, the friction reducer powder and the anti-friction agent powder are mechanically vibrated and mixed at a frequency of 45 Hz for 50 min, and the spherical self-healing powder and the TiCoNb matrix spherical powder are mechanically vibrated and mixed at a frequency of 40 Hz for 45 min.

[0018] Preferably, the laser melting deposition power is 110W, the scanning mode is line scanning, the filling spacing is 0.05μm, the linear speed is 3500mm / s, the powder feeding rate is 5g / min, the cladding thickness is 300nm, the protective gas is nitrogen, the applied pressure is 0.25Mpa, and the mixed powder of the friction reducer and the anti-friction agent is placed in the inner channel 4 and the annular cavity 5. The infiltration temperature is 1000℃, the infiltration pressure is 40MPa, the infiltration time is 100min, and the heating rate is 100℃ / min. When processing the inner surface of the outer ring lining 2 and the outer surface of the outer ring 6, the turning speed is 1000r / min, the turning thickness is 200μm, and the fine grinding speed is 1350r / min for fine grinding. The surface and peripheral burrs and flash of the TiCoNb-based sliding bearing are cleaned with a polishing machine. The equipment speed is 700r / min and the temperature is 70℃.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention introduces friction reducers and anti-friction agents, prepares sinusoidal microporous flow channels on the friction surface, enhances the enrichment of friction reducers and anti-friction agents on the friction surface, and guides the friction reducers and anti-friction agents to flow on the friction surface under the action of friction force, accelerates the formation of solid lubricating film, promotes the surface fluidity of friction reducers and anti-friction agents, enhances the improvement of lubrication performance of friction interface, and meets the lubrication requirements of sliding bearings under extreme working conditions such as load mutation, high temperature and heavy load, strong radiation and high vacuum;

[0021] 2. The present invention introduces friction reducers, anti-friction agents and annular cavities inside the friction surface of the outer ring lining, and sets elastic elements in the annular cavity. The friction reducers and anti-friction agents are melt-infiltrated into the annular cavity by vacuum hot pressing technology, so that the friction reducers and anti-friction agents can be precipitated from the annular cavity to the friction surface by porous capillary principle, high temperature expansion characteristics and extrusion principle under variable load or high temperature heavy load conditions, thereby improving the self-regulating ability of the TiCoNb-based sliding bearing lubrication, and obtaining a small friction coefficient, low wear rate, stable lubrication performance, an average friction coefficient of 0.15-0.17, a fluctuation value of 0.01-0.03, and an average wear rate of 0.19-0.21×10 -5 cm 3 N -1 m -1 , the fluctuation value is 0.02-0.04.

[0022] 3. The present invention uses shape memory alloy NiAl / MoCu as a self-healing material, uses vacuum gas atomization technology to prepare it into spherical particles, and then mixes it with TiCoNb matrix spherical powder. A TiCoNb-based sliding bearing with self-healing ability and lubrication self-regulation function is prepared by combining spherical powder with laser melting deposition technology. The self-healing function of friction surface damage and the self-regulation ability of lubrication performance are realized during the friction process. Such a friction surface has a short preparation cycle, simple process, high efficiency, low energy consumption, easy to master and control operation process, good repeatability and stability of results, and can be produced on a large scale, in batches and mechanized.

[0023] 4. The spherical powder prepared by the vacuum gas atomization technology used in the present invention has high purity, low oxygen content, small particle size and narrow size distribution. The porous butterfly spring and sine-cosine microporous structure prepared by laser melting deposition technology have high precision, regular shape and uniform distribution. TiCoNb-based sliding bearings have dense structure, low density, high specific strength, stable high-temperature mechanical physical and chemical properties, high friction surface bearing capacity, good surface self-healing and damage resistance, excellent lubrication performance, etc., which can well replace grease lubrication to improve the lubrication requirements of sliding bearings under extreme working conditions such as load mutation, high temperature and heavy load, strong radiation and high vacuum. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1is a schematic diagram of the structure of a TiCoNb-based sliding bearing in implementation case 1;

[0025] Figure 2 This is a schematic diagram of the overall dissection of a TiCoNb-based sliding bearing structure in Example 1;

[0026] Figure 3 is a cross-sectional view of an elastic element of a TiCoNb-based sliding bearing structure in Example 1;

[0027] Figure 4 It is a process flow chart for preparing TiCoNb-based sliding bearings;

[0028] Figure 5 This is a field emission electron microscope scanning morphology image of TiCoNb-based spherical powder prepared by vacuum gas atomization technology;

[0029] Figure 6 This is a field emission electron microscope scanning morphology of the cross-sectional structure of the inner lining of the outer ring of a TiCoNb-based sliding bearing;

[0030] Figure 7 It is a bar graph of the average friction coefficient of the inner lining of the outer ring of the TiCoNb-based sliding bearing after 160 minutes of dry sliding in implementation case 1-3;

[0031] Figure 8 It is a bar chart of the average wear rate of the outer ring liner of the TiCoNb-based sliding bearing after 160 minutes of dry sliding in implementation case 1-3;

[0032] Fig. 9 This is the field emission scanning electron microscope morphology of the friction surface of the inner lining of the outer ring of the TiCoNb-based sliding bearing when the sliding friction lasts for 160 minutes in implementation case 1;

[0033] Fig.10 This is the field emission scanning electron microscope morphology of the fracture of the friction surface of the inner lining of the outer ring of the TiCoNb-based sliding bearing when the sliding friction lasted for 160 minutes in implementation case 1;

[0034] Fig.11 This is the field emission scanning electron microscope morphology of the self-healing process of the friction surface of the outer ring lining of the TiCoNb-based sliding bearing in the implementation case 2 with sliding friction time ranging from 65min to 75min: a-sliding time 65min, b-sliding time 69min, c-sliding time 72min, d-sliding time 75min

[0035] Fig.12 This is the field emission scanning electron microscope morphology of the fractured surface of the inner lining of the friction outer ring of the TiCoNb-based sliding bearing when the sliding friction was 80 minutes in implementation case 3;

[0036] Fig.13This is the field emission scanning electron microscope morphology of the fractured surface of the inner lining of the friction outer ring of the TiCoNb-based sliding bearing at 83 minutes of sliding friction in implementation case 3;

[0037] Fig.14 It is a cross-sectional view of the outer ring lining.

[0038] Figure numerals: 1-elastic element, 101-connecting hole one, 2-outer ring lining, 201-self-healing material, 202-TiCoNb matrix, 203-connecting hole two, 3-inner ring, 4-inner channel, 5-annular cavity, 6-outer ring. DETAILED DESCRIPTION

[0039] To fully understand the present invention, Figure 1 The design and preparation process and performance test flow chart of a TiCoNb-based sliding bearing shown in the figure illustrates the specific contents disclosed in the present invention in combination with specific implementation cases and drawings. The test conditions are dry friction time of 160 min, applied load of 50-70 N, ambient temperature of 700-800 ° C, sliding speed of 0.50-0.75 m / s, friction radius of 3-5 mm, and friction test of 5 times under the same working condition. The lubrication performance, self-regulating function and self-healing function of the dry sliding bearing are disclosed, but the present invention is not limited to the following implementation cases.

[0040] A TiCoNb-based sliding bearing comprises: an elastic element 1, an outer ring liner 2, an inner ring 3, an inner channel 4, an annular cavity 5, an outer ring 6, and an outer ring 7. Figure 1 The up and down directions and the left and right directions of the present application are defined respectively to facilitate the description of the present application. The outer ring 6 is coaxially arranged with the outer ring liner 2. An annular cavity 5 is arranged between the outer ring 6 and the outer ring liner 2. Multiple groups of elastic elements 1 are arranged in the annular cavity 5 along the up and down directions. Each group of elastic elements is composed of elastic elements 1 uniformly distributed along the circumferential direction of the outer cylindrical surface of the outer ring 6. The elastic element 1 is a butterfly spring structure with two large ends arranged opposite to each other. The outer small end of the elastic element 1 is fixed to the inner wall of the outer ring 6, and the inner small end of the elastic element 1 is fixed to the outer ring liner 2. The elastic element 1 is a butterfly spring structure with two large ends arranged opposite to each other. The outer small end of the elastic element 1 is fixed to the inner wall of the outer ring 6, and the inner small end of the elastic element 1 is fixed to the outer ring liner 2. The inner cavity of element 1 and the elastic element 1 are provided with a plurality of axially penetrating connecting holes 101 uniformly distributed along the circumferential direction of the elastic element 1, which are used to connect the inner cavity of the elastic element 1 with the annular cavity 5. The inner cavity of the elastic element 1 is also connected with the connecting holes 203 provided on the outer ring liner 2. The outer ring liner 2 is provided with a plurality of groups of connecting holes 203 along the upper and lower sides. Each group of connecting holes 203 is uniformly provided with a plurality of connecting holes 203 along the circumferential direction of the outer cylindrical surface of the outer ring 6. The number of groups of connecting holes 203 is the same as that of the elastic element 1. The inner ring 3 and the outer ring liner 2 are spherical clearance fits.

[0041] Implementation Case 1

[0042] The inner surface of the outer ring lining 2 is evenly distributed with multiple groups of inner channels 4 along the up and down directions, and the shape of each group of inner channels 4 is a trajectory of two sinusoidal functions y=A×sin(x / T), the two sinusoidal functions y=A×sin(x / T) have the same period and amplitude, but the initial phase difference is π, each sinusoidal function is connected end to end, where A is 2000μm, T is 10μs, the channel hole diameter is 800μm, the channel hole cross-section is semicircular, x is the central angle of the outer ring lining 2 along the vertical center, the unit is radian, y is the vertical displacement, and the connecting hole 203 is located in the middle position of the two sinusoidal function trajectories.

[0043] The elastic element has a large end diameter of 2000 μm, a small end diameter of 800 μm, a wall thickness of 100 μm, a height of 600 μm, and a connecting hole 101 with a diameter of 50 μm.

[0044] The materials for making the outer ring lining 2 of the TiCoNb-based sliding bearing include a friction reducer composed of AuCuZn, AuCd and AgCd, an anti-friction agent composed of ZrO and TiSiC, a self-healing material, a TiCoNb matrix, and the bearing outer ring lining 2 is the same as the elastic element 1 and the inner channel 4. The mass ratio of the friction reducer to the anti-friction agent is 5:1, and the mass ratio of AuCuZn:AuCd:AgCd in the friction reducer is 3:2:1; wherein the atomic ratio of AuCuZn is 4:3:1, the atomic ratio of AuCd is 2:1, and the atomic ratio of AgCd is 3:2:1. The Cd atomic ratio is 4:1, the ZrO:TiSiC mass ratio in the anti-friction agent is 2:1, of which the ZrO atomic ratio is 1:1, the TiSiC atomic ratio is 2:1:2, and the mass ratio of the TiCoNb matrix to the self-healing material is 7:1; the self-healing material includes NiAl and MoCu, of which the NiAl:MoCu mass ratio is 3:1, the NiAl atomic ratio is 1:1, the MoCu atomic ratio is 10:7, and the Ti, Co, Nb, B and Cr atomic ratios in the TiCoNb matrix are 6:5:4:3:1.

[0045] A method for preparing a TiCoNb-based sliding bearing comprises the following steps:

[0046] According to the above ratio, the friction reducer, anti-friction agent, self-healing material and TiCoNb matrix powder are weighed, the anti-friction agent is mechanically ball-milled into a 500nm mixed powder, the self-healing material is mechanically ball-milled into a 700nm powder, the Ti, Co, Nb, B and Cr powders of the TiCoNb matrix are mechanically ball-milled into a 300nm mixed powder, the self-healing material is mechanically ball-milled at a speed of 1000 rpm, the ball-to-material mass ratio is 9:2, the ball-milling time is 15 hours, the TiCoNb matrix powder is mechanically ball-milled at a speed of 11000 rpm, the ball-to-material mass ratio is 9:2, and the ball-milling time is 16 hours. Subsequently, the self-healing mixed powder, TiCoNb matrix powder, friction reducer powder and anti-friction agent powder are mechanically vibrated and mixed respectively. The mechanical vibration mixing frequency of the spherical self-healing powder is 60 Hz, and the vibration time is 140 min. The mechanical vibration mixing frequency of the TiCoNb matrix spherical powder is 65 Hz, and the vibration time is 150 min. The mechanical vibration mixing frequency of the friction reducer is 55 Hz, and the vibration time is 110 min. The mechanical vibration mixing frequency of the anti-friction agent is 57 Hz, and the vibration time is 120 min.

[0047] The self-healing material was prepared into spherical self-healing powder by vacuum air atomization technology, and TiCoNb matrix powder was prepared into TiCoNb matrix spherical powder. The vacuum air atomization melting temperature of the spherical self-healing powder was 1250℃, the melting time was 120min, the cooling liquid was ultrapure water, and the vacuum degree was 5.4×10 -2 Pa, TiCoNb matrix spherical powder vacuum gas atomization melting temperature is 1300 ℃, melting time is 125min, cooling liquid is ultrapure water, vacuum degree is 5.7×10 -2 Pa, Figure 5 Shown is a field emission electron microscope scanning morphology image of TiCoNb-based spherical powder prepared by vacuum air atomization technology. The friction reducer powder and the anti-friction agent powder are mechanically vibrated and mixed at a frequency of 45 Hz for 50 min. The spherical self-healing powder and the TiCoNb matrix spherical powder are mechanically vibrated and mixed at a frequency of 40 Hz for 45 min.

[0048] The spherical self-healing powder and the TiCoNb matrix spherical powder were mechanically vibrated and mixed to obtain the laser additive manufacturing material. The laser additive manufacturing material was laser melt deposited layer by layer from bottom to top to form the structure of elastic element 1, outer ring lining 2, inner channel 4, annular cavity 5, and outer ring 6. The laser melting deposition power was 110W, the scanning mode was line scanning, the filling spacing was 0.05μm, the line speed was 3500mm / s, the powder feeding rate was 5g / min, the cladding thickness was 300nm, the protective gas was nitrogen, the applied pressure was 0.25Mpa, and the friction reducer and anti-friction agent mixed powder was placed in the inner channel 4 and the annular cavity 5 by vacuum hot pressing infiltration technology. The infiltration temperature was 1000℃, infiltration pressure of 40MPa, infiltration time of 100min, heating rate of 100℃ / min, then the inner surface of the outer ring liner 2 and the outer surface of the outer ring 6 are processed, the turning speed is 1000r / min, the turning thickness is 200μm, the fine grinding speed is 1350r / min, the surface and surrounding burrs and flash of the TiCoNb-based sliding bearing are cleaned by a polishing machine, the equipment speed is 700r / min, the temperature is 70℃, and then the inner ring 3 of the bearing is pressed into a TiCoNb-based sliding bearing. Figure 6 Shown is a field emission electron microscope scanning morphology of the cross-sectional structure of a TiCoNb-based sliding bearing.

[0049] After Vickers hardness test, the prepared TiCoNb-based sliding bearing has an average Vickers hardness of 6.35GPa in three tests. When the load is 50N, the ambient temperature is 700℃, the sliding speed is 0.50m / s, the friction radius is 3mm, and the dry sliding friction time is 160min, the average friction coefficient and the average wear rate after three friction and wear tests are as follows: Figure 7 and Figure 8 As shown by Figure 7 and Figure 8 It can be seen that the average friction coefficient of a TiCoNb-based sliding bearing is 0.15, the maximum fluctuation amplitude is 0.01, and the average wear rate is 0.21×10 -5 cm 3 N -1 m -1 , the maximum fluctuation amplitude is 0.04, Fig. 9 This is a field emission scanning electron microscope morphology image of the surface of the inner lining of the friction outer ring of a TiCoNb-based sliding bearing when the sliding friction lasted for 160 minutes in implementation case 1. The TiCoNb-based sliding bearing has excellent self-lubricating performance, good self-regulation function and interface self-healing ability.

[0050] Implementation Case 2

[0051] The mass ratio of friction reducer to anti-friction agent is 10:3, the mass ratio of AuCuZn:AuCd:AgCd is 6:4:3, among which the atomic ratio of AuCuZn is 8:6:3, the atomic ratio of AuCd is 20:13, the atomic ratio of AgCd is 2:1, the mass ratio of ZrO:TiSiC is 5:3; among which the atomic ratio of ZrO is 2:3, the atomic ratio of TiSiC is 5:2:4, the mass ratio of TiCoNb matrix to self-healing material is 14:3; among which the mass ratio of NiAl:MoCu in the self-healing material is 2:1, the atomic ratio of NiAl is 2:1, and the atomic ratio of MoCu is 4:3; the atomic ratio of Ti, Co, Nb, B and Cr in TiCoNb is 12:10:8:6:3, the inner channel 4 function y=A×sin(x / T), among which A is 2100μm, T is 10μs, and the inner channel diameter is 900μm.

[0052] The elastic element has a large end diameter of 2500 μm, a small end diameter of 900 μm, a wall thickness of 130 μm, an elastic element height of 800 μm, and a connecting hole 101 with a diameter of 55 μm.

[0053] The friction reducer, anti-friction agent, self-healing material and TiCoNb matrix powder are weighed according to the above proportions. The anti-friction agent is mechanically ball-milled into a 650nm mixed powder, the self-healing material is mechanically ball-milled into a 750nm self-healing mixed powder, the TiCoNb matrix Ti, Co, Nb, B and Cr powders are mechanically ball-milled into a 390nm mixed powder, the self-healing material is mechanically ball-milled at a speed of 1200 rpm, the ball-to-material mass ratio is 3:1, and the ball milling time is 17 hours, the TiCoNb matrix powder is mechanically ball-milled at a speed of 1200 rpm, the ball-to-material mass ratio is 9:2, and the ball milling time is 16 hours, and then the self-healing mixed powder and TiCoNb matrix powder are mechanically vibrated and mixed, the spherical self-healing powder is mechanically vibrated and mixed at a frequency of 75Hz, and the vibration time is 160min, the TiCoNb matrix spherical powder is mechanically vibrated and mixed at a frequency of 60Hz, and the vibration time is 140min, the friction reducer is mechanically vibrated and mixed at a frequency of 60Hz, and the vibration time is 130min, and the anti-friction agent is mechanically vibrated and mixed at a frequency of 55Hz, and the vibration time is 110min.

[0054] The self-healing mixed powder was prepared into spherical self-healing powder by vacuum air atomization technology, and TiCoNb matrix powder was prepared into TiCoNb matrix spherical powder. The obtained spherical self-healing powder and TiCoNb matrix spherical powder were mechanically vibrated and mixed to obtain laser additive manufacturing material. The vacuum air atomization melting temperature of the spherical self-healing powder was 1450℃, the melting time was 150min, the cooling liquid was ultrapure water, and the vacuum degree was 7.2×10 -2Pa, TiCoNb matrix spherical powder vacuum gas atomization melting temperature is 1450 ℃, melting time is 150min, cooling liquid is ultrapure water, vacuum degree is 6.75×10 -2 Pa, the obtained friction reducer powder and anti-friction agent powder are mechanically vibrated and mixed at a frequency of 50 Hz for 60 min, and the spherical self-healing powder and TiCoNb matrix spherical powder are mechanically vibrated and mixed at a frequency of 45 Hz for 50 min.

[0055] The laser additive manufacturing material is laser melt-deposited layer by layer from bottom to top to form the structure of elastic element 1, outer ring lining 2, inner channel 4, annular cavity 5, and outer ring 6. The laser melting deposition power is 135W, the scanning mode is line scanning, the filling spacing is 0.10μm, the line speed is 4500mm / s, the powder feeding rate is 7.2g / min, the cladding thickness is 400nm, the protective gas is nitrogen, the applied pressure is 0.30Mpa, and the friction reducer and anti-friction agent are placed in the inner channel 4 and the annular cavity by vacuum hot pressing infiltration technology. The infiltration temperature is 1050℃ and the infiltration pressure is 2000nm. The pressure is 45MPa, the infiltration time is 130min, and the heating rate is 110℃ / min to obtain a TiCoNb-based sliding bearing, which is then machined. The inner surface of the outer ring liner 2 and the outer surface of the outer ring 6 are then machined at a turning speed of 1150r / min, a turning thickness of 300μm, and a fine grinding speed of 1550r / min. The bearing surface and surrounding burrs and flash are cleaned using a polishing machine. The equipment speed is 750r / min, the temperature is 75℃, and the inner ring 3 is pressed into a TiCoNb-based sliding bearing as described in claim 1.

[0056] Vickers hardness test shows that the average Vickers hardness of the TiCoNb-based sliding bearing prepared in this case is 6.55GPa after three tests. When the load is 50-70N, the ambient temperature is 750℃, the sliding speed is 0.62m / s, the friction radius is 4mm, and the dry sliding friction time is 160min. After three friction and wear tests, the average friction coefficient and average wear rate are as follows: Figure 7 and Figure 8 As shown. Figure 7 and Figure 8 It can be seen that the average friction coefficient of a TiCoNb-based sliding bearing is 0.16, the maximum fluctuation amplitude is 0.02, and the average wear rate is 0.20×10 -5 cm 3 N -1 m -1 , the maximum fluctuation amplitude is 0.03. Fig.11Shown is a field emission scanning electron microscope morphology of the self-healing process of the inner lining surface of the friction outer ring of a TiCoNb-based sliding bearing in the sliding friction time range from 65min to 75min in implementation case 2. From the figure, it is not difficult to find that after the sliding friction test was carried out for 65min, a peeling area appeared on the friction surface. When the friction test was from 65min to 72min, the friction surface morphology confirmed that the surface peeling area was well repaired. When the friction test was carried out for 75min, the friction surface had been completely repaired, forming a smooth friction and wear morphology. This confirms that a TiCoNb-based sliding bearing has good self-healing and lubrication self-regulation functions, and has excellent self-lubricating performance, good self-regulation function and interface self-healing ability.

[0057] Implementation Case 3

[0058] The mass ratio of friction reducer to anti-friction agent is 5:2, the mass ratio of AuCuZn:AuCd:AgCd is 3:2:2; the atomic ratio of AuCuZn is 4:3:2, the atomic ratio of AuCd is 4:3, the atomic ratio of AgCd is 4:3, the mass ratio of ZrO:TiSiC is 10:7, the atomic ratio of ZrO is 1:2, the atomic ratio of TiSiC is 3:1:2, the mass ratio of TiCoNb matrix to self-healing material is 7:2, the mass ratio of self-healing material NiAl:MoCu is 3:2, the atomic ratio of NiAl is 3:1, the atomic ratio of MoCu is 5:4, and the atomic ratio of Ti, Co, Nb, B and Cr in TiCoNb matrix is ​​6:5:4:3:2. The inner channel 4 function y=A×sin(x / T), where A is 2200μm, T is 10μs, and the inner channel diameter is 100μm.

[0059] The elastic element has a large end diameter of 3000 μm, a small end diameter of 1000 μm, a wall thickness of 150 μm, an elastic element height of 100 μm, and a connecting hole 101 with a diameter of 80 μm.

[0060] The friction reducer, anti-friction agent, self-healing material and TiCoNb-based powder were weighed according to the above proportions. The anti-friction agent was mechanically ball-milled into a mixed powder of 800 nm. The NiAl and MoCu powders were mechanically ball-milled into 900nm self-healing mixed powders, and the TiCoNb matrix Ti, Co, Nb, B and Cr powders were mechanically ball-milled into 450nm mixed powders. The mechanical ball-milling speed of NiAl and MoCu powders was 1300 rpm, the ball-to-material mass ratio was 9:4, and the ball-milling time was 20 hours. The mechanical ball-milling speed of TiCoNb matrix powder was 1300 rpm, the ball-to-material mass ratio was 18:7, and the ball-milling time was 17.5 hours. Subsequently, the self-healing mixed powder, TiCoNb matrix powder, friction reducer powder, and anti-friction agent powder were mechanically vibrated and mixed respectively. The mechanical vibration mixing frequency of the spherical self-healing powder was 75Hz, and the vibration time was 160min. The mechanical vibration mixing frequency of the TiCoNb matrix spherical powder was 70Hz, and the vibration time was 150min. The mechanical vibration mixing frequency of the friction reducer was 60Hz, and the vibration time was 120min. The mechanical vibration mixing frequency of the anti-friction agent was 60Hz, and the vibration time was 115min.

[0061] The self-healing material powder was prepared into spherical self-healing powder by vacuum gas atomization technology, and Ti, Co, Nb, B and Cr mixed powder was prepared into TiCoNb matrix spherical powder. The spherical self-healing powder and TiCoNb matrix spherical powder were mechanically vibrated and mixed to obtain a laser additive manufacturing material. The vacuum gas atomization melting temperature of the spherical self-healing powder was 1750℃, the melting time was 180min, the cooling liquid was ultrapure water, and the vacuum degree was 8.2×10 -2 The vacuum gas atomization melting temperature of TiCoNb matrix spherical powder is 1750℃, the melting time is 150min, the cooling liquid is ultrapure water, and the vacuum degree is 7.55×10 -2 Pa, the friction reducer powder and the anti-friction agent powder are mechanically vibrated and mixed at a frequency of 55 Hz for 70 min, and the spherical self-healing powder and the TiCoNb matrix spherical powder are mechanically vibrated and mixed at a frequency of 50 Hz for 55 min.

[0062] The laser additive manufacturing material is laser melt deposited layer by layer from bottom to top to form the structure of elastic element 1, outer ring lining 2, inner channel 4, annular cavity 5, and outer ring 6. The laser melting deposition power is 145W, the scanning mode is line scanning, the filling spacing is 0.15μm, the line speed is 5000mm / s, the powder feeding rate is 10g / min, the cladding thickness is 500nm, the protective gas is nitrogen, and the applied pressure is 0.35Mpa. Subsequently, the friction reducer and anti-friction agent are placed in the inner channel 4 and the annular cavity using vacuum hot pressing infiltration technology. The infiltration temperature is 1100℃, the infiltration pressure is 50MPa, the infiltration time is 150min, and the heating rate is 120℃ / min. The inner channel 4 function y=A×sin(x / T), where A is 2200μm, T is 10μs, and the inner channel diameter is 100μm.

[0063] The elastic element has a large end diameter of 3000 μm, a small end diameter of 1000 μm, a wall thickness of 150 μm, an elastic element height of 100 μm, and a connecting hole 101 with a diameter of 80 μm.

[0064] Subsequently, the inner surface of the outer ring liner 2 and the outer surface of the outer ring 6 are processed, with a turning speed of 1250r / min, a turning thickness of 400μm, and a fine grinding speed of 1650r / min. The burrs and flash on the bearing surface and the surrounding area are cleaned by a polishing machine. The equipment speed is 800r / min, the temperature is 80℃, and the inner ring 3 is pressed in to obtain a TiCoNb-based sliding bearing.

[0065] After Vickers hardness test, it is known that the average Vickers hardness value of a TiCoNb-based sliding bearing prepared in this case is 6.72GPa after three tests. When the applied load is 70N, the ambient temperature is 800℃, the sliding speed is 0.75m / s, the friction radius is 5mm, and the dry sliding friction time is 160min. After three friction and wear tests, the average friction coefficient and average wear rate are as follows Figure 7 and Figure 8 As shown. Figure 7 and Figure 8 It can be seen that the average friction coefficient of a TiCoNb-based sliding bearing is 0.17, the maximum fluctuation amplitude is 0.03, and the average wear rate is 0.19×10 -5 cm 3 N -1 m -1 , the maximum fluctuation amplitude is 0.02. Fig.12 This is the field emission scanning electron microscope morphology image of the fracture surface of the inner lining of the friction outer ring of the TiCoNb-based sliding bearing when the sliding friction was 80 minutes in implementation case 3. Fig.13 This is the field emission scanning electron microscope morphology of the fracture surface of the inner lining of the friction outer ring of the TiCoNb-based sliding bearing at 83 minutes of sliding friction in implementation case 3. Fig.12 and Fig.13 The fracture morphology of the friction surface shown in the figure shows that a large micro crack appeared at the friction section when the sliding friction time was 80 minutes; when the friction test was carried out to 83 minutes, the micro cracks at the friction section were well repaired, forming an excellent sliding friction section without damage defects. This confirms that the friction section of the TiCoNb-based sliding bearing has a good self-healing ability, which can significantly improve the lubrication performance of the sliding bearing and also play a good lubrication self-regulation function on its friction and wear performance.

[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, and these are all protected by the present invention.

Claims

1. A TiCoNb-based sliding bearing, characterized in that: The invention comprises an elastic element (1), an outer ring lining (2), an inner ring (3), an inner channel (4), and an outer ring (6). An annular cavity (5) is arranged between the outer ring (6) and the outer ring lining (2). A plurality of groups of elastic elements (1) are arranged in the annular cavity (5) along the up-down direction. Each group of elastic elements is composed of elastic elements (1) uniformly distributed along the circumferential direction of the outer cylindrical surface of the outer ring (6). The elastic element (1) is a butterfly spring structure with two large ends arranged opposite to each other. The outer ring lining (2) is connected to the annular cavity (5) through the elastic element (1). A plurality of groups of inner channels (4) are uniformly arranged on the inner surface of the outer ring lining (2) along the up-down direction. The shape of each group of inner channels (4) is the trajectory of two sinusoidal functions y=A×sin(x / T). The two sinusoidal functions y=A×sin(x / T) have the same period and amplitude, but the initial phase differs by π. Each sinusoidal function is connected end to end. The inner surface of the outer ring lining (2) is a porous structure.

2. The TiCoNb-based sliding bearing according to claim 1, characterized in that: The structure of the outer ring lining (2) being connected to the annular cavity (5) through the elastic element (1) is as follows: the outer small end of the elastic element (1) is fixed on the inner wall of the outer ring (6), the inner small end of the elastic element (1) is fixed on the outer ring lining (2), and the inner cavity of the elastic element (1) and the elastic element (1) are provided with a plurality of axially penetrating connecting holes (101) evenly distributed along the circumferential direction of the elastic element (1), which are used to connect the inner cavity of the elastic element (1) with the annular cavity (5), and the inner cavity of the elastic element (1) is also connected with the connecting holes (203) provided on the outer ring lining (2), and a plurality of groups of connecting holes (203) are provided on the outer ring lining (2) along the upper and lower sides, and each group of connecting holes (203) is provided with a plurality of connecting holes (203) evenly distributed along the circumferential direction of the outer cylindrical surface of the outer ring (6), and the number of groups of connecting holes (203) is the same as the number of groups of elastic elements (1).

3. The TiCoNb-based sliding bearing according to claim 2, characterized in that: In the above-mentioned y=A×sin(x / T), A is 2000 μm, T is 10 μs, the channel hole diameter of the inner channel (4) is 800 μm, the channel hole cross-section is semicircular, x is the central angle of the outer ring lining (2) along the vertical center, the unit is radian, y is the vertical displacement, and the second connecting hole (203) is located in the middle position of the two sine function trajectories.

4. The TiCoNb-based sliding bearing according to claim 3, characterized in that: The elastic element has a large end diameter of 2000 μm, a small end diameter of 800 μm, a wall thickness of 100 μm, a height of 600 μm, and a connecting hole 1 (101) with a diameter of 50 μm.

5. The TiCoNb-based sliding bearing according to claim 3, characterized in that: The materials for making the TiCoNb-based sliding bearing outer ring lining (2) include a friction reducer composed of AuCuZn, AuCd and AgCd, an anti-friction agent composed of ZrO and TiSiC, a self-healing material and a TiCoNb matrix.

6. The TiCoNb-based sliding bearing according to claim 5, characterized in that: The mass ratio of the friction reducer to the anti-friction agent is 5:1, the mass ratio of AuCuZn:AuCd:AgCd in the friction reducer is 3:2:1, wherein the atomic ratio of AuCuZn is 4:3:1, the atomic ratio of AuCd is 2:1, and the atomic ratio of AgCd is 4:1; the mass ratio of ZrO:TiSiC in the anti-friction agent is 2:1, wherein the atomic ratio of ZrO is 1:1, and the atomic ratio of TiSiC is 2:1:2; the mass ratio of TiCoNb matrix to the self-healing material is 7:1; the self-healing material comprises NiAl and MoCu, wherein the mass ratio of NiAl:MoCu is 3:1, the atomic ratio of NiAl is 1:1, and the atomic ratio of MoCu is 10:7; the atomic ratio of Ti, Co, Nb, B and Cr in the TiCoNb matrix is ​​6:5:4:3:1; the bearing outer ring lining (2) is made of the same material as the elastic element (1) and the inner channel (4).

7. A method for preparing a TiCoNb-based sliding bearing according to claim 5, characterized in that: The steps include: (1) weighing a friction reducer, an anti-friction agent, a self-healing material and a TiCoNb matrix powder according to a proportion, mechanically ball-milling the anti-friction agent into a 500 nm mixed powder, mechanically ball-milling the self-healing material into a 700 nm powder, mechanically ball-milling the Ti, Co, Nb, B and Cr powders of the TiCoNb matrix into a 300 nm mixed powder, and mechanically vibrating and mixing the self-healing mixed powder, the TiCoNb matrix powder, the friction reducer powder and the anti-friction agent powder respectively; (2) preparing the self-healing material into spherical self-healing powder by vacuum gas atomization technology, and preparing the TiCoNb matrix powder into TiCoNb matrix spherical powder; (3) mechanically vibrating and mixing the spherical self-healing powder and the TiCoNb matrix spherical powder to obtain a laser additive manufacturing material, and laser melting and depositing the laser additive manufacturing material layer by layer from bottom to top to form a structure of an elastic element (1), an outer ring lining (2), an inner channel (4), an annular cavity (5), and an outer ring (6); (4) laser additive manufacturing materials are subjected to laser melting deposition, and a mixed powder of a friction reducer and an anti-friction agent is placed in the inner channel (4) and the annular cavity (5) by using a vacuum hot pressing infiltration technique; (5) The inner surface of the outer ring liner (2) and the outer surface of the outer ring (6) are processed and then pressed into the bearing inner ring (3) to obtain a TiCoNb-based sliding bearing.

8. The method for preparing a TiCoNb-based sliding bearing according to claim 7, characterized in that: The mechanical ball milling speed of the self-healing material is 1000 rpm, the ball-to-material mass ratio is 9:2, and the ball milling time is 15 hours. The mechanical ball milling speed of the TiCoNb matrix powder is 11000 rpm, the ball-to-material mass ratio is 9:2, and the ball milling time is 16 hours. The mechanical vibration mixing frequency of the spherical self-healing powder is 60 Hz, and the vibration time is 140 minutes. The mechanical vibration mixing frequency of the TiCoNb matrix spherical powder is 65 Hz, and the vibration time is 150 minutes. The mechanical vibration mixing frequency of the friction reducer is 55 Hz, and the vibration time is 110 minutes. The mechanical vibration mixing frequency of the anti-friction agent is 57 Hz, and the vibration time is 120 minutes.

9. The method for preparing a TiCoNb-based sliding bearing according to claim 7, characterized in that: The spherical self-healing powder is melted by vacuum gas atomization at a temperature of 1250°C for 120 min, with ultrapure water as the cooling liquid and a vacuum degree of 5.4×10 -2 Pa, TiCoNb matrix spherical powder vacuum gas atomization melting temperature is 1300 ℃, melting time is 125min, cooling liquid is ultrapure water, vacuum degree is 5.7×10 -2 Pa, the friction reducer powder and the anti-friction agent powder are mechanically vibrated and mixed at a frequency of 45 Hz for 50 min, and the spherical self-healing powder and the TiCoNb matrix spherical powder are mechanically vibrated and mixed at a frequency of 40 Hz for 45 min.

10. The method for preparing a TiCoNb-based sliding bearing according to any one of claims 7 to 9, characterized in that: The laser melting deposition power is 110W, the scanning mode is line scanning, the filling spacing is 0.05μm, the line speed is 3500mm / s, the powder feeding rate is 5g / min, the cladding thickness is 300nm, the protective gas is nitrogen, the applied pressure is 0.25Mpa, the mixed powder of the friction reducer and the anti-friction agent is placed in the inner channel (4) and the annular cavity (5), the infiltration temperature is 1000℃, the infiltration pressure is 40MPa, the infiltration time is 100min, and the heating rate is 100℃ / min. When the inner surface of the outer ring lining (2) and the outer surface of the outer ring (6) are processed, the turning speed is 1000r / min, the turning thickness is 200μm, and the fine grinding speed is 1350r / min for fine grinding. The surface and peripheral burrs and flash of the TiCoNb-based sliding bearing are cleaned by a polishing machine. The equipment speed is 700r / min and the temperature is 70℃.