Surface-perovskite-controlled double-phase sodium-electrode layered positive electrode material and preparation method thereof
By using the O3/P3 composite phase structure controlled by surface perovskite in the positive electrode material of sodium ion battery, the content and sintering temperature of sodium and B elements are regulated, the problem of insufficient performance of single-phase structure is solved, and high cycle stability and high The capacity of biphasic sodium electrolaminated cathode material significantly improves the electrochemical performance.
Patent Information
- Application Number
- CN202411020938.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
AI Technical Summary
The single-phase structure of the existing sodium ion battery positive electrode material is difficult to achieve excellent rate performance, cycle stability and high capacity at the same time. In particular, O-type and P-type structures have their own shortcomings, making it difficult to take into account both stability and capacity.
The biphasic sodium electrolaminated cathode material with O3/P3 composite phase structure controlled by surface perovskite is prepared by regulating the content of sodium and B elements and controlling the sintering temperature, combined with wet ball milling method and solid phase sintering method, so the material is realized. Composite structure.
A high-purity and good crystallinity material was obtained, which significantly improved the transfer efficiency of sodium ions, suppressed irreversible phase change, improved the cyclic stability and rate performance of the material, and had high capacity and excellent electrochemical properties.
Smart Images

Figure HDA0004967239690000011 
Figure HDA0004967239690000012 
Figure HDA0004967239690000021
Abstract
Description
Technical Field
[0001] The invention relates to a sodium ion battery positive electrode material, and in particular to a surface perovskite-controlled dual-phase sodium-ion battery layered positive electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are widely used due to their high energy density, good cycle characteristics and low pollution. However, the shortage and high cost of lithium resources have limited their development to a certain extent. As the next generation of ion batteries, sodium-ion batteries have great potential in grid-scale storage applications due to their high sodium abundance, low cost and good availability. Among them, the positive electrode material is a key component that determines the energy density of sodium-ion batteries. The positive electrode materials of sodium-ion batteries mainly include layered oxides, polyanions and Prussian blue. Layered oxides have the characteristics of periodic layered structure, simple preparation method and high specific capacity, and are the main positive electrode materials for sodium-ion batteries.
[0003] At present, layered oxide materials can be divided into O-type and P-type structures. The P-type structure has good rate performance and cycle stability due to its lower sodium ion diffusion barrier, but its capacity is low due to its low sodium content. The O-type structure has a higher initial sodium content, so it has a higher specific capacity, but its structural phase change is complex, resulting in poor stability and rate performance. For example, the CN115064693A patent application discloses an O3 phase high entropy sodium ion battery positive electrode material, which is formed by mixing sodium salt and metal salt evenly and then firing by sol-gel method, but its high entropy configuration fails to effectively suppress the irreversible phase change during charging and discharging, and on the other hand, it fails to give full play to the capacity advantage of the O3 phase, and the electrochemical performance of the resulting positive electrode needs to be improved. The CN117638042A patent application discloses a P2 phase sodium ion battery positive electrode material, which is obtained by mixing sodium source, nickel manganese precursor, and tungsten source evenly and then calcining multiple times, but its capacity is negligible after tungsten doping, and its multiple calcination process is also time-consuming and labor-intensive. In short, the simple O phase and P phase are limited by their structural characteristics and are difficult to show excellent comprehensive performance. Therefore, combining single-phase materials to form multiphase materials, thereby constructing a composite multiphase structured positive electrode material is the most promising way to solve the above problems. For example, the CN115148984A patent application discloses an O3 / P2 composite phase sodium ion battery positive electrode material, which is a mixture of a sodium source and a transition metal M source, sintered, and ultra-rapidly cooled after sintering to obtain an O3-type oxide layer in the sintered material, and the sintered material is annealed at 200 to 800 ° C to form a P2-type oxide layer to obtain a core-shell structured O3 / P2 composite phase sodium ion positive electrode material. Thanks to the core-shell structure of the O3 / P2 composite phase, it has excellent charge and discharge specific capacity, excellent cycle performance, low surface residual alkali content, and excellent comprehensive performance of the material.
[0004] In summary, if the P phase and O phase are combined to complement each other to form a composite phase, it is a feasible solution. Therefore, by designing the P3 / O3 composite phase, the various properties of the P phase and the O phase can be compromised. However, how to design and introduce the composite phase and adjust the ratio of different phases to achieve the best performance is a difficult problem that needs to be solved urgently. Summary of the invention
[0005] In order to overcome the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a surface perovskite-controlled dual-phase sodium-electrode layered positive electrode material and a preparation method thereof. The composite positive electrode material is an O3 / P3 symbiotic phase structure controlled by a surface perovskite, which can be prepared by regulating the content of sodium and B elements and controlling the sintering temperature. It does not require new raw materials and additional synthesis processes, and has the characteristics of simple preparation process and low equipment requirements.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A double-phase sodium-electrode layered positive electrode material controlled by surface perovskite, which is a layered oxide, is a double-phase structure of O3 / P3 controlled by surface perovskite, and has the following general formula
[0008] A a B b O 3+u / Na c [Ni d Mn e B y-b A x-a ]O 2+f , where the general formula of perovskite is A a B b O 3+u The double intergrowth phase structure is O3 / P3 intergrowth phase, and the general structural formula is Na c [Ni d Mn e B y-b A x-a ]O 2+f , A is one of Ce, Y, La, and Gd, and B is one or more of transition metals Fe, Ti, Cr, and Mg.
[0009] The a, b, c, d, e, and f respectively correspond to the molar percentages of the elements; x and y respectively correspond to the addition amounts of element A and element B; and the relationship between them satisfies d+e+y-b+xa=1, (a+b) / (3+u)=1 / 3.
[0010] The a, b, c, d, e, and f respectively correspond to the molar percentages of the elements, 0.8≤a≤1, 0≤b≤0.9, 0.78≤c≤0.89, 0≤e≤0.5, 0 <y-b≤0.33,0<x-a≤0.05,-0.03≤f≤0.03。
[0011] A method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material comprises the following steps:
[0012] S1: according to the stoichiometric ratio of each element in the sodium ion battery positive electrode material to be prepared, a sodium source, a manganese source, a nickel source, a rare earth metal compound and a transition metal compound are weighed and dispersed in a solvent, and the mixed system is ball-milled to obtain a slurry;
[0013] S2: filtering, washing, and drying the slurry to obtain a precursor;
[0014] S3: The precursor is placed in air or oxygen atmosphere for high-temperature calcination. After the reaction is completed, it is naturally cooled to room temperature to obtain a surface perovskite-controlled dual-phase sodium-ion battery layered positive electrode material.
[0015] In step S1, the selected sodium source is a mixture of one or more of sodium sulfate, sodium carbonate, sodium bicarbonate, sodium nitrate, sodium chloride, and sodium acetate in any ratio;
[0016] In step S1, the selected manganese source is a mixture of one or more of manganese trioxide, manganese dioxide, manganese tetraoxide, manganese carbonate, manganese nitrate, manganese sulfate, manganese chloride, and manganese acetate in any ratio;
[0017] In step S1, the selected nickel source is one or a mixture of any ratio of nickel oxide, nickel sulfate, nickel chloride, nickel hydroxide, nickel nitrate, and nickel acetate;
[0018] In step S1, the selected rare earth metal compound is one or a mixture of any ratio of lanthanum oxide, lanthanum nitrate, cerium oxide, cerium nitrate, yttrium oxide, yttrium nitrate, gadolinium oxide, and gadolinium nitrate;
[0019] In step S1, the transition metal compound selected is a mixture of any ratio of one or more of ferric oxide, ferrous oxide, ferrous chloride, ferrous sulfate, ferrous carbonate, ferrous oxalate, ferrous nitrate, titanium dioxide, titanium tetrachloride, and magnesium chloride.
[0020] In the step S1, the solvent is a mixed solvent of deionized water and anhydrous ethanol, and the mixed volume ratio is 1:0-1.
[0021] In the step S1, the rotation speed of the ball mill is 500-800 r / min, and the ball milling time is 8-12 h.
[0022] In step S2, the washing liquid is an alkaline washing liquid.
[0023] In step S2, the drying method is spray drying, blast drying or vacuum drying.
[0024] In step S2, the drying temperature is 80-100°C, and the drying time is 8-12h.
[0025] In the step S3, the precursor is calcined in an air atmosphere, with a heating rate of 3-5°C / min, a calcination temperature of 700-950°C, a holding time of 10-24h, and a final sample is obtained when the temperature drops to room temperature.
[0026] In the step S3, the precursor is calcined in an oxygen atmosphere with a gas flow rate of 1-6 m / s.
[0027] Compared with the prior art, the invention is beneficial in that:
[0028] 1. The present invention adopts a wet ball milling method combined with a solid phase sintering method to synthesize a surface perovskite-controlled dual-phase sodium electrode layered positive electrode material, which has a simple synthesis process, a high yield, a low cost, and is easy for large-scale production.
[0029] 2. The typical feature of the composite layered positive electrode material of the present invention is that the surface perovskite and the bulk O3 / P3 structure are introduced into the structure to coexist. It is prepared by adjusting the content of sodium and B elements and controlling the sintering temperature, without the need for new raw materials and additional synthesis processes.
[0030] 3. The composite layered cathode material preparation method provided by the present invention has high phase purity, good crystallinity, defect-free crystal morphology, uniform particles, and sharp corners and edges. The electrode-electrolyte contact area is increased, the diffusion distance is shortened, the transfer of sodium ions is greatly promoted, and the side reaction between the active material and the electrolyte can be significantly inhibited.
[0031] 4. The composite layered cathode material of the present invention is doped with rare earth elements to improve the O3 type NaNi 0.33 Mn 0.33 Fe 0.33 The electronic structure of O2 is regulated to improve its electronic conductivity, expand the unit cell gap, stabilize the crystal structure, optimize the sodium ion transmission path, and significantly improve the sodium ion transmission kinetics. At the same time, the two-phase symbiotic structure can inhibit irreversible phase change and improve the overall structural stability of the material. Therefore, in addition to greatly improving the cycle stability, the electrochemical performance of the material also has both rate performance and capacity.
[0032] In summary, the surface perovskite-controlled dual-phase sodium-electrolyte layered positive electrode material of the present invention has a P3+O3 composite structure, which improves the cycle stability of the material, and uses rare earth element doping to stabilize the crystal structure and improve electronic conductivity, and the material has excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the SEM image of Example 1.
[0034] Figure 2 The first charge and discharge curves of the materials obtained in Example 1 and the comparative example at a 1C rate.
[0035] Figure 3 The first charge and discharge curves of the materials obtained in Example 2 and the comparative example at a 1C rate.
[0036] Figure 4 The first charge and discharge curves of the materials obtained in Example 3 and the comparative example at a 1C rate.
[0037] Figure 5 The first charge and discharge curves of the materials obtained in Example 4 and the comparative example at a 1C rate.
[0038] Figure 6 The graphs are the cycle performances of four embodiments and comparative example materials at 1C rate. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the embodiments described are only a part of the embodiments of the present invention, rather than the features in all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0040] Example 1
[0041] In this embodiment, a surface perovskite-controlled dual-phase sodium-electrode layered cathode material and a preparation method thereof include the following steps:
[0042] S1. Weigh a certain amount of sodium carbonate, manganese dioxide, nickel oxide, lanthanum oxide, and iron oxide according to the stoichiometric ratio, add them into a solvent consisting of deionized water and anhydrous ethanol in a volume ratio of 1:1 and disperse them. Then transfer the above system into a ball mill, adjust the speed to 500 r / min, and ball mill for 8 h to obtain a mixture slurry;
[0043] S2, filtering the obtained slurry, washing it with an alkaline detergent, and placing it in a blast drying oven for drying at a temperature of 80° C. for 8 h to obtain a precursor powder;
[0044] S3, the precursor powder was heated to 900℃ in air atmosphere at a heating rate of 3℃ / min and sintered for 12h to obtain LaFeO3 / Na[Ni 0.33 Mn 0.28 Fe 0.33 La 0.05 ]O2 electrode material.
[0045] The surface perovskite-controlled dual-phase sodium-electrode layered cathode material obtained in this embodiment is subjected to electrochemical testing, which specifically comprises the following steps:
[0046] The positive electrode material is mixed with a conductive additive (Super P) and a binder (polyvinylidene fluoride) in a mass ratio of 8:1:1. After sufficient grinding, an appropriate amount of solvent (N-methylpyrrolidone) is added to form a uniform black slurry. The positive electrode sheet is prepared through coating, drying and other process flows. The metal sodium sheet is used as the negative electrode, and a mixed solution of 1 mol / L NaPF6 and EC (ethylene carbonate) / DEC (diethyl carbonate) in a volume ratio of 1:1 is used as the electrolyte. A glass fiber separator is used to assemble the button battery in a glove box filled with argon gas with a water oxygen value below 0.1 ppm.
[0047] Charge and discharge test: The voltage range of button cell charge and discharge is 2.0-4.0V. Before the cycle test, it is activated at a smaller rate of 0.2C, and then cycled at a rate of 1C within the same voltage range to test its performance.
[0048] Example 2
[0049] In this embodiment, a surface perovskite-controlled dual-phase sodium-electrode layered cathode material and a preparation method thereof include the following steps:
[0050] S1. Weigh a certain amount of sodium sulfate, manganese chloride, nickel chloride, gadolinium nitrate, and ferrous oxide according to a stoichiometric ratio and disperse them in a solvent consisting of deionized water and anhydrous ethanol in a volume ratio of 1:0.5. Then transfer the above system to a ball mill, adjust the speed to 600 r / min, and ball mill for 9 hours to obtain a mixture slurry;
[0051] S2, filtering the obtained slurry, washing it with an alkaline detergent, and drying it in a blast drying oven at a temperature of 90° C. for 12 h to obtain a precursor powder;
[0052] S3, the precursor powder was heated to 950℃ in air atmosphere at a heating rate of 3℃ / min and sintered for 15h to obtain GdFeO3 / Na[Ni 0.33 Mn 0.28 Fe 0.33 G 0.05 ]O2 electrode material.
[0053] The surface perovskite-controlled dual-phase sodium-electrode layered cathode material obtained in this embodiment is subjected to electrochemical testing, which specifically comprises the following steps:
[0054] The positive electrode material is mixed with a conductive additive (Super P) and a binder (polyvinylidene fluoride) in a mass ratio of 8:1:1. After sufficient grinding, an appropriate amount of solvent (N-methylpyrrolidone) is added to form a uniform black slurry. The positive electrode sheet is prepared through coating, drying and other process flows. The metal sodium sheet is used as the negative electrode, and a mixed solution of 1 mol / L NaPF6 and EC (ethylene carbonate) / DEC (diethyl carbonate) with a volume ratio of 1:1 is used as the electrolyte. A glass fiber separator is used to assemble the button battery in a glove box filled with argon gas with a water oxygen value below 0.1 ppm.
[0055] Charge and discharge test: The voltage range of button cell charge and discharge is 2.0-4.0V. Before the cycle test, it is activated at a smaller rate of 0.2C, and then cycled at a rate of 1C within the same voltage range to test its performance.
[0056] Example 3
[0057] In this embodiment, a surface perovskite-controlled dual-phase sodium-electrode layered cathode material and a preparation method thereof include the following steps:
[0058] S1. Weigh a certain amount of sodium nitrate, manganese sulfate, nickel nitrate, yttrium nitrate, and ferrous chloride according to the stoichiometric ratio and disperse them in deionized water. Then transfer the above system to a ball mill, adjust the speed to 600 r / min, and ball mill for 10 h to obtain a mixture slurry;
[0059] S2, filtering the obtained slurry, washing it with an alkaline detergent, and drying it in a blast drying oven at a temperature of 100° C. for 12 h to obtain a precursor powder;
[0060] S3, the precursor powder was heated to 800℃ in air atmosphere at a heating rate of 5℃ / min and sintered for 16h to obtain YFeO3 / Na[Ni 0.33 Mn 0.28 Fe 0.33 Y 0.05 ]O2 electrode material.
[0061] The surface perovskite-controlled dual-phase sodium-electrode layered cathode material obtained in this embodiment is subjected to electrochemical testing, which specifically comprises the following steps:
[0062] The positive electrode material is mixed with a conductive additive (Super P) and a binder (polyvinylidene fluoride) in a mass ratio of 8:1:1. After sufficient grinding, an appropriate amount of solvent (N-methylpyrrolidone) is added to form a uniform black slurry. The positive electrode sheet is prepared through coating, drying and other process flows. The metal sodium sheet is used as the negative electrode, and a mixed solution of 1 mol / L NaPF6 and EC (ethylene carbonate) / DEC (diethyl carbonate) in a volume ratio of 1:1 is used as the electrolyte. A glass fiber separator is used to assemble the button battery in a glove box filled with argon gas with a water oxygen value below 0.1 ppm.
[0063] Charge and discharge test: The voltage range of button cell charge and discharge is 2.0-4.0V. Before the cycle test, it is activated at a smaller rate of 0.2C, and then cycled at a rate of 1C within the same voltage range to test its performance.
[0064] Example 4
[0065] In this embodiment, a surface perovskite-controlled dual-phase sodium-electrode layered cathode material and a preparation method thereof include the following steps:
[0066] S1. Weigh a certain amount of sodium bicarbonate, manganese acetate, nickel hydroxide, cerium oxide, and ferrous sulfate according to the stoichiometric ratio, add them into a solvent consisting of deionized water and anhydrous ethanol in a volume ratio of 1:1 and disperse them. Then transfer the above system to a ball mill, adjust the speed to 800 r / min, and ball mill for 11 h to obtain a mixture slurry;
[0067] S2, filtering the obtained slurry, washing it with an alkaline detergent, and drying it in a blast drying oven at a temperature of 90° C. for 12 h to obtain a precursor powder;
[0068] S3, the precursor powder was heated to 950℃ in air atmosphere at a heating rate of 4℃ / min and sintered for 16h to obtain CeFeO3 / Na[Ni 0.33 Mn 0.28 Fe 0.33 Ce 0.05 ]O2 electrode material.
[0069] The surface perovskite-controlled dual-phase sodium-electrode layered cathode material obtained in this embodiment is subjected to electrochemical testing, which specifically comprises the following steps:
[0070] The positive electrode material is mixed with a conductive additive (Super P) and a binder (polyvinylidene fluoride) in a mass ratio of 8:1:1. After sufficient grinding, an appropriate amount of solvent (N-methylpyrrolidone) is added to form a uniform black slurry. The positive electrode sheet is prepared through coating, drying and other process flows. The metal sodium sheet is used as the negative electrode, and a mixed solution of 1 mol / L NaPF6 and EC (ethylene carbonate) / DEC (diethyl carbonate) in a volume ratio of 1:1 is used as the electrolyte. A glass fiber separator is used to assemble the button battery in a glove box filled with argon gas with a water oxygen value below 0.1 ppm.
[0071] Charge and discharge test: The voltage range of button cell charge and discharge is 2.0-4.0V. Before the cycle test, it is activated at a smaller rate of 0.2C, and then cycled at a rate of 1C within the same voltage range to test its performance.
[0072] Comparative Example
[0073] This comparative example prepares a sodium ion battery positive electrode material, and the specific process is as follows:
[0074] S1. Weigh a certain amount of sodium carbonate, manganese dioxide, nickel oxide, and ferrous oxide according to a stoichiometric ratio, add them into a solvent consisting of deionized water and anhydrous ethanol, and disperse them. Then transfer the above system to a ball mill, adjust the speed to 500 r / min, and ball mill for 12 h to obtain a mixture slurry;
[0075] S2, filtering the obtained slurry, washing it with an alkaline detergent, and placing it in a blast drying oven for drying at a temperature of 80° C. for 8 h to obtain a precursor powder;
[0076] S3, the precursor powder was heated to 900℃ in air atmosphere at a heating rate of 5℃ / min and sintered for 20h to obtain Na[Ni 0.33 Mn 0.33 Fe 0.33 ]O2 electrode material.
[0077] The sodium ion battery positive electrode material obtained in this comparative example is subjected to electrochemical testing, specifically comprising the following steps:
[0078] The positive electrode material is mixed with a conductive additive (SuperP) and a binder (polyvinylidene fluoride) in a mass ratio of 8:1:1. After sufficient grinding, an appropriate amount of solvent (N-methylpyrrolidone) is added to form a uniform black slurry. The positive electrode sheet is prepared through coating, drying and other process flows. The metal sodium sheet is used as the negative electrode, and a mixed solution of 1 mol / L NaPF6 and EC (ethylene carbonate) / DEC (diethyl carbonate) with a volume ratio of 1:1 is used as the electrolyte. A glass fiber separator is used to assemble the button battery in a glove box filled with argon gas with a water oxygen value below 0.1 ppm.
[0079] Charge and discharge test: The voltage range of button cell charge and discharge is 2.0-4.0V. Before the cycle test, it is activated at a smaller rate of 0.2C, and then cycled at a rate of 1C within the same voltage range to test its performance.
[0080] like Figure 1 The SEM image of Example 1 is shown. It can be seen from the image that the material has a smooth morphology and sharp corners and edges.
[0081] like Figure 2 The first charge and discharge curves of the materials obtained in Example 1 and the comparative example at a 1C rate are shown, wherein the first charge and discharge capacity of the material in Example 1 at a 1C rate is 112.88 mAh / g.
[0082] like Figure 3 The first charge and discharge curves of the materials obtained in Example 2 and the comparative example at a 1C rate are shown, wherein the first charge and discharge capacity of the material in Example 2 at a 1C rate is 109.13 mAh / g.
[0083] like Figure 4 The first charge and discharge curves of the materials obtained in Example 3 and the comparative example at a 1C rate are shown, wherein the first charge and discharge capacity of the material in Example 3 at a 1C rate is 115.59 mAh / g.
[0084] like Figure 5 The first charge and discharge curves of the materials obtained in Example 4 and the comparative example at a 1C rate are shown, wherein the first charge and discharge capacity of the material in Example 4 at a 1C rate is 110.76 mAh / g.
[0085] like Figure 6 Shown is the cycle performance diagram of the embodiment and comparative example materials at a 1C rate, wherein the capacity retention rates of embodiments 1, 2, 3, 4 and the comparative example after 100 cycles at a 1C rate are 79.63%, 86.59%, 82.47%, 80.21% and 76.54%, respectively. Compared with the comparative example, the capacity and cycle stability of all the embodiments are improved to varying degrees.
[0086] The above description is not intended to limit the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by a person skilled in the art within the essential scope of the present invention shall also fall within the protection scope of the present invention.
Claims
1. A surface perovskite-controlled dual-phase sodium-electrode layered cathode material, characterized in that: It is a layered oxide with a surface perovskite-controlled O3 / P3 dual-phase structure and has the following general formula A a B b O 3+u / Na c [Ni d Mn e B y-b A x-a ]O 2+f , where the general formula of perovskite is A a B b O 3+u The double symbiotic phase structure is an O3 / P3 symbiotic phase, and the general structural formula is Na c [Ni d Mn e B y-b A x-a ]O 2+f , A is one of Ce, Y, La, and Gd, and B is one or more of transition metals Fe, Ti, Cr, and Mg; The a, b, c, d, e, and f respectively correspond to the molar percentages of the elements; x and y respectively correspond to the addition amounts of element A and element B; the relationship between them satisfies d+e+y-b+xa=1, (a+b) / (3+u)=1 / 3; The a, b, c, d, e, and f respectively correspond to the molar percentages of the elements, 0.8≤a≤1, 0≤b≤0.9, 0.78≤c≤0.89, 0≤e≤0.5, 0 <y-b≤0.33,0<x-a≤0.05,-0.03≤f≤0.03。 2. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 1, characterized in that: The following steps are involved: S1: according to the stoichiometric ratio of each element in the sodium ion battery positive electrode material to be prepared, a sodium source, a manganese source, a nickel source, a rare earth metal compound and a transition metal compound are weighed and dispersed in a solvent, and the mixed system is ball-milled to obtain a slurry; S2: filtering, washing, and drying the slurry to obtain a precursor; S3: The precursor is placed in air or oxygen atmosphere for high-temperature calcination. After the reaction is completed, it is naturally cooled to room temperature to obtain a surface perovskite-controlled dual-phase sodium-ion battery layered positive electrode material.
3. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 2, characterized in that: In step S1, the selected sodium source is a mixture of one or more of sodium sulfate, sodium carbonate, sodium bicarbonate, sodium nitrate, sodium chloride, and sodium acetate in any ratio; In step S1, the selected manganese source is a mixture of one or more of manganese trioxide, manganese dioxide, manganese tetraoxide, manganese carbonate, manganese nitrate, manganese sulfate, manganese chloride, and manganese acetate in any ratio; In step S1, the selected nickel source is one or a mixture of any ratio of nickel oxide, nickel sulfate, nickel chloride, nickel hydroxide, nickel nitrate, and nickel acetate; In step S1, the selected rare earth metal compound is one or a mixture of any ratio of lanthanum oxide, lanthanum nitrate, cerium oxide, cerium nitrate, yttrium oxide, yttrium nitrate, gadolinium oxide, and gadolinium nitrate; In step S1, the transition metal compound selected is a mixture of any ratio of one or more of ferric oxide, ferrous oxide, ferrous chloride, ferrous sulfate, ferrous carbonate, ferrous oxalate, ferrous nitrate, titanium dioxide, titanium tetrachloride, and magnesium chloride.
4. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 2, characterized in that: In the step S1, the solvent is a mixed solvent of deionized water and anhydrous ethanol, and the mixed volume ratio is 1:0-1.
5. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 2, characterized in that: In the step S1, the rotation speed of the ball mill is 500-800 r / min, and the ball milling time is 8-12 h.
6. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 2, characterized in that: In step S2, the washing liquid is an alkaline washing liquid.
7. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 2, characterized in that: In step S2, the drying method is spray drying, blast drying or vacuum drying.
8. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 2, characterized in that: In step S2, the drying temperature is 80-100° C., and the drying time is 8-12 hours.
9. The method for preparing a surface perovskite-controlled dual-phase sodium ion battery layered positive electrode material according to claim 2, characterized in that: In the step S3, the precursor is calcined in an air atmosphere, with a heating rate of 3-5°C / min, a calcination temperature of 700-950°C, a holding time of 10-24h, and a final sample is obtained when the temperature drops to room temperature.