Reverse spinel type high-entropy oxide for negative electrode of lithium ion battery

By using the technology of organic ligands and metal-organic framework templates in high-entropy oxides, the preparation of inverse spinel-type high-entropy oxides for lithium-ion battery anode materials has been achieved, solving the problem of poor performance and cycling at high current densities. To solve the problem of poor stability, materials with high specific capacity and good cycle performance were obtained.

CN118782784APending Publication Date: 2024-10-15CHENGDU UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410896369.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing high-entropy oxide lithium-ion battery anode materials have poor electrochemical performance at high current densities, and it is difficult to achieve long-term cycle stability and uniform non-equimolar component adjustment, resulting in problems of phase separation and impurity introduction.

Method used

Organic ligands are used to capture strong metals, and metal-organic frameworks are used as templates to achieve atomic-level uniform mixing of 5-element metal elements. By adjusting the non-equimolar component ratios of metal elements, an inverse spinel-type single-phase high Entropic oxide (FexCryMnzNi0.1Zn0.1)3O4, combined with a specific heat treatment process, ensures the phase purity and performance optimization of the material.

Benefits of technology

It significantly improves the charge-discharge specific capacity and large current responsiveness of the material, achieves good cycle stability and high phase purity, reduces raw material costs, and is suitable for lithium-ion battery anodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782784A_ABST
    Figure CN118782784A_ABST
Patent Text Reader

Abstract

The invention relates to a reverse spinel type high-entropy oxide for a negative electrode of a lithium ion battery, and belongs to the technical field of lithium ion battery materials. The chemical formula of the reverse spinel type high-entropy oxide is (FexCryMnzNi0. 1Zn0. 1) 3O4, X + Y + Z + 0.2 = 1, 0.2 < = X < = 0.3, 0.2 < = Y < = 0.3, and 0.2 < = Z < = 0.3. The preparation method of the material comprises the following steps of: reacting a prepared metal ion mixed solution with an organic ligand dimethylimidazole solution by taking five nitrates of iron, nickel, chromium, manganese and zinc in non-equal molar ratio as metal ion sources to form a metal organic framework precursor, and roasting to obtain the single-phase high-entropy oxide with an inverse spinel type Fe3O4 crystal structure. According to the reverse spinel type high-entropy oxide, through adjustment of metal ion components, the coordination effect of all elements is fully exerted, the electrochemical performance is remarkably improved, the raw material cost is low, and application and popularization are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an inverse spinel high entropy oxide for a negative electrode of a lithium ion battery, belonging to the technical field of negative electrode materials for lithium ion batteries. Background Art

[0002] Transition metal oxides have been considered as a type of conversion-type anode materials for lithium-ion batteries. These materials exhibit multi-electron redox reactions, enabling them to achieve high specific capacities. However, they also suffer from a number of drawbacks, including poor cycling stability due to severe volume expansion and insufficient electronic conductivity.

[0003] High entropy oxide refers to an oxide that contains 5 or more metal elements in a single-phase structure. Due to the synergistic effect between the various metal elements, the electrochemical properties of the oxide can be significantly improved. In recent years, reports have begun to appear on the application of high entropy oxides in lithium-ion battery negative electrodes. Patent CN 202210559670.1 discloses a one-dimensional spinel-type (FeCoNiCrMn)3O4 high-entropy oxide negative electrode material. The cycle performance curve of the material when charged and discharged at a current density of 100 mA / g, after 100 cycles, its specific capacity is 410 mAh / g. The key point of this patent is to use an electrospinning process to prepare a one-dimensional spinel-type high-entropy oxide. Although the electrochemical performance of this material is improved to a certain extent at a low current density, it does not show the effect of a large current on its electrochemical performance. Patent CN201910886682.3 uses a solution combustion method to prepare a (Cr 0.2 Fe 0.2 Mn 0.2 Zn 0.2 Ni 0.2 )3O4 high entropy oxide negative electrode material. The first charge specific capacity of this material is 1126 mAh / g. After 30 cycles at a current density of 200mA / g, the reversible specific capacity is stabilized at 563 mAh / g. This material only shows a specific capacity of 30 charge and discharge cycles, and does not reflect the long-term cycle stability of the material. Most of the high entropy oxides reported in recent years have improved the electrochemical properties of the materials from the perspective of elemental composition or material morphology, and have not yet considered optimizing the electrochemical performance from the perspective of adjusting the ratio of metal ions. Patent CN116768614B uses ball milling to synthesize a high entropy oxide with a non-equimolar ratio of metal ions, and its chemical formula is (Co 0.4-n Ni n Cu 0.2 Zn 0.2 Al 0.2)Fe2O4, and found that high entropy oxides with non-equimolar ratios of metal ions are better in electromagnetic wave absorption. However, the material uses ball milling, which is not only easy to introduce impurities, but also cannot strictly control the amount of each element. The subsequent calcination temperature is also very high, and it is limited to electromagnetic wave absorption.

[0004] In fact, each element in the high entropy oxide has different valence change ranges and different functions. In order to give full play to the coordination effect of each element, the present invention proposes a large-scale component ratio adjustment of non-equimolar ratios of metal ions. The target chemical formula is (Fe x Cr y Mn z Ni 0.1 Zn 0.1 )3O4, wherein, X+Y+Z+0.2=1, 0.2≤X≤0.3, 0.2≤Y≤0.3, 0.2≤Z≤0.3. However, a large range of component ratio adjustment can easily lead to phase separation and the appearance of a heterogeneous phase, so it is very difficult to obtain a single-phase high-entropy oxide with uniform non-equimolar metal ions. The present invention utilizes the strong metal capture force of organic ligands and adopts a metal-organic framework as a template to achieve atomic-level uniform mixing of 5-element metal elements, and can accurately control the content of metal elements according to performance requirements over a large range, thereby successfully achieving an inverse spinel single-phase (Fe2O3) for lithium-ion battery negative electrode. x Cr y Mn z Ni 0.1 Zn 0.1 )3O4 high entropy oxide was prepared, and the charge-discharge specific capacity and large current responsiveness of the synthesized material were significantly improved. Summary of the invention

[0005] The purpose of the present invention is to provide an inverse spinel high entropy oxide for lithium ion battery negative electrode, which is an oxide of five metal elements, namely iron, nickel, chromium, manganese and zinc, in non-equimolar ratios, and provides a new component ratio and a matching preparation process for achieving high capacity of lithium ion battery negative electrode materials.

[0006] In order to achieve the above object, the present invention also provides a preparation process of the above-mentioned inverse spinel high entropy oxide, comprising the following steps: (1) According to the molar ratio of metal elements Fe:Cr:Mn:Ni:Zn=X:Y:Z:1:1, 4.04 g~6.06 g Fe(NO3)3·9H2O, 4 g~6 g Cr(NO3)2·9H2O, 2.51 g~3.765 g Mn(NO3)2·4H2O, 1.455 g Ni(NO3)2·6H2O, and 1.487 g Zn(NO3)2·4H2O were weighed and dissolved in 100 mL deionized water and mixed evenly to form solution A; (2) Weigh 16.422 g of dimethylimidazole and dissolve it in a mixed solution of 100 mL of deionized water and 50 mL of triethylamine. Mix well to form solution B. (3) Solution A and solution B were mixed and stirred for 4 h and aged for 4 h. The precipitated product was separated by centrifugation, washed with deionized water for 3 times, and dried at 60 °C for 8 h to obtain the precursor. (4) Place the precursor in a corundum crucible, heat it to 650-950°C at a rate of 5°C / min in an air atmosphere, keep it at that temperature for 1-5 h, and cool it to room temperature in the furnace to obtain the target product.

[0007] The present invention provides a chemical formula (FexNi1Cr y Mn z The new component ratio of Zn1)3O4 is an inverse spinel single-phase high entropy oxide with high phase purity. Compared with the high entropy oxide with equal molar ratio, the present invention better exerts the cocktail effect of multiple components through reasonable component adjustment, and the obtained metal ion non-equal molar ratio high entropy oxide has obvious advantages in capacity and rate performance, and also has good cycle stability. In addition, the raw material cost of the negative electrode material is low, which is conducive to promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 It is prepared in Example 1 (FexNi1Cr y Mn z SEM image of Zn1)3O4 inverse spinel high entropy oxide.

[0009] Figure 2 It is prepared in Example 1 (FexNi1Cr y Mn z XRD pattern of Zn1)3O4 inverse spinel high entropy oxide.

[0010] Figure 3 It is prepared in Example 1 (FexNi1Cr y Mn z Cycling performance diagram of Zn1)3O4 inverse spinel high entropy oxide.

[0011] Figure 4 It is prepared in Example 1 (FexNi1Cr y Mn z Rate performance diagram of Zn1)3O4 inverse spinel high entropy oxide. DETAILED DESCRIPTION

[0012] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It is particularly noted that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention. The raw materials used in the embodiments can all be obtained by commercial purchase. Example

[0013] (1) According to the molar ratio of the five elements Fe:Cr:Mn:Ni:Zn=3:3:2:1:1, 6.06 g Fe(NO3)3·9H2O, 6 g Cr(NO3)2·9H2O, 2.51 g Mn(NO3)2·4H2O, 1.455 g Ni(NO3)2·6H2O, and 1.487 g Zn(NO3)2·4H2O were weighed and dissolved in 100 mL deionized water and mixed evenly to form solution A. 16.422 g dimethylimidazole was weighed and dissolved in a mixed solution of 100 mL deionized water and 50 mL triethylamine, and mixed evenly to form solution B. The two solutions were then mixed, stirred for 4 h, aged for 4 h, centrifuged, and dried for 8 h. The dried precursor was ground and placed in a crucible, heated to 850 °C at a rate of 5 °C / min in an air atmosphere, kept at that temperature for 3 h, and cooled to room temperature in the furnace to obtain an inverse spinel high entropy oxide.

[0014] (2) The negative electrode material, binder (polyvinylidene fluoride), and conductive agent (acetylene black) were weighed in a ratio of 7:2:1 and mixed evenly in a mortar. Then, an appropriate amount of N-methylpyrrolidone was added and stirred with a magnetic stirrer for 12 h to obtain a uniform slurry.

[0015] (3) Copper foil was used as the current collector for coating. The coating was dried at 80 ºC under vacuum conditions for 24 h, cut into pieces and the mass of active material was weighed. Then, a CR2032 button battery case, a pure lithium sheet as the counter electrode, 1 mol / L LiPF6 / EC-DEC (volume ratio 1:1) as the electrolyte, and a polypropylene porous membrane as the separator were selected. The battery was assembled in an argon-filled glove box and the electrochemical performance was tested.

[0016] Figure 1 3 is a SEM photograph of the inverse spinel high entropy oxide obtained in Example 1. As shown in the figure, the average particle size of the inverse spinel high entropy oxide synthesized by the present invention is 60 nm.

[0017] Figure 2 This is the XRD spectrum of the inverse spinel high entropy oxide obtained in Example 1. As shown in the figure, the characteristic diffraction peaks of the inverse spinel high entropy oxide synthesized by the present invention are highly consistent with Fe3O4 (JCPDS: PDF#88-0866), without any impurity peaks, and the high peak intensity and narrow peak width indicate that the material has good crystallinity.

[0018] Figure 3 This is a cycle test diagram of the inverse spinel high entropy oxide obtained in Example 1. As shown in the figure, at a current density of 500 mA / g, the specific capacity can still reach 810 mAh / g after 420 cycles.

[0019] Figure 4 This is a rate test diagram of the inverse spinel high entropy oxide obtained in Example 1. As shown in the figure, at a high current density of 2000 mA / g, the average discharge specific capacity is still 320 mAh / g, and the structure of the material is stable after high current density charging and discharging. Example

[0020] According to the molar ratio of the five elements of Fe:Cr:Mn:Ni:Zn=3:2:3:1:1, 6.06 g Fe(NO3)3·9H2O, 4 g Cr(NO3)2·9H2O, 3.765 g Mn(NO3)2·4H2O, 1.455 g Ni(NO3)2·6H2O, and 1.487 g Zn(NO3)2·4H2O were weighed and dissolved in 100 mL deionized water and mixed evenly to form solution A. 16.422 g dimethylimidazole was weighed and dissolved in a mixed solution of 100 mL deionized water and 50 mL triethylamine, and mixed evenly to form solution B. The two solutions were then mixed, stirred for 4 h, aged for 4 h, centrifuged and dried for 8 h. The dried precursor was ground and placed in a crucible, heated to 850 °C at a rate of 5 °C / min in an air atmosphere, kept at that temperature for 3 h, and cooled to room temperature in the furnace to obtain an inverse spinel high entropy oxide. Example

[0021] According to the molar ratio of the five elements of Fe:Cr:Mn:Ni:Zn=2.5:3:2.5:1:1, 5.05 g Fe(NO3)3·9H2O, 6 g Cr(NO3)2·9H2O, 3.1375 g Mn(NO3)2·4H2O, 1.455 g Ni(NO3)2·6H2O, and 1.487 g Zn(NO3)2·4H2O were weighed and dissolved in 100 mL deionized water and mixed evenly to form solution A. 16.422 g dimethylimidazole was weighed and dissolved in a mixed solution of 100 mL deionized water and 50 mL triethylamine, and mixed evenly to form solution B. The two solutions were then mixed, stirred for 4 h, aged for 4 h, centrifuged and dried for 8 h. The dried precursor was ground and placed in a crucible, heated to 650 °C at a rate of 5 °C / min in an air atmosphere, kept at this temperature for 3 h, and cooled to room temperature in the furnace to obtain an inverse spinel high entropy oxide. Example

[0022] According to the molar ratio of the five elements of Fe:Cr:Mn:Ni:Zn=2.5:2.5:3:1:1, 5.05 g Fe(NO3)3·9H2O, 5 g Cr(NO3)2·9H2O, 3.765 g Mn(NO3)2·4H2O, 1.455 g Ni(NO3)2·6H2O, and 1.487 g Zn(NO3)2·4H2O were weighed and dissolved in 100 mL deionized water and mixed evenly to form solution A. 16.422 g dimethylimidazole was weighed and dissolved in a mixed solution of 100 mL deionized water and 50 mL triethylamine, and mixed evenly to form solution B. The two solutions were then mixed, stirred for 4 h, aged for 4 h, centrifuged and dried for 8 h. The dried precursor was ground and placed in a crucible, heated to 750 °C at a rate of 5 °C / min in an air atmosphere, kept at that temperature for 3 h, and cooled to room temperature in the furnace to obtain an inverse spinel high entropy oxide. Example

[0023] According to the molar ratio of the five elements of Fe:Cr:Mn:Ni:Zn=3:2.5:2.5:1:1, 6.06 g Fe(NO3)3·9H2O, 5 g Cr(NO3)2·9H2O, 3.1375 g Mn(NO3)2·4H2O, 1.455 g Ni(NO3)2·6H2O, and 1.487 g Zn(NO3)2·4H2O were weighed and dissolved in 100 mL deionized water and mixed evenly to form solution A. 16.422 g dimethylimidazole was weighed and dissolved in a mixed solution of 100 mL deionized water and 50 mL triethylamine, and mixed evenly to form solution B. The two solutions were then mixed, stirred for 4 h, aged for 4 h, centrifuged and dried for 8 h. The dried precursor was ground and placed in a crucible, heated to 950 °C at a rate of 5 °C / min in an air atmosphere, kept at this temperature for 3 h, and then cooled to room temperature in the furnace to obtain an inverse spinel high entropy oxide. Example

[0024] According to the molar ratio of the five elements of Fe:Cr:Mn:Ni:Zn=2:3:3:1:1, 4.04 g Fe(NO3)3·9H2O, 6 g Cr(NO3)2·9H2O, 3.765 g Mn(NO3)2·4H2O, 1.455 g Ni(NO3)2·6H2O, and 1.487 g Zn(NO3)2·4H2O were weighed and dissolved in 100 mL deionized water and mixed evenly to form solution A. 16.422 g dimethylimidazole was weighed and dissolved in a mixed solution of 100 mL deionized water and 50 mL triethylamine, and mixed evenly to form solution B. The two solutions were then mixed, stirred for 4 h, aged for 4 h, centrifuged and dried for 8 h. The dried precursor was ground and placed in a crucible, heated to 850 °C at a rate of 5 °C / min in an air atmosphere, kept at that temperature for 3 h, and cooled to room temperature in the furnace to obtain an inverse spinel high entropy oxide.

Claims

1. An inverse spinel high entropy oxide, the chemical formula of the high entropy oxide is (Fe x Cr y Mn z Ni 0.1 Zn 0.1 ) 3 O 4 , in, X+Y+Z+0.2=1,0.2≤X≤0.3,0.2≤Y≤0.3,0.2≤Z≤0.

3.

2. The inverse spinel high entropy oxide according to claim 1, It is characterized in that With single phase phase spinel Fe 3 O 4 Crystal structure.

3. The inverse spinel high entropy oxide according to claim 1, It is characterized in that Used as negative electrode material for lithium-ion batteries.

4. The molar ratio range of the elements of the inverse spinel high entropy oxide according to claim 1, in particular, the chemical formula ratio is (Fe 0.3 Cr 0.3 Mn 0.2 Ni 0.1 Zn 0.1 ) 3 O 4 The high-entropy oxide has a specific capacity of 810 mAh / g after 420 cycles at a current density of 500 mA / g, and a specific capacity of 350 mAh / g after 1000 charge and discharge cycles at a high current density of 2000 mA / g.

Citation Information

Cited By

  • Double-phase high-entropy oxide negative electrode material, preparation method and application

    CN121938888A

  • A two-phase high-entropy oxide negative electrode material, a preparation method and applications thereof

    CN121938888B