Preparation method of fuel cell and fuel cell
Through the process of combining multi-layer tape-casting and single-layer tape-casting, combined with hot isostatic pressing lamination, the problems of long anode casting time and poor stability in fuel cell preparation are solved, achieving efficient and stable fuel cell production and improving improved battery performance and batch-to-batch consistency.
Patent Information
- Application Number
- CN202411112115.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing fuel cell preparation process, the anode casting time is long, the production capacity is low, and cracking and electrode sheet curling are prone to occur, resulting in poor batch stability, high ohmic resistance, low power density, and short lifespan.
A multi-layer tape-casting process is used to prepare the anode green embryo, and a single-layer tape-casting and lamination process is combined to achieve a close combination of the electrolyte and the anode. Through mechanical mixing and hot isostatic pressing, the thickness of each layer is precisely controlled to reduce cracking. and warping, improving battery performance.
It improves the quality and stability of the fuel cell, reduces the ohmic resistance, increases the power density, simplifies the process steps, improves the work efficiency and performance consistency, and achieves large-scale production and batch stability.
Smart Images

Figure CN118782849A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present disclosure relate to the field of fuel cell technology, and in particular, to a method for preparing a fuel cell and a fuel cell. Background Art
[0002] Fuel cell technology represented by solid oxide fuel cells (SOFC) is an important technical support for future energy transformation. How to mass-produce SOFCs with high flatness, high mechanical strength and excellent performance in a simple and high yield rate is a major problem that needs to be solved in the process of industrialization.
[0003] In the related technology, the preparation process using the cast film method mainly includes anode casting, lamination, hot pressing, sintering, and finally screen printing the cathode. The anode casting is usually a single-layer casting and then lamination. This will consume a lot of time in the lamination process, with low production capacity. In the sintering process, it is very easy to find that the anode cracks, the electrode sheets are severely curled and difficult to smooth, and the batch stability is poor. In addition, the electrode sheets prepared by this process have a large ohmic resistance, low power density, short life, and poor battery performance. Summary of the invention
[0004] The purpose of the present disclosure is to provide a method for preparing a fuel cell and a fuel cell, thereby overcoming the problems of low fuel cell preparation efficiency and poor quality caused by the limitations and defects of the relevant technology at least to a certain extent.
[0005] According to one aspect of the present disclosure, a method for preparing a fuel cell is provided, comprising: mechanically mixing an anode raw material and an electrolyte raw material to obtain an anode slurry and an electrolyte slurry; performing multi-layer tape casting on the anode slurry to obtain a multi-layer green embryo, and drying and curing the multi-layer green embryo to obtain an anode green embryo; performing single-layer tape casting on the electrolyte slurry to obtain a single-layer green embryo, and obtaining an electrolyte green embryo after drying and curing; cutting the anode green embryo and the electrolyte green embryo, and stacking the cut anode green embryo and electrolyte green embryo to make a single cell green embryo; and sintering the single cell green embryo to prepare the fuel cell.
[0006] In an exemplary embodiment of the present disclosure, the anode slurry is subjected to multi-layer tape casting to obtain a multi-layer green embryo, and the multi-layer green embryo is dried and solidified to obtain the anode green embryo, comprising: performing multi-layer tape casting of the anode slurry on a tape casting machine to obtain a multi-layer green embryo, and drying and solidifying each layer of the green embryo to obtain the anode green embryo; wherein, after drying, the thickness of the first layer of the green embryo is 100-140 μm, the difference in thickness between the second layer of the green embryo and the first layer of the green embryo is 20-40 μm, the difference in thickness between each layer of the green embryo after the second layer and the next layer of the green embryo is 10-20 μm, the thickness of the last layer of the green embryo is 20-30 μm, and the total thickness of the anode green embryo is 370-660 μm.
[0007] In an exemplary embodiment of the present disclosure, the number of layers of the green embryo is 6 to 9, and the time interval for drying and curing between each layer of the green embryo is 20 to 40 minutes.
[0008] In an exemplary embodiment of the present disclosure, the rotation speed of the roller of the casting machine is 0.1-0.3 m / min, and the oven temperature of the casting machine is 45-65°C.
[0009] In an exemplary embodiment of the present disclosure, the electrolyte slurry is subjected to single-layer tape casting to obtain a single-layer green embryo, and the electrolyte green embryo is obtained after drying and solidification, comprising: single-layer tape casting of the electrolyte slurry by a tape casting machine to obtain a single-layer electrolyte green embryo after drying and solidification; wherein, during tape casting, the roller rotates at a speed of 0.05 to 0.2 m / min, the thickness of the single-layer electrolyte green embryo is 10 μm to 20 μm, and the drying time is 30 min to 60 min.
[0010] In an exemplary embodiment of the present disclosure, the anode green embryo and the electrolyte green embryo are cut, and the cut anode green embryo and electrolyte green embryo are stacked to form a single cell green embryo, comprising: cutting the anode green embryo and the electrolyte green embryo to the same size to obtain the cut anode green embryo and the electrolyte green embryo; and stacking the cut anode green embryo and the electrolyte green embryo by a stacking machine under hot isostatic pressing to form a single cell green embryo.
[0011] In an exemplary embodiment of the present disclosure, when the anode green embryo and the electrolyte green embryo are laminated by hot isostatic pressing, the pressure is 20-40 MPa, the temperature is 30-50° C., the holding time is 10-15 minutes, and the thickness of the single cell green embryo ranges from 380 to 665 μm.
[0012] In an exemplary embodiment of the present disclosure, during the sintering process, the sintering temperature is 1280°C to 1400°C, the holding time is 24 to 36 hours, the cooling method is furnace cooling, and the thickness of the fuel cell ranges from 300 to 525 μm.
[0013] In an exemplary embodiment of the present disclosure, the anode slurry includes at least one of nickel oxide, a pore former, a dispersant, a plasticizer, a binder and a ball milling aid, and the viscosity of the anode slurry is 0.5 to 1 KPa·S; the electrolyte raw material includes at least one of yttrium-stabilized zirconia, a dispersant and a ball milling aid, and the viscosity of the electrolyte slurry is 0.05 to 0.5 KPa·S.
[0014] According to one aspect of the present disclosure, a fuel cell is provided. The fuel cell is prepared according to any one of the above-mentioned methods for preparing a fuel cell.
[0015] In the technical solution provided in the embodiment of the present disclosure, on the one hand, the anode embryo is prepared by a multi-layer casting process, and the electrolyte embryo and the anode embryo are closely combined by a process combining multi-layer casting, single-layer casting and lamination, which solves the problem of solvent penetration in the traditional full-cell multi-layer casting causing the functional layers to penetrate each other. And the thickness of each layer of embryo can be accurately controlled to prepare a fuel cell without cracking and warping, reduce the ohmic resistance of the fuel cell, increase the power density, and increase the service life, improve the quality and stability of the fuel cell, and improve the battery performance. On the other hand, through the preparation process combining multi-layer casting, single-layer casting and lamination, the process steps are simplified, the work efficiency is improved, the production capacity is increased, and the reliability and performance consistency of the same batch of single cells are improved, the battery performance is improved, and the preparation time of the single cell can be greatly shortened, thereby reducing the production cost and realizing the large-scale production and batch stability of the anode-supported solid oxide fuel cell.
[0016] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0018] Figure 1 A flow chart schematically illustrates a method for preparing a fuel cell in an embodiment of the present disclosure.
[0019] Figure 2 Schematic diagram of the SEM image of the anode prepared by the full lamination method Figure 1 .
[0020] Figure 3Schematic diagram of the SEM image of the anode prepared by the full lamination method Figure 2 .
[0021] Figure 4 The EIS impedance spectrum of a single cell prepared by the full stacking method is schematically shown.
[0022] Figure 5 Schematic diagrams of an anode green embryo, a single cell green embryo and a single cell sheet after sintering obtained according to the preparation method of Example 1 are schematically shown; Figure a shows a schematic diagram of the anode green embryo, Figure b shows a schematic diagram of the single cell green embryo, and Figure c shows a schematic diagram of the single cell sheet after sintering.
[0023] Figure 6 The SEM image of the anode prepared according to the preparation method of Example 1 is schematically shown. Figure 1 .
[0024] Figure 7 The SEM image of the anode prepared according to the preparation method of Example 1 is schematically shown. Figure 2 .
[0025] Figure 8 The EIS impedance spectrum of a single cell prepared according to the preparation method of Example 1 is schematically shown.
[0026] Fig. 9 The stability test curve of the single battery prepared according to the preparation method of Example 1 is schematically shown.
[0027] Fig.10 The SEM image of the anode prepared according to Example 2 is schematically shown.
[0028] Fig.11 The EIS impedance spectrum of the single cell prepared according to Example 2 is schematically shown.
[0029] Fig.12 The SEM image of the anode prepared according to Example 3 is schematically shown.
[0030] Fig.13 The EIS impedance spectrum of the single cell prepared according to Example 3 is schematically shown.
[0031] Fig.14 The SEM image of the anode prepared according to Example 4 is schematically shown.
[0032] Fig.15 The EIS impedance spectrum of the single cell prepared according to Example 4 is schematically shown. DETAILED DESCRIPTION
[0033] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.
[0034] The terms "a", "an", "the" and "said" used in this specification are used to indicate the presence of one or more elements / components, etc.; the terms "including" and "having" are used to express an open-ended inclusion and mean that there may be additional elements / components, etc. in addition to the listed elements / components, etc.; the terms "first" and "second" etc. are used only as labels and are not intended to limit the quantity of their objects.
[0035] Solid oxide fuel cells (SOFCs) can directly convert the chemical energy of hydrogen or hydrocarbons (i.e., synthesis gas produced by propane, butane, methane or liquid hydrocarbons) into electrical energy through electrochemical reactions, thereby achieving efficient, green, and low-carbon utilization of energy. They have high energy conversion efficiency and excellent fuel flexibility. Therefore, fuel cell technology represented by solid oxide fuel cells is an important technical support for future energy transformation.
[0036] According to the different support forms and materials, solid oxide fuel cells SOFC can be divided into anode support, electrolyte support, cathode support and metal support. The anode support is composed of three parts: a porous anode layer, a dense electrolyte layer and a porous cathode layer. The anode has the dual functions of a support and an electrode. The electrolyte of the anode-supported SOFC is very thin, so the ohmic polarization loss is relatively small and the battery performance is better.
[0037] At present, the commonly used SOFC preparation processes are mainly the following: dry pressing, centrifugal deposition, spin coating, phase conversion, screen printing and tape casting. In the production and manufacturing of SOFC, the current preparation process using tape casting is mainly anode tape casting, lamination, hot pressing, sintering, and finally screen printing cathode. The anode tape casting is usually a single-layer tape casting and then lamination. This will consume a lot of time in the lamination process, with low production capacity, and it is very easy to find anode cracking, severe curling of electrode sheets that are difficult to smooth out, and poor batch stability during the sintering process. In addition, the electrode sheets prepared by this process have large ohmic resistance, low power density, short life, and poor overall battery performance.
[0038] In order to solve the above technical problems, the present disclosure provides a method for preparing a fuel cell in an embodiment for preparing a positive support solid oxide fuel cell, referring to Figure 1 As shown in , it mainly includes the following steps:
[0039] In step S110, the anode raw material and the electrolyte raw material are mechanically mixed to obtain an anode slurry and an electrolyte slurry;
[0040] In step S120, the anode slurry is subjected to multi-layer tape casting, and after drying and curing, an anode green body is obtained;
[0041] In step S130, the electrolyte slurry is subjected to single-layer tape casting, and after drying and solidification, an electrolyte green body is obtained;
[0042] In step S140, the anode green embryo and the electrolyte green embryo are cut, and the cut anode green embryo and electrolyte green embryo are stacked to form a single cell green embryo;
[0043] In step S150, the single cell green body is sintered to prepare the fuel cell.
[0044] Next, the method for preparing the fuel cell in the embodiment of the present disclosure is described in detail.
[0045] In step S110 , the anode raw material and the electrolyte raw material are mechanically mixed to obtain anode slurry and electrolyte slurry.
[0046] In the disclosed embodiment, the anode raw material comprises at least one of nickel oxide (NiO), a pore former, a dispersant, a plasticizer, a binder and a ball milling aid. The electrolyte raw material comprises at least one of yttrium-stabilized zirconia (YSZ), a dispersant and a ball milling aid. When mechanical mixing is performed, mechanical mixing can be performed in a ball mill according to the ball mill speed and the ball milling time. The ball mill speed can be 200 to 500 rpm, and the ball milling time of the ball milling process can be 8 to 10 hours. Based on this, the anode raw material and the electrolyte raw material can be mechanically mixed in a ball mill to obtain anode slurry and electrolyte slurry with viscosity and uniform mixing. Among them, the viscosity of the electrolyte slurry can be less than or equal to the viscosity of the anode slurry, for example, the viscosity of the anode slurry is 0.5 to 1 KPa·S, and the viscosity of the electrolyte slurry is 0.05 to 0.5 KPa·S.
[0047] In step S120, the anode slurry is subjected to multi-layer tape casting, and after drying and curing, an anode green body is obtained.
[0048] In the disclosed embodiment, the anode slurry can be vacuum degassed, and the degassed anode slurry can be subjected to anode multi-layer casting. Casting refers to the process of scraping the slurry on the substrate to form a slurry film of a certain thickness through a scraper, and obtaining a large area of flat embryonic membrane after drying.
[0049] In some embodiments, the anode slurry can be subjected to multi-layer casting of the anode based on a casting machine to obtain a multi-layer green embryo. Exemplarily, the first layer can be cast first, the second layer can be cast on the basis of the first layer, and the third layer can be cast on the basis of the second layer, until the last layer is cast, so as to complete the multi-layer casting of the anode. Wherein each casting can obtain a layer of green embryo. The number of cast layers can be used to indicate the number of castings, and the number of cast layers can be determined according to the thickness range of the fuel cell after sintering, and the thickness range can be used to indicate the thickness range that the fuel cell after sintering can be formed. Exemplarily, the number of cast layers can be 6 to 9 layers, that is, the number of casts can be 6 to 9 times, so 6 to 9 layers of green embryos can be formed. There is a thickness difference between each layer of green embryos, and the thickness of the green embryos decreases with the increase of the number of cast layers, the thickness of the first layer of green embryos is the largest, and the thickness of the last layer of green embryos is the smallest. Specifically, after drying, the thickness of the first layer of green embryo is 100-140 μm, the thickness difference between the second layer of green embryo and the first layer of green embryo is 20-40 μm, the thickness difference between each layer of green embryo after the second layer and the next layer of green embryo is 10-20 μm, the thickness of the last layer of green embryo is 20-30 μm, and the total thickness range of the anode green embryo is 370-660 μm.
[0050] After obtaining a multi-layer green embryo based on multi-layer casting, each layer of the green embryo can be dried and cured to obtain an anode green embryo with uniform thickness and smooth surface, that is, an anode film. It should be noted that in the multi-layer casting process, the parameters of each casting are: the rotation speed of the roller of the casting machine is 0.1 to 0.3 m / min, the oven temperature of the casting machine is 45 to 65°C, and the drying and curing time interval between each layer of the green embryo is 20 to 40 minutes.
[0051] In step S130, the electrolyte slurry is subjected to single-layer tape casting to obtain a single-layer electrolyte green body, and the electrolyte green body is obtained after drying and solidification.
[0052] In the disclosed embodiment, the obtained electrolyte slurry is subjected to vacuum degassing, and at a certain temperature, the degassed electrolyte slurry is subjected to single-layer tape casting on a tape casting machine, with the number of casting layers being 1, to obtain a single-layer electrolyte green embryo, and after the single-layer electrolyte green embryo is dried and solidified, an electrolyte green embryo with uniform thickness and smooth surface, i.e., an electrolyte film, is obtained.
[0053] During the single-layer casting of the electrolyte slurry, the roller rotates at a speed of 0.05 to 0.2 m / min, the oven temperature of the casting machine is 40 to 55° C., the thickness of the single-layer electrolyte embryo after drying and curing is 10 to 20 μm, and the drying time is 30 to 60 min.
[0054] Next, continue to refer to Figure 1 As shown in FIG. 1 , in step S140 , the anode green embryo and the electrolyte green embryo are cut, and the cut anode green embryo and electrolyte green embryo are stacked to form a single cell green embryo.
[0055] In the disclosed embodiment, the obtained anode green embryo and electrolyte green embryo can be cut into the same size, and the specific size can be determined according to actual needs. The cut anode green embryo and the cut electrolyte green embryo are stacked with a stacking machine under hot isostatic pressing to make a single cell green embryo. Among them, the anode green embryo and the electrolyte green embryo can be stacked by hot isostatic pressing. When hot isostatic pressing is performed, the pressure is 20-40Mpa, the temperature during the stacking process is 30-50°C, the holding time is 10-15 minutes, and the thickness of the single cell green embryo after stacking is in the range of 380-665μm.
[0056] Continue to refer Figure 1 As shown in FIG. 1 , in step S150 , the single cell green body is sintered to prepare the fuel cell.
[0057] In the disclosed embodiment, the single cell embryo can be cut, and the cut single cell embryo can be sintered, and the single cell can be obtained after the sintered single cell is cooled, and the single cell is a fuel cell. Exemplarily, the single cell embryo can be cut into square cells and sintered in a muffle furnace. Further, the sintered single cell can be cooled to obtain a single cell. During the sintering process, the sintering crucible is an alumina crucible, the sintering temperature is 1280°C to 1400°C, and the insulation time is 24 to 36 hours. During the cooling process, the cooling method is furnace cooling. The thickness range of the sintered single cell is 300 to 525 μm, that is, the thickness range of the fuel cell is 300 to 525 μm.
[0058] In some embodiments, an anode-supported solid oxide fuel cell may be prepared based on a conventional full stacking method, and the specific process includes the following steps:
[0059] Step 1, slurry preparation: weigh the anode raw materials including nickel oxide (NiO), pore former, dispersant, plasticizer, binder and ball milling aid; weigh the electrolyte raw materials including yttrium-stabilized zirconia (YSZ), dispersant and ball milling aid, set the ball mill speed to 300 rpm, the ball milling time to 8 h, the viscosity of the anode slurry prepared after ball milling is 0.8 KPa·S, and the viscosity of the electrolyte slurry is 0.1 KPa·S.
[0060] Step 2, anode single-layer tape casting: a single-layer anode tape casting is performed on a tape casting machine, the roller rotates at a speed of 0.15 m / min, the oven temperature of the tape casting machine is set to 60° C., and the thickness of the single-layer green embryo after drying is 100 μm.
[0061] Step 3: Electrolyte monolayer casting: During casting, the roller rotates at a speed of 0.05 m / min, the oven temperature of the casting machine is set to 40° C., and the thickness of the single-layer electrolyte embryo after drying and curing is 20 μm.
[0062] Step 4, lamination: Lamination of single-layer anode green sheets, the number of laminations is 5, and then hot isostatic pressing is performed with electrolyte green sheets after 5 layers of anode lamination. The pressure used is 30Mpa, the temperature is 40°C, and the holding time is 10 minutes. After lamination, the thickness of the single cell green sheet is 480μm.
[0063] Step 5, sintering: sinter the stacked single cells, the sintering crucible is an alumina crucible, the sintering temperature is 1300°C, the holding time is 28 hours, the cooling method is furnace cooling, and the thickness of the sintered single cell is 400μm.
[0064] Figure 2 and Figure 3 The SEM image of the anode prepared by the full lamination method is schematically shown. Figure 2 and Figure 3It can be seen that there are obvious cracks or grooves on the anode side, indicating that the layers are not tightly fitted together, and there is a phenomenon of collapse between the layers after sintering. There are also obvious cracks between the anode and the electrolyte, indicating a loose bond.
[0065] Figure 3 The EIS impedance spectrum of a single cell prepared by the full stacking method is shown schematically. Figure 3 It can be seen that the ohmic resistance of the prepared single cell is 0.19Ωcm 2 The higher ohmic resistance indicates that the single cell prepared by the full stacking method further proves that the bonding between the electrolyte and the anode is not tight and the performance is poor.
[0066] In order to solve the technical problems existing in the full lamination method, the present disclosure provides a method for preparing a fuel cell including anode multilayer casting and electrolyte single layer casting. The preparation method of the fuel cell is described in detail below in conjunction with the embodiments.
[0067] Example 1
[0068] The preparation method of the anode supported solid oxide fuel cell mainly comprises the following steps:
[0069] Step 1, slurry preparation: weigh the anode raw materials, which include nickel oxide (NiO), pore former, dispersant, plasticizer, binder and ball milling aid; weigh the electrolyte raw materials including yttrium-stabilized zirconia (YSZ), dispersant and ball milling aid. Set the ball mill speed to 300 rpm and the ball milling time to 8 hours. The viscosity of the anode slurry prepared after ball milling is 0.8 KPa·S, and the viscosity of the electrolyte slurry is 0.1 KPa·S.
[0070] Step 2, anode multi-layer casting: The anode multi-layer casting is carried out on the casting machine, the roller rotates at a speed of 0.15 m / min, the oven temperature of the casting machine is set to 60°C, the first layer is cast first, the thickness of the first layer of green embryo after drying is 120 μm, the thickness of the second layer of green embryo is 100 μm, the thickness of the third layer of green embryo is 80 μm, the thickness of the fourth layer of green embryo is 60 μm, the thickness of the fifth layer of green embryo is 40 μm, and the thickness of the last layer of green embryo is 30 μm. The time interval between drying and curing of each layer of green embryo is 30 minutes, and the thickness of the final anode green embryo is 430 μm.
[0071] Step 3, electrolyte single layer casting: during casting, the roller rotates at a speed of 0.05 m / min, the oven temperature of the casting machine is set to 40°C, and the thickness of the single layer electrolyte embryo after drying and curing is 10 μm; the drying time is 30 min.
[0072] Step 4, lamination: The anode green embryo and the electrolyte green embryo are laminated by hot isostatic pressing. The pressure used in the lamination process is 30 MPa, the temperature is 40° C., and the pressure holding time is 10 minutes. The thickness of the single cell green embryo after lamination is 437 μm.
[0073] Step 5, sintering: sinter the stacked single cells, the sintering crucible is an alumina crucible, the sintering temperature is 1300°C, the holding time is 28 hours, the cooling method is furnace cooling, and the thickness of the sintered single cell sheet is 350μm.
[0074] Depend on Figure 5 It can be seen from the anode green embryo shown in Figure a, the single cell green embryo shown in Figure b, and the single cell sheet after sintering shown in Figure c that the co-cast anode green embryo is relatively uniform without grooves or cracks, the single cell green embryo sheet after superimposing the electrolyte is regular, and the single cell sheet after sintering is overall flat without obvious curling or warping.
[0075] refer to Figure 5 From the SEM image of the anode prepared in Example 1, it can be seen that the anode has no obvious cracks or places where the layers are not in contact with each other, and the anode has a uniform porous structure as a whole.
[0076] Figure 6 The EIS impedance spectrum and stability test curve of the single cell prepared according to Example 1 are schematically shown. From the EIS impedance spectrum, it can be seen that the ohmic resistance of the single cell is 0.035Ωcm 2 Therefore, the ohmic resistance of the single cell obtained by this preparation method is low, and is lower than the ohmic resistance of the single cell prepared by the full stacking method in the related art. The SEM image further shows that the electrolyte and the anode are tightly combined and have good matching. The single cell open circuit voltage test results show that within the test time range, the open circuit voltage remains stable, basically stable at around 1.1V, indicating that the single cell prepared by this method has good stability and can work for a long time.
[0077] In the embodiments of the present disclosure, a method for preparing an anode-supported solid oxide fuel cell is provided. The method is based on anode raw materials and electrolyte raw materials, and through process flows such as slurrying, anode multi-layer casting, electrolyte single-layer casting, lamination and sintering, the method can effectively improve the production capacity, flatness and stable performance of the SOFC anode electrode, solve the problems of time and energy consumption and high manufacturing cost in actual production, and prepare single cells with excellent performance and good batch stability.
[0078] Example 2
[0079] The preparation method of the anode supported solid oxide fuel cell mainly comprises the following steps:
[0080] Step 1, slurry preparation: weigh the anode raw material containing nickel oxide (NiO), pore former, dispersant, plasticizer, binder and ball milling aid; weigh the electrolyte raw material containing yttrium-stabilized zirconia (YSZ), dispersant and ball milling aid, set the ball mill speed to 200 rpm, the ball milling time to 10 h, the viscosity of the anode slurry prepared after ball milling is 0.5 KPa·S, and the viscosity of the electrolyte slurry is 0.05 KPa·S.
[0081] Step 2, anode multi-layer casting: The anode multi-layer casting is carried out on the casting machine, the roller rotates at a speed of 0.3 m / min, the oven temperature of the casting machine is set to 45°C, the first layer is cast first, and the thickness of the first layer of green embryo after drying is 100 μm, the thickness of the second layer of green embryo is 70 μm, the thickness of the third layer of green embryo is 60 μm, the thickness of the fourth layer of green embryo is 50 μm, the thickness of the fifth layer of green embryo is 40 μm, the thickness of the sixth layer of green embryo is 30 μm, and the thickness of the last layer of green embryo is 20 μm. The time interval between drying and curing of each layer of green embryo is 30 minutes, and the thickness of the anode green embryo finally obtained is 370 μm.
[0082] Step 3, electrolyte single layer casting: during casting, the roller rotates at a speed of 0.2 m / min, the oven temperature of the casting machine is set to 45°C, and the thickness of the single layer electrolyte embryo after drying and curing is 20 μm; the drying time is 60 min.
[0083] Step 4, lamination: The anode embryo and the electrolyte embryo are laminated by hot isostatic pressing. The pressure used in the lamination process is 20 MPa, the temperature is 30°C, and the pressure holding time is 10 minutes. After lamination, the thickness of the single cell embryo is 380 μm.
[0084] Step 5, sintering: sinter the laminated single cell embryos, the sintering crucible is an alumina crucible, the sintering temperature is 1280°C, the holding time is 24 hours, the cooling method is furnace cooling, and the thickness of the sintered single cell sheet is 300μm.
[0085] refer to Figure 7 The SEM image of the anode prepared according to Example 2 and the EIS impedance spectrum of the single cell are shown. From the SEM image, it can be seen that the anode has no obvious cracks or places where the layers are not attached to each other, and is tightly combined with the electrolyte without obvious cracks, and the whole evenly presents a porous structure. From the EIS impedance spectrum of the single cell, it can be seen that the ohmic resistance of the single cell is 0.09Ωcm 2 , indicating that the ohmic resistance of the single cell is low, thus proving that the electrolyte and the anode are tightly bonded and well matched.
[0086] Example 3
[0087] The preparation method of the anode-supported solid oxide fuel cell mainly comprises the following steps:
[0088] Step 1, slurry preparation: weigh the anode raw material containing nickel oxide (NiO), pore former, dispersant, plasticizer, binder and ball milling aid; weigh the electrolyte raw material containing yttrium-stabilized zirconia (YSZ), dispersant and ball milling aid, set the ball mill speed to 500 rpm / min, the ball milling time to 9 hours, the viscosity of the anode slurry prepared after ball milling is 1 KPa·S, and the viscosity of the electrolyte slurry is 0.5 KPa·S.
[0089] Step 2, anode multi-layer casting: The anode multi-layer casting is carried out on the casting machine, the roller rotates at a speed of 0.1 m / min, the oven temperature of the casting machine is set to 65°C, the first layer is cast first, the thickness of the first layer of green embryo after drying is 140μm, the thickness of the second layer of green embryo is 100μm, the thickness of the third layer of green embryo is 90μm, the thickness of the fourth layer of green embryo is 80μm, the thickness of the fifth layer of green embryo is 70μm, the thickness of the sixth layer of green embryo is 60, the thickness of the seventh layer of green embryo is 50μm, the thickness of the eighth layer of green embryo is 40μm, and the thickness of the last layer of green embryo is 30μm. The drying and curing time interval between layers is 40min, and the thickness of the anode green embryo finally obtained is 660μm.
[0090] Step 3, electrolyte single layer casting: during casting, the roller rotates at a speed of 0.1 m / min, the oven temperature of the casting machine is set to 55°C, and the thickness of the single layer electrolyte embryo after drying and curing is 18 μm; the drying time is 50 min.
[0091] Step 4, lamination: The anode green embryo and the electrolyte green embryo are laminated by hot isostatic pressing. The pressure used in the lamination process is 40 MPa, the temperature is 50° C., and the pressure holding time is 15 minutes. The thickness of the single cell green embryo after lamination is 665 μm.
[0092] Step 5, sintering: sinter the laminated single cell embryos, the sintering crucible is an alumina crucible, the sintering temperature is 1400°C, the holding time is 36 hours, the cooling method is furnace cooling, and the thickness of the sintered single cell sheet is 525μm.
[0093] Figure 8 The SEM image of the anode prepared in Example 3 and the EIS impedance spectrum of the single cell show that the anode has no obvious cracks or places where the layers do not fit together, and is tightly combined with the electrolyte without obvious cracks, and presents a uniform porous structure as a whole. The EIS impedance spectrum of the single cell shows that the ohmic resistance of the single cell is 0.12Ωcm 2 The ohmic resistance of the single cell is low and is smaller than the ohmic resistance of the single cell prepared by the full stacking method in the related art, which also proves that the electrolyte and the anode are tightly combined and have good matching.
[0094] Example 4
[0095] The preparation method of the anode-supported solid oxide fuel cell mainly comprises the following steps:
[0096] Step 1, slurry preparation: weigh the anode raw material, the anode raw material includes nickel oxide (NiO), pore former, dispersant, plasticizer, binder and ball milling aid; weigh the electrolyte raw material, the electrolyte raw material includes yttrium-stabilized zirconia (YSZ), dispersant and ball milling aid, set the ball mill speed to 400 rpm, the ball milling time to 8.5 h, the viscosity of the anode slurry prepared after ball milling is 0.85 KPa·S, and the viscosity of the electrolyte slurry is 0.4 KPa·S.
[0097] Step 2, anode multi-layer casting: The anode multi-layer casting is carried out on the casting machine, the roller rotates at a speed of 0.2 m / min, the oven temperature of the casting machine is set to 55°C, and the first layer is cast first. After drying, the thickness of the first layer of green embryo is 110 μm, the thickness of the second layer of green embryo is 90 μm, the thickness of the third layer of green embryo is 75 μm, the thickness of the fourth layer of green embryo is 60 μm, the thickness of the fifth layer of green embryo is 45 μm, and the thickness of the last layer of green embryo is 30 μm. The time interval between drying and curing of each layer of green embryo is 40 minutes, and the thickness of the final anode green embryo is 410 μm. Among them, the thickness of each layer of green embryo refers to the thickness of the green embryo after drying.
[0098] Step 3, electrolyte single layer casting: during casting, the roller rotates at a speed of 0.15 m / min, the oven temperature of the casting machine is set to 55°C, and the thickness of the single layer electrolyte embryo after drying and curing is 15 μm; the drying time is 40 min.
[0099] Step 4, lamination: The anode green embryo and the electrolyte green embryo are laminated by hot isostatic pressing. The pressure used in the lamination process is 35 MPa, the temperature is 50°C, and the pressure holding time is 15 minutes. After lamination, the thickness of the single cell green embryo is 520 μm.
[0100] Step 5, sintering: sinter the stacked single cells, the sintering crucible is an alumina crucible, the sintering temperature is 1350°C, the holding time is 28 hours, the cooling method is furnace cooling, and the thickness of the sintered single cell sheet is 340μm.
[0101] Fig. 9 The SEM image of the anode prepared in Example 4 and the EIS impedance spectrum of the single cell show that the anode has no obvious cracks or places where the layers do not fit together, and is tightly combined with the electrolyte without obvious cracks, and presents a uniform porous structure as a whole. The EIS impedance spectrum of the single cell shows that the ohmic resistance of the single cell is 0.09Ωcm 2, indicating that the ohmic resistance of the prepared single cell is low and is lower than the ohmic resistance of the single cell prepared by the full stacking method in the related art. At the same time, it proves that the combination between the electrolyte and the anode is very close and the matching is good.
[0102] In summary, in the disclosed embodiment, the anode green embryo is prepared by a multilayer casting process, and the ohmic resistance of the prepared single cell is much smaller than the ohmic resistance of the single cell obtained by the preparation method in the related art through the process of combining multilayer casting, single layer casting and lamination. Due to the low ohmic resistance, it is further proved that the electrolyte and the anode are closely combined, the performance is improved, and the problem of solvent penetration in the traditional full-cell multilayer casting causing the functional layers to penetrate each other is solved. The thickness of the single layer can be accurately controlled to achieve a non-cracking, non-warping anode-supported solid oxide fuel cell. And the preparation process of the single cell is optimized, the production capacity is improved, and the reliability and performance consistency of the single cells in the same batch are improved. The production process steps are simple, and the work efficiency is greatly improved compared with the single-layer lamination method; compared with the full-cell co-casting, the preparation process is greatly reduced and the battery performance is improved. Through fine process control, the preparation time of the single cell can be greatly shortened, thereby reducing the production cost and realizing the large-scale production and batch stability of the anode-supported solid oxide fuel cell.
[0103] In this exemplary embodiment, a device is also provided. The device may be a device having the fuel cell, such as a mobile phone, a tablet computer, a laptop computer, a smart bracelet, a smart watch, a smart helmet, smart glasses, a vehicle, a robot, and any type of industrial equipment, etc., as long as the fuel cell can be included, and this exemplary embodiment does not specifically limit this.
[0104] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.
[0105] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.
[0106] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.
Claims
1. A method for preparing a fuel cell, characterized in that: include: Mechanically mixing the anode raw material and the electrolyte raw material to obtain the anode slurry and the electrolyte slurry; Performing multi-layer tape casting on the anode slurry to obtain a multi-layer green embryo, and drying and curing the multi-layer green embryo to obtain an anode green embryo; The electrolyte slurry is subjected to single-layer tape casting to obtain a single-layer green embryo, and the electrolyte green embryo is obtained after drying and solidification; Cutting the anode green embryo and the electrolyte green embryo, and stacking the cut anode green embryo and electrolyte green embryo to make a single cell green embryo; The single cell green body is sintered to prepare the fuel cell.
2. The method for preparing a fuel cell according to claim 1, characterized in that: The anode slurry is subjected to multi-layer casting to obtain a multi-layer green embryo, and the multi-layer green embryo is dried and solidified to obtain the anode green embryo, comprising: Performing multi-layer tape casting of the anode slurry on a tape casting machine to obtain a multi-layer green body, and drying and curing each layer of the green body to obtain an anode green body; Among them, the thickness of the first layer of green embryo after drying is 100-140μm, the thickness difference between the second layer of green embryo and the first layer of green embryo is 20-40μm, the thickness difference between each layer of green embryo after the second layer and the next layer of green embryo is 10-20μm, the thickness of the last layer of green embryo is 20-30μm, and the total thickness of the anode green embryo is 370-660μm.
3. The method for preparing a fuel cell according to claim 1 or 2, characterized in that: The number of layers of the green embryo is 6 to 9, and the time interval for drying and curing between each layer of the green embryo is 20 to 40 minutes.
4. The method for preparing a fuel cell according to claim 2, characterized in that: The rotation speed of the roller of the casting machine is 0.1-0.3 m / min, and the oven temperature of the casting machine is 45-65°C.
5. The method for preparing a fuel cell according to claim 1, characterized in that: The electrolyte slurry is subjected to single-layer tape casting to obtain a single-layer green embryo, and the electrolyte green embryo is obtained after drying and solidification, comprising: Performing single-layer tape casting on the electrolyte slurry by a tape casting machine to obtain a single-layer electrolyte green body after drying and solidification; During the casting process, the roller rotates at a speed of 0.05 to 0.2 m / min, the thickness of the single-layer electrolyte green body is 10 μm to 20 μm, and the drying time is 30 min to 60 min.
6. The method for preparing a fuel cell according to claim 1, characterized in that: The step of cutting the anode green embryo and the electrolyte green embryo, and stacking the cut anode green embryo and the electrolyte green embryo to form a single cell green embryo comprises: Cutting the anode green embryo and the electrolyte green embryo into the same size to obtain cut anode green embryo and electrolyte green embryo; The cut anode green sheets and electrolyte green sheets are stacked by a stacking machine under hot isostatic pressing to form single cell green sheets.
7. The method for preparing a fuel cell according to claim 1, characterized in that: When the anode green embryo and the electrolyte green embryo are laminated by hot isostatic pressing, the pressure is 20-40 MPa, the temperature is 30-50° C., the pressure holding time is 10-15 minutes, and the thickness of the single cell green embryo ranges from 380 to 665 μm.
8. The method for preparing a fuel cell according to claim 1, characterized in that: In the sintering process, the sintering temperature is 1280° C. to 1400° C., the heat preservation time is 24 to 36 hours, the cooling method is furnace cooling, and the thickness of the fuel cell ranges from 300 to 525 μm.
9. The method for preparing a fuel cell according to claim 1, characterized in that: The anode slurry comprises at least one of nickel oxide, a pore former, a dispersant, a plasticizer, a binder and a ball milling aid, and the viscosity of the anode slurry is 0.5 to 1 KPa·S; The electrolyte raw material comprises at least one of yttrium-stabilized zirconia, a dispersant and a ball milling aid, and the viscosity of the electrolyte slurry is 0.05-0.5 KPa·S.
10. A fuel cell, characterized in that: The fuel cell is prepared according to the method for preparing a fuel cell according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method of half-cell solid oxide anode
CN119340407A