Preparation method of self-supporting sea-urchin-shaped nickel cobalt selenide electrode material and product and application of self-supporting sea-urchin-shaped nickel cobalt selenide electrode material

By preparing sea urchin-like nickel cobalt selenide electrode materials through hydrothermal reaction and selenization reaction on a nickel foam substrate, the problems of low energy density and insufficient cycle performance of supercapacitor electrode materials are solved, and high specific capacitance and excellent rate performance are achieved. Enhanced electrochemical and mechanical stability, suitable for supercapacitors.

CN118782401APending Publication Date: 2024-10-15CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966592.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The energy density of existing supercapacitor electrode materials is low, which affects their widespread commercial utilization. The cycle and rate performance of bimetallic selenides need to be improved, and the binder also affects the electrochemical performance.

Method used

Using the preparation method of self-supporting sea urchin-like nickel cobalt selenide electrode material, the nickel cobalt precursor is grown on the nickel foam substrate through hydrothermal reaction and selenization reaction to form a sea urchin-like structure, which is combined with the conductive base nickel foam to improve the electrochemical performance and Mechanical stability.

Benefits of technology

It significantly improves the specific capacitance, rate performance and cycle stability of the electrode material, enhances the electrochemical performance and mechanical stability, and is suitable for supercapacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782401A_ABST
    Figure CN118782401A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a self-supporting sea-urchin-shaped nickel-cobalt selenide electrode material, which comprises the following specific steps: 1) taking foamed nickel, firstly adding the foamed nickel into hydrochloric acid for soaking, then thoroughly washing the foamed nickel with ultrapure water and absolute ethyl alcohol, and placing the washed foamed nickel in a vacuum oven for drying to obtain A; 2) taking a beaker, adding ultrapure water, weighing Ni (NO3) 2.6 H2O, Co (NO3) 2.6 H2O, urea and ammonium fluoride, adding into the beaker, and stirring to obtain B; (3) taking a reaction kettle, adding the prepared A and B, and carrying out hydrothermal reaction to obtain a nickel-cobalt precursor; and 4) placing the nickel-cobalt precursor in a porcelain boat, covering the nickel-cobalt precursor with selenium powder, and then annealing the nickel-cobalt precursor in an argon atmosphere for 4 hours to obtain the self-supporting sea urchin-shaped nickel-cobalt selenide electrode material directly grown on the foamed nickel. The molar ratio of the Ni (NO3) 2.6 H2O to the Co (NO3) 2.6 H2O is 1: (2-3), the molar dosage of the urea is 4 times of the sum of the molar dosage of the Ni (NO3) 2.6 H2O and the molar dosage of the Co (NO3) 2.6 H2O, and the molar dosage of the ammonium fluoride is equal to the molar dosage of the urea.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of supercapacitors and electrode materials, and in particular, relates to a preparation method of a self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material, a product thereof and an application thereof. Background Art

[0002] Supercapacitors have broad application prospects due to their excellent power density, fast charge and discharge, and long service life. However, their relatively moderate energy density limits their widespread commercial use. The electrode material is the main factor affecting the electrochemical performance of supercapacitors. Therefore, the development of electrode materials with high specific capacity is of great research significance.

[0003] Compared with metal oxides and sulfides, metal selenides have higher conductivity and lower electronegativity, which is conducive to promoting redox reactions and can effectively improve electrochemical performance, gradually becoming a very promising supercapacitor material. Experiments and theories have proved that compared with single metal selenides, bimetallic selenides can provide richer redox reactions and lower charge transfer resistance due to the synergistic effect between the two metal elements, improve conductivity, and generally show better electrochemical performance. However, the cycle and rate performance of bimetallic selenides still need to be improved. In addition, the binder often used in electrode materials is also an important factor affecting their electrochemical performance. Summary of the invention

[0004] In view of this, the present invention aims to provide a preparation method of a self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material and its products and applications.

[0005] The present invention provides a method for preparing a self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material, and the specific steps are as follows:

[0006] A method for preparing a self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material, the specific steps are as follows:

[0007] 1) Take nickel foam, soak it in hydrochloric acid, rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven to obtain A;

[0008] 2) Take a beaker, add ultrapure water, weigh Ni(NO 3 ) 2 6H 2 O、Co(NO 3 ) 2 6H 2 O, urea and ammonium fluoride are added into a beaker, stirred, and B is obtained;

[0009] 3) Take a reaction kettle, add the prepared A and B to carry out hydrothermal reaction, and obtain a nickel-cobalt precursor;

[0010] 4) placing the nickel-cobalt precursor in a porcelain boat, covering it with selenium powder, and then annealing it in an argon atmosphere for 4 hours to obtain a self-supporting sea urchin-shaped nickel-cobalt selenide electrode material directly grown on nickel foam;

[0011] The Ni(NO 3 ) 2 6H 2 O and Co(NO 3 ) 2 6H 2 The molar ratio of Ni(NO) to O is 1:2-3, and the molar amount of urea is 3 ) 2 6H 2 O and Co(NO 3 ) 2 6H 2 The molar amount of ammonium fluoride is equal to the molar amount of urea.

[0012] In order to solve the above problems, the present invention uses nickel nitrate hexahydrate as a nickel source and cobalt nitrate hexahydrate as a cobalt source, firstly self-grows a nickel-cobalt precursor on a nickel foam substrate through a hydrothermal reaction, and then undergoes a selenization reaction to obtain an urchin-shaped nickel-cobalt selenide / nickel foam binder-free electrode material with excellent electrochemical performance and good cycle stability. This urchin-like structure can promote the full penetration of the electrolyte, accelerate the transmission of ions and electrons, improve the utilization rate of the electrode material, and thus improve the electrochemical performance; the introduced conductive substrate nickel foam not only strengthens the conductive network of the electrode material, provides sufficient active centers and abundant electroactive sites, ensures efficient and smooth electron transmission, but also enhances the mechanical stability and durability of the electrode through its unique physical structure, solving the problem of the binder affecting the electrochemical performance of the electrode material.

[0013] Furthermore, in step 1), the concentration of hydrochloric acid is 1-2 mol / L, the soaking time is 1-2 h, and the oven temperature is 40-50°C.

[0014] Furthermore, the quality of the ultrapure water in step 2) is Ni(NO 3 ) 2 6H 2 O、Co(NO 3 ) 2 6H 2 O, 30 to 80 times the weight of urea and ammonium fluoride.

[0015] Furthermore, the hydrothermal reaction conditions in step 3) are: temperature 130° C., time 5 h.

[0016] Furthermore, in step 4), the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.15.

[0017] Furthermore, the annealing conditions in step 4) are: temperature 400° C., time 4 h.

[0018] The second aspect of the present invention provides a self-supporting sea urchin-shaped nickel cobalt selenide electrode material prepared by the above method.

[0019] The present invention also provides an application of a self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material, which is used in a supercapacitor.

[0020] Beneficial effects:

[0021] The invention provides a method for preparing a self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material, wherein Ni(NO 3 ) 2 6H 2 O is a nickel source, Co(NO 3 ) 2 6H 2 O is the cobalt source. Under the conditions of urea and ammonium fluoride, the specific raw material ratio is: Ni(NO 3 ) 2 6H 2 O and Co(NO 3 ) 2 6H 2 The molar ratio of Ni(NO) to O is 1:2-3; the molar amount of urea is 3 ) 2 6H 2 O and Co(NO 3 ) 2 6H 2The molar amount of O is equal to 4 times of the molar amount of ammonium fluoride; the molar amount of ammonium fluoride is equal to the molar amount of urea. The present invention self-grows a nickel-cobalt precursor on a nickel foam substrate through a hydrothermal reaction, and then selenizes the nickel-cobalt precursor through a selenization annealing treatment to obtain a self-supporting sea urchin-shaped nickel-cobalt selenide electrode material. The present invention in situ grows a layer of sea urchin-shaped nickel-cobalt selenide on nickel foam through a simple hydrothermal reaction and selenization reaction. This unique sea urchin-shaped microsphere structure is assembled from nanorods radiating from the same central point, which increases the specific surface area, cleverly promotes the comprehensive penetration of the electrolyte, makes it easy to approach the active site, and greatly accelerates the migration rate of ions and electrons inside the material, thereby significantly improving the utilization rate of the active substances of the electrode material and further optimizing the overall electrochemical performance. At the same time, the conductive substrate nickel foam introduced not only strengthens the conductive network of the electrode material, ensuring the efficient and smooth electron transmission, but also enhances the mechanical stability and durability of the electrode through its unique physical structure, providing a more solid and reliable platform for electrochemical reactions. The electrode material prepared by the present invention has high specific capacitance and excellent rate performance, and shows excellent cycle stability (capacity retention rate is 90.4% after 5000 cycles), and has good application prospects in the energy field. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a SEM image of the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material prepared in Example 2 of the present invention;

[0023] Figure 2 This is the XRD pattern of the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material prepared in Example 2 of the present invention;

[0024] Figure 3 This is an XPS image of the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material prepared in Example 2 of the present invention;

[0025] Figure 4 CV and GCD diagrams of the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material prepared in Example 2 of the present invention;

[0026] Figure 5 This is a cyclic stability diagram of the self-supporting sea urchin-shaped nickel cobalt selenide electrode material prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification. The methods described are all conventional methods unless otherwise specified, and the raw materials described can be obtained from public commercial channels unless otherwise specified.

[0028] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0029] The preparation method of the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material provided by the present invention comprises the following specific steps:

[0030] 1) Take nickel foam, soak it in hydrochloric acid, rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven to obtain A;

[0031] 2) Take a beaker, add ultrapure water, weigh Ni(NO 3 ) 2 6H 2 O、Co(NO 3 ) 2 6H 2 O, urea and ammonium fluoride are added into a beaker, stirred, and B is obtained;

[0032] 3) Take a reaction kettle, add the prepared A and B to carry out hydrothermal reaction, and obtain a nickel-cobalt precursor;

[0033] 4) placing the nickel-cobalt precursor in a porcelain boat, covering it with selenium powder, and then annealing it in an argon atmosphere for 4 hours to obtain nickel-cobalt selenide grown directly on nickel foam;

[0034] The Ni(NO 3 ) 2 6H 2 O and Co(NO 3 ) 2 6H 2 The molar ratio of Ni(NO) to O is 1:2-3, and the molar amount of urea is 3 ) 2 6H 2 O and Co(NO 3 ) 2 6H 2 The molar amount of ammonium fluoride is equal to the molar amount of urea.

[0035] According to the present invention, preferably, the concentration of the hydrochloric acid is 1-2 mol / L, the soaking time is 1-2 h, and the oven temperature is 40-50 ° C; the mass of the ultrapure water in step 2) is Ni(NO 3 ) 2 6H 2 O、Co(NO 3 ) 2 6H 2O, urea and ammonium fluoride by weight 30 to 80 times; the hydrothermal reaction conditions in the step 3) are: temperature 130 ° C, time 3-12h; the annealing conditions in the step 4) are: 400 ° C, time 4h, and the mass ratio of the nickel cobalt precursor to the selenium powder in the step 4) is 1:1.15.

[0036] Example 1

[0037] 1) Take nickel foam, soak it in 1 mol / L hydrochloric acid for 1 hour, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0038] 2) Take a beaker, add 40 mL of ultrapure water, weigh 0.33 mmol Ni(NO 3 ) 2 6H 2 O, 0.67mmol Co(NO 3 ) 2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0039] 3) Take a 50mL reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5 hours to obtain a nickel-cobalt precursor;

[0040] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to selenium powder is 1:1.15), and then annealed at 400°C in an argon atmosphere for 4 hours to obtain a self-supporting sea urchin-shaped nickel-cobalt selenide electrode material directly grown on nickel foam.

[0041] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 1818 F / g.

[0042] Example 2

[0043] 1) Take nickel foam, soak it in 2 mol / L hydrochloric acid for 30 min, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0044] 2) Take a beaker, add 40 ml of ultrapure water, weigh 0.25 mmol Ni(NO 3 ) 2 6H 2 O, 0.75mmol Co(NO 3 )2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0045] 3) Take a 50ml reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5h to obtain a nickel-cobalt precursor;

[0046] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to selenium powder is 1:1.15), and then annealed at 400°C in an argon atmosphere for 4 hours to obtain a self-supporting sea urchin-shaped nickel-cobalt selenide electrode material directly grown on nickel foam.

[0047] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 2082 F / g.

[0048] Figure 1 This is a SEM image of the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material. A layer of sea urchin-shaped nickel-cobalt-selenide is in situ grown on the surface nickel foam. This unique sea urchin-shaped microsphere structure is assembled from nanorods radiating from the same central point, which increases the specific surface area and cleverly promotes the full penetration of the electrolyte, making it easy for it to approach the active sites, greatly accelerating the migration rate of ions and electrons inside the material, thereby significantly improving the utilization rate of the active substances of the electrode material and further optimizing the overall electrochemical performance.

[0049] Figure 2 The XRD pattern of the prepared self-supporting sea urchin-shaped nickel cobalt selenide electrode material. It can be seen from the figure that the diffraction peaks of the prepared self-supporting sea urchin-shaped nickel cobalt selenide can be compared with (Ni, Co)Se 2 The diffraction peaks of the standard card correspond to those of the electrode material, indicating that the electrode material was successfully prepared;

[0050] Figure 3 XPS image of the prepared self-supporting sea urchin-shaped nickel-cobalt selenide electrode material, indicating the successful selenization of nickel and selenium;

[0051] Figure 4 The CV and GCD diagrams of the prepared self-supporting sea urchin-shaped nickel cobalt selenide electrode material show obvious redox peaks in the CV curve, indicating that the electrode material has pseudocapacitive properties; the GCD curve shows that the specific capacitance of the electrode material at a current density of 1 A / g is as high as 2082 F / g.

[0052] Figure 5The cycling stability diagram of the prepared self-supporting sea urchin-shaped nickel cobalt selenide electrode material. After 5000 cycles, the capacity retention rate is as high as 90.4%, indicating that the electrode material has excellent cycling stability.

[0053] Comparative Example 1

[0054] 1) Take nickel foam, soak it in 2 mol / L hydrochloric acid for 30 min, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0055] 2) Take a beaker, add 40 ml of ultrapure water, weigh 1 mmol Co(NO 3 ) 2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0056] 3) Take a 50ml reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5h to obtain a nickel-cobalt precursor;

[0057] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.15), and then annealed at 400° C. in an argon atmosphere for 4 h to obtain nickel-cobalt selenide directly grown on nickel foam.

[0058] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 937 F / g.

[0059] Comparative Example 2

[0060] 1) Take nickel foam, soak it in 2 mol / L hydrochloric acid for 30 min, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0061] 2) Take a beaker, add 40 ml of ultrapure water, weigh 0.05 mmol Ni(NO 3 ) 2 6H 2 O, 0.95mmol Co(NO 3 ) 2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0062] 3) Take a 50ml reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5h to obtain a nickel-cobalt precursor;

[0063] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.15), and then annealed at 400°C in an argon atmosphere for 6 hours to obtain nickel-cobalt selenide directly grown on nickel foam.

[0064] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 978 F / g.

[0065] Comparative Example 3

[0066] 1) Take nickel foam, soak it in 1 mol / L hydrochloric acid for 30 min, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0067] 2) Take a beaker, add 40 ml of ultrapure water, weigh 0.5 mmol Ni(NO 3 ) 2 6H 2 O, 0.5mmol Co(NO 3 ) 2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0068] 3) Take a 50ml reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5h to obtain a nickel-cobalt precursor;

[0069] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.15), and then annealed at 400° C. in an argon atmosphere for 4 h to obtain nickel-cobalt selenide directly grown on nickel foam.

[0070] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 1312 F / g.

[0071] Comparative Example 4

[0072] 1) Take nickel foam, soak it in 1 mol / L hydrochloric acid for 30 min, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0073] 2) Take a beaker, add 40 ml of ultrapure water, weigh 0.67 mmol Ni(NO 3 ) 2 6H 2 O, 0.33mmol Co(NO 3 ) 2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0074] 3) Take a 50ml reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5h to obtain a nickel-cobalt precursor;

[0075] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.15), and then annealed at 400° C. in an argon atmosphere for 4 h to obtain nickel-cobalt selenide directly grown on nickel foam.

[0076] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 1068 F / g.

[0077] Comparative Example 5

[0078] 1) Take nickel foam, soak it in 1 mol / L hydrochloric acid for 30 min, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0079] 2) Take a beaker, add 40 ml of ultrapure water, weigh 0.75 mmol Ni(NO 3 ) 2 6H 2 O, 0.25mmol Co(NO 3 ) 2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0080] 3) Take a 50ml reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5h to obtain a nickel-cobalt precursor;

[0081] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.15), and then annealed at 400° C. in an argon atmosphere for 4 h to obtain nickel-cobalt selenide directly grown on nickel foam.

[0082] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 726 F / g.

[0083] Comparative Example 6

[0084] 1) Take nickel foam, soak it in 1 mol / L hydrochloric acid for 30 min, then rinse it thoroughly with ultrapure water and anhydrous ethanol, and dry it in a vacuum oven at 40°C to obtain A;

[0085] 2) Take a beaker, add 40 ml of ultrapure water, weigh 1 mmol Ni(NO 3 ) 2 6H 2 O, 4mmol urea and 4mmol ammonium fluoride were added into a beaker and stirred for 30min to obtain B;

[0086] 3) Take a 50ml reaction kettle, add the prepared A and B, and carry out hydrothermal reaction at 130°C for 5h to obtain a nickel-cobalt precursor;

[0087] 4) The nickel-cobalt precursor is placed in a porcelain boat, covered with selenium powder (the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.15), and then annealed at 400° C. in an argon atmosphere for 4 h to obtain nickel-cobalt selenide directly grown on nickel foam.

[0088] Electrochemical performance tests were conducted in a three-electrode system using an electrochemical workstation, including CV curves and GCD curves. Using nickel cobalt selenide as the working electrode, Pt mesh electrode as the counter electrode, Hg / HgO electrode as the reference electrode, and 3 mol / L KOH solution as the electrolyte solution, the specific capacitance of nickel cobalt selenide at a current density of 1 A / g was tested to be 137 F / g.

[0089] Table 1 Specific capacitance of selenides in Examples 1 to 2 and Comparative Examples 1 to 6 at a current density of 1 A / g

[0090]

[0091]

[0092] It can be seen from the results in Table 1 that the electrochemical properties of the nickel cobalt selenide prepared by the present invention are related to the ratio of nickel and cobalt metals. By optimizing different nickel and cobalt ratios, the specific capacity of the nickel cobalt selenide electrode material is effectively improved. The prepared self-supporting sea urchin-shaped nickel cobalt selenide electrode material has the characteristics of high specific capacitance, excellent rate performance and cycle stability, and has high application value.

[0093] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material, characterized in that: The specific steps are as follows: 1) Take nickel foam, soak it in hydrochloric acid, and then rinse it thoroughly with ultrapure water and anhydrous ethanol. Place in a vacuum oven to dry to obtain A; 2) Take a beaker, add ultrapure water, weigh Ni(NO3)2·6H2O, Co(NO3)2·6H2O, urea and ammonium fluoride, add them into the beaker, stir, and obtain B; 3) Take a reaction kettle, add the prepared A and B to carry out hydrothermal reaction, and obtain a nickel-cobalt precursor; 4) Place the nickel-cobalt precursor in a porcelain boat, cover it with selenium powder, and then anneal it in an argon atmosphere for 4 hours. A self-supporting sea urchin-shaped nickel cobalt selenide electrode material directly grown on nickel foam is obtained; The molar ratio of Ni(NO3)2·6H2O to Co(NO3)2·6H2O is 1:2-3, the molar amount of urea is 4 times the sum of the molar amounts of Ni(NO3)2·6H2O and Co(NO3)2·6H2O, and the molar amount of ammonium fluoride is equal to the molar amount of urea.

2. The method for preparing the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material according to claim 1, characterized in that: In the step 1), the concentration of hydrochloric acid is 1-2 mol / L, the soaking time is 1-2 hours, and the oven temperature is 40-50°C.

3. The method for preparing the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material according to claim 1, characterized in that: The mass of the ultrapure water in step 2) is 30 to 80 times the weight of Ni(NO3)2·6H2O, Co(NO3)2·6H2O, urea and ammonium fluoride.

4. The method for preparing the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material according to claim 1, characterized in that: The hydrothermal reaction conditions in step 3) are: temperature 130° C., time 5 h.

5. The method for preparing the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material according to claim 1, characterized in that: The annealing conditions in step 4) are: 400° C., time 4 h.

6. The method for preparing the self-supporting sea urchin-shaped nickel-cobalt-selenide electrode material according to claim 1, characterized in that: In the step 4), the mass ratio of the nickel-cobalt precursor to the selenium powder is 1:1.

15.

7. A self-supporting sea urchin-shaped nickel cobalt selenide electrode material prepared by the method for preparing a self-supporting sea urchin-shaped nickel cobalt selenide electrode material according to any one of claims 1 to 6.

8. Use of the self-supporting sea urchin-shaped nickel cobalt selenide according to claim 7, characterized in that it is used in a supercapacitor.