Preparation method of supported heteropoly acid modified proton exchange membrane
By embedding heteropoly acid into the porous SiO2 skeleton, the problem of water loss and modifier loss of the proton exchange membrane at high temperatures is solved, the proton conductivity and water retention performance of the membrane are improved, the membrane life is extended, and the preparation process is simplified. Suitable for industrial production.
Patent Information
- Application Number
- CN202411230177.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing proton exchange membranes lose water at high temperatures, leading to performance attenuation. Modifiers such as phosphotungstic acid are easily lost. The introduction of metal skeleton preparation processes is harsh, and non-adaptive substances may be introduced, affecting the membrane life.
The preparation method of proton exchange membrane modified by porous SiO2 loaded heteropolyacid is adopted. By embedding the heteropoly acid into the SiO2 skeleton, the high moisture absorption and chemical force of SiO2 are used to fix the heteropoly acid, reduce its loss, and use perfluorinated Sulfonic acid resin is used as raw material to prepare a casting liquid to form a loaded proton exchange membrane.
It effectively reduces the loss of heteropoly acids, improves the proton conductivity and water retention performance of the membrane, and extends the service life of the membrane. The process is simple, the operation is cheap, and it is suitable for industrial production.
Smart Images

Figure CN118782846A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fuel cells, and in particular to a method for preparing a proton exchange membrane modified by a supported heteropoly acid. Background Art
[0002] Proton exchange membrane fuel cell (PEMFC) is one of the most promising fuel cells today due to its commercial feasibility. As one of its core components, the proton exchange membrane plays an important role in conducting hydrogen ions and blocking the anode and cathode plates. Common proton exchange membranes are made of perfluorosulfonic acid resin, with polytetrafluoroethylene as the skeleton, and the side-chain sulfonic acid groups can conduct protons. The price of proton exchange membranes is expensive, and extending the service life is the development direction.
[0003] One of the main reasons for the attenuation of proton exchange membrane performance is the evaporation of water at high temperature, the decrease in environmental humidity, the loss of water in the proton membrane, and the reduction of proton conductivity. Improving the water retention rate of the membrane is a major direction of modification. Since phosphotungstic acid and the like are hygroscopic, the hydrophilicity of the membrane can be improved, and the acidic properties of phosphotungstic acid and the proton membrane sulfonic acid system are highly compatible, and the preparation of a multifunctional system modifier can significantly improve the performance of the membrane. However, in actual production, phosphotungstic acid is highly water-soluble, and it is easy to lose and penetrate other parts during long-term work, corroding equipment. In response to the above problems, patent CN116742082A reported the use of sulfonated polyetheretherketone as a base membrane, and amino dopamine wrapped magnetic nanoparticles (such as Fe3O4) loaded with phosphotungstic acid, which effectively improved the loss problem of phosphotungstic acid. However, the patent introduces iron elements into the membrane system, and there is a risk of separating free iron ions in an acidic environment, and free iron ions will affect the life of the membrane. In addition, patent CN115411324A reports a method for preparing a composite proton exchange membrane of phosphotungstic acid chitosan with a conductive metal skeleton, wherein the metal skeleton material is used to reduce the loss of phosphotungstic acid. However, the preparation of the metal skeleton material requires the use of a hydrothermal method, and the conditions of high temperature and high pressure are very harsh.
[0004] In summary, the modified additives can improve the water retention capacity of the membrane while avoiding potential hidden dangers as much as possible. Ideally, the modified membrane is prepared with a non-critical operating process and the introduction of substances that have no positive feedback to the membrane system is reduced. Summary of the invention
[0005] The main technical problem solved by the present invention is to provide a method for preparing a proton exchange membrane modified by a supported heteropolyacid, thereby reducing the introduction of non-compatible substances into the proton membrane system, avoiding the outflow of modified substances, improving the proton conductivity of the membrane, improving the problem caused by membrane water loss in a high-temperature working environment, and increasing the life of the membrane.
[0006] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a method for preparing a loaded heteropolyacid modified proton exchange membrane, comprising the following steps: S1. mixing an organic solvent, tetraethyl orthosilicate, a surfactant and a heteropolyacid, then adding dilute hydrochloric acid to control the pH to be strongly acidic, and stirring evenly to form a transparent sol; S2. dropping the above transparent sol into a template to fully immerse the sol into the template, washing and drying the template after absorbing the sol, and calcining the dried product at high temperature to obtain a porous SiO2 loaded heteropolyacid modifier; S3. using a perfluorosulfonic acid resin solution as a raw material and drying it, then adding an organic solvent to re-dissolve it to obtain a casting liquid, adding the porous SiO2 loaded heteropolyacid modifier to the casting liquid, mixing, heating, and then cooling to room temperature, and using the casting liquid to prepare a loaded heteropolyacid modified proton exchange membrane.
[0007] In a preferred embodiment of the present invention, the mass ratio of the heteropoly acid, the surfactant and tetraethyl orthosilicate in step S1 is 1:5~1:30~5.
[0008] In a preferred embodiment of the present invention, the mass ratio of the organic solvent to tetraethyl orthosilicate in step S1 is 1:1-1:3.
[0009] In a preferred embodiment of the present invention, the mass ratio of the template to the transparent sol in step S2 is 1:10-1:30.
[0010] In a preferred embodiment of the present invention, the weight fraction (wt) of the heteropolyacid loaded in the porous SiO2 loaded heteropolyacid modifier in step S2 is 10% to 40%.
[0011] In a preferred embodiment of the present invention, the mass fraction wt of the perfluorosulfonic acid resin in the casting solution of step S3 is 5% to 50%.
[0012] In a preferred embodiment of the present invention, in step S3, the mass fraction wt of the porous SiO2 loaded heteropolyacid modifier in the perfluorosulfonic acid resin is 0.1% to 5%.
[0013] In a preferred embodiment of the present invention, the heteropoly acid is silicotungstic acid, phosphotungstic acid or phosphomolybdic tungstic acid.
[0014] In a preferred embodiment of the present invention, the organic solvent in step S1 is ethanol, the organic solvent in step S1 is n-propanol, the template is PS colloidal crystal, and the surfactant is polyethylene oxide-polypropylene oxide-polyethylene oxide or polyoxyethylene polyoxypropylene ether.
[0015] In a preferred embodiment of the present invention, the pore size of the porous silicon oxide in the porous SiO2 loaded heteropolyacid modifier is in the range of 100-200 nm.
[0016] The beneficial effects of the present invention are as follows: the preparation method of the proton exchange membrane modified by the supported heteropoly acid of the present invention reduces the introduction of non-compatible substances into the proton membrane system, uses SiO2 with a porous structure as a carrier, embeds the heteropoly acid into the silicon skeleton, effectively reduces the loss of the heteropoly acid, and improves the proton conductivity of the membrane. The water retention capacity of the proton membrane is improved by using SiO2 and heteropoly acid with high hygroscopicity, improves the problem caused by membrane water loss in a high-temperature working environment, and increases the life of the membrane.
[0017] The invention discloses a method for preparing a proton exchange membrane modified by a supported heteropoly acid. During the synthesis process, ethanol volatilizes and ethyl orthosilicate undergoes hydrolysis and polycondensation. The heteropoly acid is embedded in the silicon skeleton and has a strong effect on silicon oxide. The prepared silicon-supported heteropoly acid is not easily lost in an aqueous solution environment.
[0018] The method for preparing a proton exchange membrane modified with a supported heteropolyacid of the present invention has a porous structure and the silica carrier will not agglomerate, and the high pore volume and large specific surface area will not affect the conduction of protons. The silica system itself can improve the water retention capacity of the membrane, and the dual-functional system modifier is often reported to show a more excellent effect than the single-functional system modifier. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which: Figure 1 is a SEM image of the porous SiO2 loaded with phosphotungstic acid modifier of the present invention; Figure 2 It is the infrared characterization diagram of phosphotungstic acid, silicon oxide and porous SiO2 loaded phosphotungstic acid modifier; Figure 3 This is the infrared characterization diagram of porous SiO2 loaded with phosphotungstic acid modifier after different immersion time in aqueous solution; Figure 4 It is a comparison table of conductivity and water retention performance of the embodiments and comparative examples. DETAILED DESCRIPTION
[0020] The technical scheme in the embodiment of the present invention will be described clearly and completely below. The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification, so that people familiar with this technology can understand and read them, and are not used to limit the limiting conditions that the present invention can implement, so they have no substantial technical significance. Any modification of the structure, change of the proportional relationship, or adjustment of the size should still fall within the scope that the technical content disclosed by the present invention can cover without affecting the effects that the present invention can produce and the purposes that can be achieved. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and so on quoted in this specification are only for the convenience of narration, and are not used to limit the scope that can be implemented. The change or adjustment of the relative relationship should also be regarded as the scope that the present invention can implement without substantially changing the technical content.
[0021] Example 1, take PS (polystyrene) colloidal crystal as a template. Weigh 5g ethanol, 2g P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide) and stir and dissolve in a water bath at 50°C, add 1.2g hydrochloric acid and distilled water to adjust the pH to about 1. Add 30g TEOS (tetraethyl orthosilicate) and 1g phosphotungstic acid (HPW) and stir vigorously to form a solution. Take PS colloidal crystal and spread it on the Buchner funnel, slowly add the above solution until the template is soaked, the mass ratio of the template to the transparent sol is 1:2, vacuum filter 1-2, and then dry at 60°C for 2h, and repeat the above steps once. Dry at 100°C for 12h, and finally calcine at 400°C for 10h, with a heating rate of 5°C / min, to obtain SiO2-HPW modifier (porous SiO2 loaded heteropoly acid modifier), the mass fraction wt of HPW is 20%. S3. First, evaporate the commercially available Nafion solution in an oven at 60°C, cut it into pieces, weigh 10g, dissolve it in 52ml of n-propanol solvent to re-form Nafion solution, in which the mass fraction of perfluorosulfonic acid resin is 20% by weight. Add 0.55g of SiO2-HPW modifier to the Nafion solution, and then place it in a water bath at 40°C for 12 hours to obtain a casting solution, in which the mass fraction of phosphotungstic acid in perfluorosulfonic acid resin is 1% by weight.
[0022] Lay the PET backing on the scraper coater, adjust the scraper spacing, set the equipment temperature to 60℃, turn on the vacuum pump (vacuum degree <-0.08mpa), and when the temperature reaches the target, set the scraper speed to 5mm / s, evenly apply the casting liquid on the PET backing, and start the scraper to make the film. When the film is dry, remove it and place it in a drying oven at 100~120℃ for 12h.
[0023] Example 2, take PS (polystyrene) colloidal crystal as a template. Weigh 1g ethanol, 1g P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide) and stir and dissolve in a water bath at 50°C, add 1.2g hydrochloric acid and distilled water to adjust the pH to about 1. Add 5g TEOS (tetraethyl orthosilicate) and 1g phosphotungstic acid (HPW) and stir vigorously to form a solution. Take PS colloidal crystal and spread it on the Buchner funnel, slowly add the above solution until the template is soaked, and the mass ratio of the template to the transparent sol is 1:5. After vacuum filtration for 1-2, dry at 60°C for 2h, and repeat the above steps once. Dry at 100°C for 12h, and finally calcine at 400°C for 10h, with a heating rate of 5°C / min, to obtain SiO2-HPW modifier, and the mass fraction wt of HPW is 10%. S3, first evaporate the commercially available Nafion solution in an oven at 60°C, cut it into pieces, weigh 10g, dissolve it in 70ml of n-propanol solvent to re-form Nafion solution, in which the mass fraction of perfluorosulfonic acid resin is 15% by weight. Add 0.12g of SiO2-HPW modifier to the Nafion solution, then place it in a water bath at 40°C for 12 hours to obtain a casting solution, in which the mass fraction of phosphotungstic acid in perfluorosulfonic acid resin is 0.1% by weight.
[0024] Lay the PET backing on the scraper coater, adjust the scraper spacing, set the equipment temperature to 60℃, turn on the vacuum pump (vacuum degree <-0.08mpa), and when the temperature reaches the target, set the scraper speed to 5mm / s, evenly apply the casting liquid on the PET backing, and start the scraper to make the film. When the film is dry, remove it and place it in a drying oven at 100~120℃ for 12h.
[0025] Example 3, take PS (polystyrene) colloidal crystal as a template. Weigh 40g ethanol, 5g P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide) and stir and dissolve in a water bath at 50°C, add 1.7g hydrochloric acid and distilled water to adjust the pH to about 1. Add 20g TEOS (tetraethyl orthosilicate) and 3.84g phosphotungstic acid and stir vigorously to form a solution. Take PS colloidal crystal and spread it on the Buchner funnel, slowly add the above solution until the template is soaked, and the mass ratio of the template to the transparent sol is 1:1. After vacuum filtration for 1-2, dry at 60°C for 2h, and repeat the above steps once. Dry at 100°C for 12h, and finally calcine at 400°C for 10h, with a heating rate of 5°C / min, to obtain SiO2-HPW modifier, the mass fraction wt of HPW is 40%. S3, first evaporate the commercially available Nafion solution in an oven at 60°C, cut it into pieces, weigh 12g, dissolve it in 45ml of n-propanol solvent to re-form Nafion solution, in which the mass fraction of perfluorosulfonic acid resin is 25% by weight. Add 1.65g of SiO2-HPW modifier to the Nafion solution, then place it in a water bath at 40°C for 12 hours to obtain a casting solution, in which the mass fraction of phosphotungstic acid in perfluorosulfonic acid resin is 5% by weight.
[0026] Lay the PET backing on the scraper coater, adjust the scraper spacing, set the equipment temperature to 60℃, turn on the vacuum pump (vacuum degree <-0.08mpa), and when the temperature reaches the target, set the scraper speed to 5mm / s, evenly apply the casting liquid on the PET backing, and start the scraper to make the film. When the film is dry, remove it and place it in a drying oven at 100~120℃ for 12h.
[0027] Example 4, weigh 30g ethanol, 5g F127 (polyoxyethylene polyoxypropylene ether), mix, add distilled water and 1.3g hydrochloric acid to adjust the pH to close to 1. Add 30g TEOS (tetraethyl orthosilicate) and 2.5g phosphomolybdic tungstic acid (PMTA) and stir vigorously to form a solution. Take PS colloidal crystals and spread them all over the Buchner funnel, and slowly drip the above solution until the template is soaked. After vacuum filtration, dry at 60°C for 2h. After repeating the above steps once, dry at 100°C for 12h. Finally, calcined at 400°C for 10h, the heating rate was 5°C / min to prepare SiO2-PM modifier, and the phosphomolybdic tungstic acid loading was 20%. Take 100g of the commercially available Nafion solution reconfigured with n-propanol. Add SiO2-PM modifier to the newly prepared Nafion solution, and then water bath at 40°C for 12 hours to obtain a casting solution, and the final phosphomolybdic tungstic acid in the casting solution is 1% by weight.
[0028] Lay the PET backing on the scraper coater, adjust the scraper spacing, set the equipment temperature to 60℃, turn on the vacuum pump (vacuum degree <-0.08mpa), and when the temperature reaches the target, set the scraper speed to 5mm / s, evenly apply the casting liquid on the PET backing, start the scraper to make the film, and when the film is dry, remove it and place it in a drying oven. Dry at 100~120℃ for 12 hours.
[0029] Comparative Example: The difference between the comparative example and Example 1 is that no modifier is added, that is, the Nafion solution is reconfigured with n-propanol, and the resin mass fraction is 20%. Then, the proton exchange membrane is prepared by direct coating method, and the solid conditions and process are the same as those in Example 1.
[0030] Performance test: Figure 1 As shown, SiO2-HPW was subjected to SEM test to characterize its porous structure; since the content of phosphotungstic acid in the proton membrane is low and there are many interferences in infrared detection, the infrared characterization effects of SiO2-HPW, SiO2, and HPW were taken; SiO2-HPW was soaked in an aqueous solution, and samples were taken after soaking for 0h, 24h, 72h, and 120h, respectively, and infrared tests were performed after drying; the conductivity of the proton exchange membranes in the embodiments and comparative examples was tested at different temperatures and humidities to characterize the mass transfer performance and water retention performance.
[0031] SEM test results: The porous SiO2 carrier structure can be seen from the scanning electron microscope image, with a pore size of about 200nm.
[0032] Infrared characterization results: Figure 2 , phosphotungstic acid spectrum at 700cm -1 Up to 1300cm -1 There are four characteristic absorption peaks at 890cm -1 and 985cm -1 The two characteristic peaks appearing at the corresponding positions of the SiO2-HPW spectrum also exist, and the absorption peaks are offset, but pure SiO2 has no corresponding characteristic peaks. This shows that phosphotungstic acid has been embedded in the silicon skeleton and there is a chemical reaction. The peak intensity is positively correlated with the content of phosphotungstic acid. The remaining characteristic peaks cannot characterize the interaction between phosphotungstic acid and silicon oxide due to overlap.
[0033] Results of phosphotungstic acid loss: SiO2-HPW was dried and tested for infrared after being immersed in aqueous solution for 0h, 24h, 72h, and 120h. After immersion for 120h, 890cm -1 and 985cm -1 Two obvious infrared characteristic peaks indicate the presence of phosphotungstic acid in SiO2-HPW. The SiO2 carrier has a strong fixation on phosphotungstic acid, and the phosphotungstic acid in the modifier is not easy to lose.
[0034] Conductivity and water retention results: Figure 4 As shown, after the conductivity test, it can be found that the conductivity of the proton membrane doped with SiO2-HPW is significantly improved compared with that without doping, and the conductivity under low humidity is significantly improved.
[0035] The strong proton conductivity of phosphotungstic acid significantly improves the mass transfer performance of the proton membrane, and the dual moisture absorption function of silicon dioxide enhances the water retention capacity of the membrane. This effectively improves the performance degradation of the membrane under low humidity, avoids the loss of water at high temperature and causes the membrane performance to deteriorate, and significantly enhances the life of the proton membrane.
[0036] Heteropolyacids such as phosphotungstic acid are highly water soluble and can easily dissolve in water and separate from the membrane. Using a porous silica skeleton as a carrier, phosphotungstic acid is embedded into the silicon skeleton, allowing phosphotungstic acid to produce chemical forces with silicon oxide, which can fix phosphotungstic acid in an aqueous solution environment, effectively avoiding the problem of easy loss of phosphotungstic acid and further improving the life of the proton exchange membrane. The fixation effect of silicon oxide on phosphotungstic acid is characterized by a variety of modern analytical techniques such as SEM and infrared. Figure 3 .
[0037] Using porous SiO2 as a carrier, phosphotungstic acid is embedded into the silicon skeleton, effectively reducing the loss of phosphotungstic acid and improving the proton conductivity of the membrane. Highly hygroscopic SiO2 and phosphotungstic acid are used to improve the water retention capacity of the proton membrane, improve the problem caused by membrane water loss in high-temperature working environments, and increase the life of the membrane. The entire preparation process is simple and reliable, with a wide range of raw materials and low prices, which is conducive to industrial production.
[0038] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a proton exchange membrane modified by a supported heteropoly acid, It is characterized in that The following steps are involved: S1. The organic solvent, surfactant, tetraethyl orthosilicate and heteropoly acid are mixed, and then dilute hydrochloric acid is added to control the pH to a strongly acidic state, and stirred to form a transparent sol; S2. Add the transparent sol dropwise to the template to fully immerse the sol into the template, wash and dry the template after adsorbing the sol, and calcine the dried product at high temperature to obtain porous SiO 2 Supported heteropolyacid modifier; S3. Using perfluorosulfonic acid resin solution as raw material and drying it, then adding organic solvent to dissolve it again to obtain casting solution, and forming porous SiO 2 The loaded heteropoly acid modifier is added into the casting solution, mixed, heated, and then cooled to room temperature, and the loaded heteropoly acid modified proton exchange membrane is prepared by using the casting solution.
2. The method for preparing a proton exchange membrane modified by a supported heteropolyacid according to claim 1, It is characterized in that In the step S1, the mass ratio of the heteropoly acid, the surfactant and tetraethyl orthosilicate is 1:5-1:30-5.
3. The method for preparing a proton exchange membrane modified by a supported heteropolyacid according to claim 2, It is characterized in that In the step S1, the mass ratio of the organic solvent to tetraethyl orthosilicate is 1:1 to 1:
3.
4. The method for preparing a proton exchange membrane modified by a supported heteropolyacid according to claim 1, It is characterized in that In step S2, the mass ratio of the template to the transparent sol is 1:10-1:
30.
5. The method for preparing a proton exchange membrane modified by a supported heteropolyacid according to claim 4, It is characterized in that In step S2, the heteropoly acid is deposited on the porous SiO 2 The loading mass fraction wt of the loaded heteropolyacid modifier is 10%~40%.
6. The method for preparing a proton exchange membrane modified by a supported heteropolyacid according to claim 1, It is characterized in that The mass fraction wt of the perfluorosulfonic acid resin in the casting solution of step S3 is 5% to 50%.
7. The method for preparing a supported heteropolyacid-modified proton exchange membrane according to claim 6, It is characterized in that In step S3, the porous SiO 2 The mass fraction of the loaded heteropolyacid modifier in the perfluorosulfonic acid resin is 0.1%~5%.
8. The method for preparing a proton exchange membrane modified by a supported heteropolyacid according to claim 1, It is characterized in that The heteropoly acid is silicotungstic acid, phosphotungstic acid or phosphomolybdic tungstic acid.
9. The method for preparing a proton exchange membrane modified by a supported heteropolyacid according to claim 1, It is characterized in that The organic solvent in step S1 is ethanol, the organic solvent in step S3 is n-propanol, the template is PS colloidal crystal, and the surfactant is polyethylene oxide-polypropylene oxide-polyethylene oxide or polyoxyethylene polyoxypropylene ether.
10. The method for preparing a proton exchange membrane modified by a supported heteropoly acid according to claim 1, It is characterized in that The porous SiO 2 The pore size of the porous silica in the loaded heteropolyacid modifier ranges from 100 to 200 nm.
Citation Information
Patent Citations
Preparation method of metal organic framework loaded phosphotungstic acid chitosan composite proton exchange membrane
CN115411324A
Preparation method of magnetic nanoparticle loaded phosphotungstic acid-sulfonated polyetheretherketone composite proton exchange membrane
CN116742082A
Inorganic proton exchange film for fuel cell and method for making same
CN101038971A
Proton exchange membrane for fuel cell applications
US20110217623A1
Cited By
Preparation method of hybrid expanded polytetrafluoroethylene membrane and composite proton exchange membrane
CN118994681A
Phosphotungstic acid modified perfluorosulfonic acid proton membrane as well as preparation method and application thereof
CN121203206A
Phosphotungstic acid modified perfluorosulfonic acid proton membrane, and preparation method and application thereof
CN121203206B