Zeolite membrane composite, method for producing zeolite membrane composite, and method for separating zeolite membrane composite
By forming a zeolite membrane with a varying Si/Al ratio on a porous support, the problem in the prior art that the zeolite membrane composite has both hydrothermal resistance and water permeability but is easy to peel off is solved, achieving efficient manufacturing and stable performance. Zeolite membrane composite.
Patent Information
- Application Number
- CN202380015161.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-16
- Publication Date
- 2024-10-15
AI Technical Summary
While existing zeolite membrane composites have high hydrothermal resistance and high water permeation flux, they are prone to membrane peeling and have low manufacturing process efficiency.
By forming a zeolite membrane on a porous support, the continuous change of the Si/Al ratio of the zeolite membrane at the interface portion and the surface portion is controlled, forming a structure in which the Si/Al ratio gradually increases from the interface portion toward the interior of the membrane, and from the interior of the membrane toward the interior of the membrane. The surface of the zeolite membrane gradually becomes smaller, and the membrane is efficiently manufactured by combining the hydrothermal synthesis method.
A zeolite membrane composite with high water permeation flux and hydrothermal resistance, suppressed membrane peeling, and improved membrane stability and manufacturing efficiency was achieved.
Smart Images

Figure CN118785960A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a zeolite membrane composite, a method for producing the zeolite membrane composite, and a separation method.
[0002] [References to related applications]
[0003] This application claims the benefit of priority of Japanese patent application JP2022-029614 filed on February 28, 2022, the entire disclosure of which is incorporated herein by reference. Background Art
[0004] Generally, it is known that a zeolite membrane with a relatively large Si / Al ratio has high hydrothermal resistance, and a zeolite membrane with a relatively small Si / Al ratio has high water permeation flux. Therefore, International Publication No. 2018 / 225787 (Document 1) discloses a separation membrane obtained by laminating a first zeolite membrane with a relatively large Si / Al ratio (high-silicon zeolite membrane) and a second zeolite membrane with a relatively small Si / Al ratio (low-silicon zeolite membrane) so as to have both high hydrothermal resistance and high water permeation flux.
[0005] It should be noted that Japanese Patent Gazette No. 6748104 (Document 2) discloses a crystalline pure silica film formed on the surface of a porous substrate. The pure silica film has a CHA-type crystal structure and is composed only of silicon and oxygen from the membrane surface to 2 μm. In the pure silica film of Document 2, the hydrophobicity is high, so it is believed that the water permeation flux is reduced. Japanese Patent Gazette No. 4759724 (Document 3) discloses a zeolite membrane manufactured on a porous substrate, wherein the Si / Al ratio thereof is continuously or stepwise inclined in the depth direction of the membrane. International Publication No. 2017 / 169591 (Document 4) discloses a method for manufacturing a porous support, etc. Japanese Patent Gazette No. 2004-83375 (Document 5) discloses a method for manufacturing a DDR type zeolite.
[0006] However, in the separation membrane of Document 1, the zeolite membrane with a relatively large Si / Al ratio (i.e., low polarity) contacts a porous support having polar hydroxyl groups on the surface, so the adhesion to the support is reduced, and the membrane is easily peeled off. In addition, in Document 1, after a first zeolite membrane is formed using a raw material solution, another raw material solution is used to form a second zeolite membrane, so the preparation of the separation membrane requires a long time. Summary of the invention
[0007] The present invention relates to a zeolite membrane composite, and an object thereof is to provide a zeolite membrane composite having high water permeation flux and hydrothermal resistance and suppressed membrane peeling, and another object thereof is to efficiently produce the zeolite membrane composite.
[0008] The invention of claim 1 is a zeolite membrane composite, comprising: a porous support, and a zeolite membrane disposed on the support. In the zeolite membrane, the Si / Al ratio increases in molar ratio from the interface with the support toward the inside of the membrane, and decreases from the inside of the membrane toward the surface on the opposite side of the support.
[0009] According to the present invention, a zeolite membrane composite having high water permeation flux and hydrothermal resistance and suppressed membrane peeling can be provided.
[0010] The invention of Scheme 2 is based on the zeolite membrane composite of Scheme 1, wherein, in the variation of the Si / Al ratio in the thickness direction of the zeolite membrane, the length of the range in which the Si / Al ratio is more than twice the Si / Al ratio of the surface portion is more than 25% of the thickness of the zeolite membrane.
[0011] The invention according to claim 3 is the zeolite membrane composite according to claim 1 or 2, wherein among changes in the Si / Al ratio in the thickness direction of the zeolite membrane, the maximum Si / Al ratio is 180 or more.
[0012] The invention according to claim 4 is the zeolite membrane composite according to any one of claims 1 to 3, wherein the Si / Al ratio at the surface portion of the zeolite membrane is 120 or less.
[0013] The invention of Scheme 5 is based on any zeolite membrane complex in Schemes 1 to 4, and in the change of the Si / Al ratio in the thickness direction of the zeolite membrane, the length of the range between the initial position where the Si / Al ratio is 1 / 2 of the maximum Si / Al ratio of the zeolite membrane and the support body from the interface toward the inside of the membrane is more than 25% of the thickness of the zeolite membrane.
[0014] The invention according to claim 6 is the zeolite membrane composite according to any one of claims 1 to 5, wherein the zeolite constituting the zeolite membrane is an 8-membered ring zeolite.
[0015] The invention of scheme 7 is a method for producing a zeolite membrane composite, which includes the following steps: a) preparing a raw material solution by mixing a Si source and two Al sources having different solubility in water in water; b) immersing a porous support in the raw material solution; c) heating the raw material solution to form a zeolite membrane on the support. In the step c), hydrothermal synthesis is performed at a temperature at which substantially all of one of the two Al sources contained in the raw material solution is dissolved and at least a portion of the other Al source is not dissolved, and then hydrothermal synthesis is performed at a temperature higher than the temperature. In this way, the above-mentioned zeolite membrane composite can be produced efficiently.
[0016] The invention of Scheme 8 is a separation method, which includes the following steps: a) preparing any zeolite membrane complex of Schemes 1 to 6; b) supplying a mixed substance containing multiple gases or liquids to the zeolite membrane complex, allowing the highly permeable substance in the mixed substance to pass through the zeolite membrane complex, thereby separating the substance from other substances.
[0017] The above-mentioned object and other objects, features, aspects and advantages will become more apparent from the following detailed description of the present invention with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a cross-sectional view of a zeolite membrane composite.
[0019] Figure 2 This is a cross-sectional view showing an enlarged portion of a zeolite membrane composite.
[0020] Figure 3 This is a diagram for explaining the change in the Si / Al ratio in the thickness direction of the zeolite membrane.
[0021] Figure 4 It is a diagram showing the production flow of a zeolite membrane composite.
[0022] Figure 5A It is a diagram schematically showing the state of the raw material solution.
[0023] Figure 5B It is a diagram schematically showing the state of the raw material solution.
[0024] Figure 5C It is a diagram schematically showing the state of the raw material solution.
[0025] Figure 6 It is a diagram showing a separation device.
[0026] Figure 7 It is a diagram showing the separation flow of mixed substances.
[0027] Fig. 8A This is a diagram showing the change in the Si / Al ratio in the thickness direction of the zeolite membrane.
[0028] Figure 8B This is a diagram showing the change in the Si / Al ratio in the thickness direction of the zeolite membrane.
[0029] Figure 8C This is a diagram showing the change in the Si / Al ratio in the thickness direction of the zeolite membrane.
[0030] Fig.8D This is a diagram showing the change in the Si / Al ratio in the thickness direction of the zeolite membrane.
[0031] Fig. 8E This is a diagram showing the change in the Si / Al ratio in the thickness direction of the zeolite membrane.
[0032] Fig. 9A This is a diagram showing changes in the Si / Al ratio in the thickness direction of a zeolite membrane of a comparative example.
[0033] Fig. 9B This is a diagram showing changes in the Si / Al ratio in the thickness direction of a zeolite membrane of a comparative example.
[0034] Fig. 9C This is a diagram showing changes in the Si / Al ratio in the thickness direction of a zeolite membrane of a comparative example.
[0035] Fig.10 This is a diagram for explaining the measurement of the vacuum degree. DETAILED DESCRIPTION
[0036] Figure 1 It is a cross-sectional view of the zeolite membrane composite 1 . Figure 2 This is a cross-sectional view showing a part of the zeolite membrane complex 1 in an enlarged manner. The zeolite membrane complex 1 comprises: a porous support 11, and a zeolite membrane 12 provided on the support 11. The zeolite membrane refers to a membrane in which zeolite is formed in a film shape at least on the surface of the support 11, and does not include a membrane in which zeolite particles are merely dispersed in an organic membrane. In addition, the zeolite membrane 12 may include two or more zeolites having different structures and compositions. Figure 1 In FIG. 1 , the zeolite membrane 12 is drawn with thick lines. Figure 2 In FIG. 1 , parallel oblique lines are marked on the zeolite membrane 12. In addition, Figure 2 In FIG. 1 , the thickness of the zeolite membrane 12 is drawn thicker than the actual thickness.
[0037] The support 11 is a porous member through which gas and liquid can pass. Figure 1 In the example shown, the support body 11 is: a columnar body obtained by integral molding and connected as a whole is provided with two Figure 1 An integral support body having multiple through holes 111 extending in the left-right direction (in the middle). Figure 1 In the example shown, the support body 11 is substantially cylindrical. The cross section of each through hole 111 (that is, cell) perpendicular to the longitudinal direction is, for example, substantially circular. Figure 1 In FIG. 1 , the diameter of the through hole 111 is drawn larger than the actual diameter, and the number of the through holes 111 is drawn less than the actual number. The zeolite membrane 12 is formed on the inner peripheral surface of the through hole 111 and covers the inner peripheral surface of the through hole 111 substantially entirely.
[0038] The length of the support 11 (i.e. Figure 1The length in the left-right direction in the through hole 11 is, for example, 10 cm to 200 cm. The outer diameter of the support body 11 is, for example, 0.5 cm to 30 cm. The distance between the central axes of adjacent through holes 111 is, for example, 0.3 mm to 10 mm. The surface roughness (Ra) of the support body 11 is, for example, 0.1 μm to 5.0 μm, preferably 0.2 μm to 2.0 μm. It should be noted that the shape of the support body 11 can be, for example, a honeycomb, a flat plate, a tubular, a cylindrical, a cylindrical or a polygonal column. When the shape of the support body 11 is tubular or cylindrical, the thickness of the support body 11 is, for example, 0.1 mm to 10 mm.
[0039] The material of the support 11 only needs to be chemically stable in the process of forming the zeolite film 12 on the surface, and various materials (such as ceramics or metals) can be used. In the present embodiment, the support 11 is formed by a ceramic sintered body. Examples of the ceramic sintered body selected as the material of the support 11 include: alumina, silica, mullite, zirconia, titanium dioxide, yttrium trioxide, silicon nitride, silicon carbide, etc. In the present embodiment, the support 11 includes at least one of alumina, mullite and zirconia.
[0040] The support 11 may contain an inorganic binder. As the inorganic binder, at least one of titanium dioxide, mullite, sinterable alumina, silicon dioxide, glass frit, clay mineral, and sinterable cordierite may be used.
[0041] The average pore diameter of the support 11 is, for example, 0.01 μm to 70 μm, preferably 0.05 μm to 25 μm. The average pore diameter of the support 11 near the surface of the zeolite membrane 12 to be formed is 0.01 μm to 1 μm, preferably 0.05 μm to 0.5 μm. For example, the average pore diameter can be measured using a mercury porosimeter, a pore size distribution meter, or a nanosize pore size distribution meter. Regarding the distribution of the overall pore diameter of the support 11, including the surface and the interior, D5 is, for example, 0.01 μm to 50 μm, D50 is, for example, 0.05 μm to 70 μm, and D95 is, for example, 0.1 μm to 2000 μm. The porosity of the support 11 near the surface of the zeolite membrane 12 to be formed is, for example, 25% to 50%.
[0042] The support 11 has, for example, a multilayer structure in which multiple layers with different average pore diameters are stacked in the thickness direction. The average pore diameter and sintered particle diameter of the surface layer including the surface on which the zeolite membrane 12 is to be formed are smaller than the average pore diameter and sintered particle diameter of the layer other than the surface layer. The average pore diameter of the surface layer of the support 11 is, for example, 0.01 μm to 1 μm, preferably 0.05 μm to 0.5 μm. When the support 11 has a multilayer structure, the materials of each layer can be the above-mentioned materials. The materials of the multiple layers forming the multilayer structure can be the same or different.
[0043] The zeolite membrane 12 is a porous membrane with fine pores. The zeolite membrane 12 can be used as a separation membrane for separating a specific substance from a mixed substance obtained by mixing multiple substances using a molecular sieving effect. In the zeolite membrane 12, other substances are less likely to permeate than the specific substance. In other words, the permeation amount of the other substance of the zeolite membrane 12 is less than the permeation amount of the above-mentioned specific substance.
[0044] The thickness of the zeolite membrane 12 is, for example, 0.05 μm to 30 μm, preferably 0.1 μm to 20 μm, and more preferably 0.5 μm to 10 μm. If the zeolite membrane 12 is thickened, the separation performance is improved. If the zeolite membrane 12 is thinned, the permeation rate increases. The surface roughness (Ra) of the zeolite membrane 12 is, for example, 5 μm or less, preferably 2 μm or less, more preferably 1 μm or less, and more preferably 0.5 μm or less.
[0045] The average pore size of the zeolite membrane 12 is, for example, less than 1 nm. The average pore size of the zeolite membrane 12 is preferably greater than 0.2 nm and less than 0.8 nm, more preferably greater than 0.3 nm and less than 0.7 nm, and further preferably greater than 0.3 nm and less than 0.6 nm. If the average pore size is greater than 1 nm, the separation performance is sometimes reduced. In addition, if the average pore size is less than 0.2 nm, the permeation rate is sometimes reduced. The average pore size of the zeolite membrane 12 is smaller than the average pore size of the support 11 near the surface where the zeolite membrane 12 is to be formed.
[0046] When the maximum number of rings of the zeolite constituting the zeolite membrane 12 is n, the arithmetic average of the short diameter and the long diameter of the n-membered ring pore is set as the average pore diameter. The n-membered ring pore refers to a pore in which the number of oxygen atoms in the part where the oxygen atom is bonded to the T atom described later to form a ring structure is n. When the zeolite has a plurality of n-membered ring pores equal in number, the arithmetic average of the short diameter and the long diameter of all types of n-membered ring pores is set as the average pore diameter of the zeolite. In this way, the average pore diameter of the zeolite membrane is uniquely determined by the skeleton structure of the zeolite, and can be obtained based on the values disclosed in the "Database of ZeoliteStructures" [online] of the International Zeolite Association and the website <URL: http: / / www.iza-structure.org / databases / >.
[0047] The type of zeolite constituting the zeolite membrane 12 is not particularly limited, and may be, for example, AEI, AEN, AFN, AFV, AFX, BEA, CHA, DDR, ERI, ETL, FAU (X, Y), GIS, LEV, LTA, MEL, MFI, MOR, PAU, RHO, SAT, SOD or other zeolites.
[0048] From the viewpoint of improving separation performance, the maximum number of rings of the zeolite constituting the zeolite membrane 12 is preferably 8. That is, the zeolite is preferably an 8-membered ring zeolite. The zeolite membrane 12 is, for example, a DDR type zeolite. In other words, the zeolite membrane 12 is a zeolite membrane composed of a zeolite having a structure code of "DDR" as specified by the International Zeolite Society. In this case, the inherent pore diameter of the zeolite constituting the zeolite membrane 12 is 0.36nm×0.44nm, and the average pore diameter is 0.40nm.
[0049] Typically, the zeolite constituting the zeolite membrane 12 is an aluminosilicate zeolite in which the atoms (T atoms) located at the center of the oxygen tetrahedron (TO4) constituting the zeolite contain silicon (Si) and aluminum (Al). A portion of the T atoms may be replaced by other elements. The zeolite membrane 12 may contain an alkali metal. The alkali metal is, for example, sodium (Na) or potassium (K).
[0050] Figure 3 1 is a diagram for explaining the change in the Si / Al ratio in the thickness direction of the zeolite membrane 12. Figure 3 The lower part of shows the change in the Si / Al ratio in the thickness direction of the zeolite membrane 12 . Figure 3 The vertical axis at the bottom of the graph shows the Si / Al ratio, and the horizontal axis shows the position in the thickness direction (depth direction) when the surface of the zeolite membrane 12 is set to 0 (described later). FIG. 8A to FIG. 8E as well as 9A to 9C The same is true in Figure 3The upper part shows a part of the cross section of the zeolite membrane 12 and the support 11, and a gradient is applied to the cross section representing the zeolite membrane 12, in which the Si / Al ratio increases and becomes denser. The Si / Al ratio is a molar ratio, which is the value obtained by dividing the molar number of Si atoms by the molar number of Al atoms. The change of the Si / Al ratio in the thickness direction is solved as follows: Using X-ray photoelectron spectroscopy (XPS: X-ray Photoelectron Spectroscopy), the depth direction composition analysis of the zeolite membrane 12 after cleaning (sputtering 1nm to remove the surface contamination layer) is performed. It should be noted that in the change of the Si / Al ratio in the thickness direction, the range in the thickness direction where the Si / Al ratio is less than 1 is set as the support 11.
[0051] The zeolite membrane 12 has an interface portion 121 and a surface portion 122. The interface portion 121 is a portion forming an interface with the support 11, and the surface portion 122 is a portion forming a surface on the opposite side of the support 11. In the zeolite membrane 12, the portion between the interface portion 121 and the surface portion 122 is set as the membrane interior, and the Si / Al ratio changes approximately continuously in the thickness direction from the interface portion 121 through the membrane interior to the surface portion 122. Specifically, as Figure 3 As shown in the lower part of the film, the Si / Al ratio gradually increases from the interface 121 toward the inside of the film, and gradually decreases from the inside of the film toward the surface 122. That is, the change in the thickness direction of the Si / Al ratio becomes a mountain shape with an inclination that increases toward the inside of the film on the interface 121 side and the surface 122 side. In fact, the value of the Si / Al ratio sometimes changes up and down due to measurement deviation. In this case, when measuring from the film surface toward the support 11, the film surface uses the measured value, the second point uses the average value of 3 points added with the measured values of the previous and next points, and the third point and the following point use the average value of 5 points added with the previous 2 points and the next 2 points to obtain the change in the thickness direction of the Si / Al ratio. In addition, when the change in the Si / Al ratio is a continuous increase trend or a decrease trend (however, except for the position where the inside of the film changes from an increase trend to a decrease trend), it is judged that the Si / Al ratio changes continuously. It should be noted that at a position inside the film, for example, when Al is less than the detection lower limit, the Si / Al ratio at this position can be excluded. The Si / Al ratio at this position may be interpolated using nearby values or calculated using the detection lower limit of Al.
[0052] In the zeolite membrane 12, the Si / Al ratio Va of the surface portion 122 is relatively small, and the surface portion 122 contains a large amount of Al. Accordingly, the polarity of the surface portion 122 becomes larger, the hydrophilicity is improved, and a high water permeation flux can be achieved. The Si / Al ratio Va of the surface portion 122 is, for example, less than half of the maximum Si / Al ratio Vb described later. The Si / Al ratio Va is preferably 120 or less, more preferably 110 or less, and further preferably 100 or less. Accordingly, the water permeation flux can be more reliably improved. The lower limit of the Si / Al ratio Va of the surface portion 122 is not particularly limited, and is, for example, 1.
[0053] In the zeolite membrane 12, high hydrothermal resistance can be achieved by having a relatively large Si / Al ratio inside the membrane. As described later, hydrothermal resistance can be evaluated by the degree of reduction in the vacuum degree before and after immersing the zeolite membrane complex 1 in heated water. In the variation of the Si / Al ratio in the thickness direction, when the range in the thickness direction in which the Si / Al ratio is more than twice the Si / Al ratio Va of the surface portion 122 is referred to as a "high Si / Al ratio range", the ratio (La / T) of the length La in the thickness direction of the high Si / Al ratio range to the thickness T of the zeolite membrane 12 is preferably 25% or more, more preferably 28% or more, and further preferably 30% or more. In addition, the maximum Si / Al ratio Vb in the variation of the Si / Al ratio in the thickness direction is preferably 180 or more, more preferably 200 or more, and further preferably 220 or more. The upper limit of the maximum Si / Al ratio Vb is not particularly limited, and is, for example, 300. As described above, the hydrothermal resistance is more reliably improved by extending the portion with a large Si / Al ratio in the zeolite membrane 12 to a wider range or / and by increasing the maximum Si / Al ratio Vb.
[0054] In the zeolite membrane 12, the membrane peeling can be suppressed by the relatively small Si / Al ratio of the interface 121. The reason why the membrane peeling is suppressed in the zeolite membrane 12 is not necessarily clear, but it is believed that: the hydroxyl groups on the surface of the support 11 are polar, and the polarity of the interface 121 where the Si / Al ratio is small and contains a large amount of Al is also large, so the adhesion between the zeolite membrane 12 and the surface of the support 11 is improved. In the change of the Si / Al ratio in the thickness direction, when the range in the thickness direction between the initial position where the Si / Al ratio is 1 / 2 of the maximum Si / Al ratio Vb of the zeolite membrane 12 from the interface 121 toward the inside of the membrane and the support 11 is called the "interface side focus range", the ratio (Lb / T) of the length Lb in the thickness direction of the interface side focus range to the thickness T of the zeolite membrane 12 is preferably 25% or more, more preferably 30% or more, and further preferably 35% or more. According to this, the membrane peeling can be more reliably suppressed.
[0055] Next, refer to Figure 4, an example of the manufacturing process of the zeolite membrane complex 1 is described. When manufacturing the zeolite membrane complex 1, first, a seed crystal for manufacturing the zeolite membrane 12 is prepared (step S11). For example, a powder of DDR type zeolite is generated by hydrothermal synthesis, and a seed crystal is obtained from the zeolite powder. The zeolite powder can be used directly as a seed crystal, or the powder can be processed by pulverizing or the like to obtain a seed crystal.
[0056] Next, the porous support 11 is immersed in the dispersion liquid in which the seed crystals are dispersed, so that the seed crystals are attached to the support 11 (step S12). Alternatively, the dispersion liquid in which the seed crystals are dispersed is brought into contact with the portion of the support 11 on which the zeolite membrane 12 is to be formed, so that the seed crystals are attached to the support 11. Thus, a seed crystal-attached support is produced. The seed crystals can also be attached to the support 11 by other methods.
[0057] In addition, a raw material solution for generating the zeolite membrane 12 is prepared (step S13). For example, a Si source, two Al sources (hereinafter referred to as "the first Al source" and "the second Al source"), and a structure-directing agent (hereinafter also referred to as "SDA") are mixed in water (H2O) to prepare a raw material solution. The Si source in this treatment example is amorphous silica (for example, silica sol). The Si source can be colloidal silica, fumed silica, sodium silicate, silicon alkoxide, water glass, etc. The solubility of the first Al source and the second Al source in water is different from each other. Specifically, in the temperature range from the initial temperature to the first synthesis temperature during the hydrothermal synthesis described later, the solubility of the first Al source in water is higher than the solubility of the second Al source. The first Al source is, for example, a water-soluble aluminum compound, and examples thereof include: sodium aluminate, aluminum hydroxide, aluminum alkoxide, etc. The second Al source is, for example, an aluminum compound that is poorly soluble in water, and examples thereof include: boehmite, alumina, etc. SDA is, for example, an organic substance. As SDA, for example, 1-adamantanamine, tetramethylammonium hydroxide, choline chloride, etc. Other raw materials such as a Na source may be mixed in the raw material solution.
[0058] After the raw material solution is prepared, the support 11 with the seed crystal attached is immersed in the raw material solution (step S14). Afterwards, hydrothermal synthesis is used to grow DDR type zeolite with the seed crystal as the nucleus, thereby forming a DDR type zeolite membrane 12 on the support 11 (step S15). In the hydrothermal synthesis, the raw material solution is heated in two stages. In this treatment example, the raw material solution is heated from an initial temperature (for example, room temperature) to a first synthesis temperature, and then maintained constant at the first synthesis temperature. When the first synthesis temperature is reached and a specified time has passed, the raw material solution is heated from the first synthesis temperature to a second synthesis temperature higher than the first synthesis temperature, and then maintained constant at the second synthesis temperature. When the second synthesis temperature is reached and a specified time has passed, the temperature of the raw material solution is returned to near the initial temperature.
[0059] FIG. 5A to FIG. 5C is a diagram schematically showing the state of the raw material solution. In the raw material solution of this treatment example, at the initial temperature, substantially all of the water-soluble first Al source is dissolved in water. During the period when the raw material solution is heated from the initial temperature to the first synthesis temperature and maintained, Figure 5A As shown in FIG. 1 , the Si source 80 dispersed in the raw material solution gradually dissolves in the water, and the Si concentration of the raw material solution (i.e., the concentration of Si dissolved in the water) increases. Figure 3 As shown in the lower part of , in the zeolite membrane 12, the Si / Al ratio gradually increases from the interface portion 121 toward the inside of the membrane. Depending on the amount of the first Al source in the raw material solution, at the first synthesis temperature, substantially all (for example, more than 99%) of the first Al source can be dissolved in water. In the raw material solution at the first synthesis temperature, the second Al source 82 is almost insoluble in water and is in a dispersed state. In the raw material solution at the first synthesis temperature, a portion of the second Al source 82 can also be dissolved in water. It should be noted that, as described above, even when a seed crystal is used, the seed crystal grows while introducing Al dissolved in the raw material solution, and therefore, the Si / Al ratio of the interface portion 121 changes substantially continuously in the thickness direction.
[0060] like Figure 5B As shown in FIG. 1 , when all the Si source 80 is dissolved in water, the dissolved Si and Al are consumed by the formation of the zeolite membrane 12 at a substantially constant ratio, and the Si / Al ratio is substantially constant near the maximum Si / Al ratio Vb. Then, while the raw material solution is heated from the first synthesis temperature to the second synthesis temperature and maintained, as shown in FIG. Figure 5C As shown, the second Al source 82 dispersed in the raw material solution gradually dissolves in water, and the Al concentration of the raw material solution (i.e., the concentration of Al dissolved in water) increases. Accordingly, in the zeolite membrane 12, the Si / Al ratio gradually decreases from the inside of the membrane toward the surface portion 122. By controlling the amount of Si and the amount of Al in the raw material solution (synthetic sol) as described above, a zeolite membrane 12 is formed in which the Si / Al ratio changes continuously and in a mountainous shape in the thickness direction. The zeolite membrane 12 in which the Si / Al ratio changes continuously can be regarded as a single-layer membrane.
[0061] The first synthesis temperature in this treatment example is a temperature at which the first Al source is substantially completely dissolved and the second Al source is not completely dissolved (i.e., at least a portion of the second Al source is not dissolved), for example, 100 to 130°C, preferably 120 to 130°C. The second synthesis temperature is a temperature higher than the first synthesis temperature, for example, 130 to 150°C, preferably 140 to 150°C. The holding time of the first synthesis temperature is, for example, 4 to 15 hours, preferably 4 to 11 hours. The holding time of the second synthesis temperature is, for example, 1 to 10 hours, preferably 2 to 7 hours. The total holding time of the first synthesis temperature and the second synthesis temperature is, for example, 5 to 25 hours. In the synthesis of the zeolite membrane 12, it is not necessarily necessary to provide a period of holding at a certain temperature. For example, by appropriately changing the temperature change rate during heating, a zeolite membrane 12 in which the Si / Al ratio increases from the interface portion 121 toward the inside of the membrane and decreases from the inside of the membrane toward the surface portion 122 can be formed.
[0062] After the hydrothermal synthesis is completed, the support 11 and the zeolite membrane 12 are washed with pure water. The washed support 11 and the zeolite membrane 12 are dried at, for example, 80° C. After the support 11 and the zeolite membrane 12 are dried, the zeolite membrane 12 is heated to burn and remove the SDA in the zeolite membrane 12 almost completely, so that the micropores in the zeolite membrane 12 are penetrated. Thus, the above-mentioned zeolite membrane composite 1 is obtained.
[0063] Next, refer to Figure 6 and Figure 7 , separation of mixed substances using the zeolite membrane composite 1 will be described. Figure 6 It is a diagram showing the separation device 2. Figure 7 1 is a diagram showing a separation flow for separating a mixed substance using the separation device 2 .
[0064] In the separation device 2, a mixed substance containing a plurality of fluids (i.e., gas or liquid) is supplied to the zeolite membrane complex 1, and a substance with high permeability (hereinafter also referred to as "high permeability substance") in the mixed substance is separated from the mixed substance by allowing it to pass through the zeolite membrane complex 1. For example, the separation in the separation device 2 may be performed for the purpose of extracting the high permeability substance from the mixed substance, or the separation in the separation device 2 may be performed for the purpose of concentrating the substance with low permeability (hereinafter also referred to as "low permeability substance").
[0065] The mixed substance (ie, mixed fluid) may be a mixed gas containing a plurality of gases, a mixed liquid containing a plurality of liquids, or a gas-liquid two-phase fluid containing both gas and liquid.
[0066] The mixed substance includes, for example, hydrogen (H2), helium (He), nitrogen (N2), oxygen (O2), water (H2O), carbon monoxide (CO), carbon dioxide (CO2), nitrogen oxides, ammonia (NH3), sulfur oxides, hydrogen sulfide (H2S), sulfur fluoride, mercury (Hg), arsine (AsH3), hydrogen cyanide (HCN), carbonyl sulfide (COS), C1-C8 hydrocarbons, organic acids, alcohols, thiols, esters, ethers, ketones, and aldehydes. The above-mentioned high permeability substance is, for example, one or more substances selected from H2, He, N2, O2, CO2, NH3, and H2O, preferably H2O.
[0067] Nitrogen oxides are compounds of nitrogen and oxygen. The above-mentioned nitrogen oxides are, for example, nitric oxide (NO), nitrogen dioxide (NO2), nitrous oxide (also known as dinitrogen monoxide) (N2O), dinitrogen trioxide (N2O3), dinitrogen tetroxide (N2O4), dinitrogen pentoxide (N2O5), etc. X (NOX) gases.
[0068] Sulfur oxides are compounds of sulfur and oxygen. The above-mentioned sulfur oxides are sulfur dioxide (SO2), sulfur trioxide (SO3), etc., which are called SO X (SOX) gas.
[0069] Sulfur fluoride is a compound of fluorine and sulfur. The above-mentioned sulfur fluoride is, for example, sulfur difluoride (FSSF, S=SF2), sulfur difluoride (SF2), sulfur tetrafluoride (SF4), sulfur hexafluoride (SF6) or sulfur decafluoride (S2F 10 )wait.
[0070] C1 to C8 hydrocarbons are hydrocarbons having more than 1 and less than 8 carbon atoms. C3 to C8 hydrocarbons may be any of straight chain compounds, side chain compounds, and cyclic compounds. In addition, C2 to C8 hydrocarbons may be any of saturated hydrocarbons (i.e., hydrocarbons without double bonds and triple bonds in the molecule) and unsaturated hydrocarbons (i.e., hydrocarbons with double bonds and / or triple bonds in the molecule). C1 to C4 hydrocarbons are, for example, methane (CH4), ethane (C2H6), ethylene (C2H4), propane (C3H8), propylene (C3H6), n-butane (CH3(CH2)2CH3), isobutane (CH(CH3)3), 1-butene (CH2=CHCH2CH3), 2-butene (CH3CH=CHCH3), or isobutylene (CH2=C(CH3)2).
[0071] The above-mentioned organic acid is a carboxylic acid or a sulfonic acid, etc. Carboxylic acid is, for example, formic acid (CH2O2), acetic acid (C2H4O2), oxalic acid (C2H2O4), acrylic acid (C3H4O2) or benzoic acid (C6H5COOH), etc. Sulfonic acid is, for example, ethanesulfonic acid (C2H6O3S), etc. The organic acid may be a chain compound or a cyclic compound.
[0072] The above-mentioned alcohol is, for example, methanol (CH3OH), ethanol (C2H5OH), isopropyl alcohol (2-propanol) (CH3CH(OH)CH3), ethylene glycol (CH2(OH)CH2(OH)) or butanol (C4H9OH) and the like.
[0073] Thiols are organic compounds having hydrogenated sulfur (SH) at the end, and are also called Thiol or Thioalcohol. Examples of the thiols include methyl mercaptan (CH3SH), ethyl mercaptan (C2H5SH), and 1-propanethiol (C3H7SH).
[0074] The above-mentioned ester is, for example, formates or acetates.
[0075] The above-mentioned ether is, for example, dimethyl ether ((CH3)2O), methyl ethyl ether (C2H5OCH3), diethyl ether ((C2H5)2O) or tetrahydrofuran ((CH2)4O) or the like.
[0076] The above-mentioned ketone is, for example, acetone ((CH3)2CO), methyl ethyl ketone (C2H5COCH3) or diethyl ketone ((C2H5)2CO) or the like.
[0077] The above-mentioned aldehyde is, for example, acetaldehyde (CH3CHO), propionaldehyde (C2H5CHO) or butyraldehyde (Butyraldehyde) (C3H7CHO).
[0078] In the following description, an example is given in which the mixed substance to be separated by the separation device 2 is a mixed liquid containing a plurality of liquids and the separation is performed by the pervaporation method (pervaporation method).
[0079] The separation device 2 includes a zeolite membrane complex 1, a sealing portion 21, a housing 22, two sealing components 23, a supply portion 26, a first recovery portion 27, and a second recovery portion 28. The zeolite membrane complex 1, the sealing portion 21, and the sealing component 23 are accommodated in the housing 22. The supply portion 26, the first recovery portion 27, and the second recovery portion 28 are arranged outside the housing 22 and connected to the housing 22.
[0080] The sealing part 21 is installed in the longitudinal direction of the support body 11 (i.e. Figure 6The sealing portion 21 is a component that seals the two end portions of the support body 11 (in the left-right direction) and covers the two end surfaces in the longitudinal direction of the support body 11 and the outer peripheral surface near the two end surfaces. The sealing portion 21 prevents liquid from flowing in and out through the two end surfaces of the support body 11. The sealing portion 21 is a plate-shaped component formed of, for example, glass or resin. The material and shape of the sealing portion 21 can be appropriately changed. It should be noted that since the sealing portion 21 is provided with a plurality of openings overlapping with the plurality of through holes 111 of the support body 11, the two ends in the longitudinal direction of each through hole 111 of the support body 11 are not covered by the sealing portion 21. Therefore, liquids and the like can flow into and out of the through holes 111 through the two ends.
[0081] The shape of the housing 22 is not particularly limited, and it is, for example, a substantially cylindrical member. The housing 22 is formed, for example, of stainless steel or carbon steel. The length direction of the housing 22 is substantially parallel to the length direction of the zeolite membrane composite 1. Figure 6 A supply port 221 is provided at the left end of the housing 22, and a first discharge port 222 is provided at the other end. A second discharge port 223 is provided on the side of the housing 22. The supply port 221 is connected to the supply unit 26. The first discharge port 222 is connected to the first recovery unit 27. The second discharge port 223 is connected to the second recovery unit 28. The internal space of the housing 22 is a closed space isolated from the space around the housing 22.
[0082] Two sealing components 23 are arranged around the outer peripheral surface of the zeolite membrane complex 1 and the inner peripheral surface of the housing 22 near both ends of the zeolite membrane complex 1 in the longitudinal direction. Each sealing component 23 is a roughly annular component formed of a liquid-impermeable material. The sealing component 23 is, for example, an O-ring formed of a flexible resin. The sealing component 23 is in close contact with the outer peripheral surface of the zeolite membrane complex 1 and the inner peripheral surface of the housing 22 around the entire circumference. Figure 6 In the example shown, the sealing member 23 is in close contact with the outer peripheral surface of the sealing portion 21, and is indirectly in close contact with the outer peripheral surface of the zeolite membrane complex 1 via the sealing portion 21. The sealing member 23 and the outer peripheral surface of the zeolite membrane complex 1 and the sealing member 23 and the inner peripheral surface of the housing 22 are sealed, and liquid can hardly pass through or cannot pass through at all.
[0083] The supply unit 26 supplies the mixed liquid to the internal space of the housing 22 via the supply port 221. The supply unit 26 includes, for example, a pump that pressurizes the mixed liquid toward the housing 22. The pump includes: a temperature regulating unit and a pressure regulating unit that respectively regulate the temperature and pressure of the mixed liquid supplied to the housing 22. The first recovery unit 27 includes: a storage container that stores the liquid discharged from the housing 22 or a pump that transfers and transports the liquid. The second recovery unit 28 includes: a vacuum pump that decompresses the outer space of the outer peripheral surface of the zeolite membrane complex 1 in the housing 22 (i.e., the space sandwiched by the two sealing components 23), and a cooling trap that cools and liquefies the gas that evaporates and passes through the zeolite membrane complex 1.
[0084] When the mixed liquid is separated, the zeolite membrane composite 1 ( Figure 7 :Step S21). Next, a mixed liquid containing a plurality of liquids having different permeabilities to the zeolite membrane 12 is supplied to the inner space of the housing 22 by the supply unit 26. For example, the main components of the mixed liquid are water (H2O) and ethanol (C2H5OH). The mixed liquid may contain liquids other than water and ethanol. The pressure (i.e., the introduction pressure) of the mixed liquid supplied from the supply unit 26 to the inner space of the housing 22 is, for example, 0.1 MPa to 2 MPa, and the temperature of the mixed liquid is, for example, 10°C to 200°C.
[0085] The mixed liquid supplied from the supply unit 26 to the housing 22 is introduced from the left end of the zeolite membrane composite 1 in the figure into each through hole 111 of the support body 11 as indicated by arrow 251. The liquid with high permeability, that is, the high permeability substance in the mixed liquid is vaporized, and passes through the zeolite membrane 12 provided on the inner peripheral surface of each through hole 111 and the support body 11, and is discharged from the outer peripheral surface of the support body 11. Thus, the high permeability substance (for example, water) is separated from the liquid with low permeability, that is, the low permeability substance (for example, ethanol) in the mixed liquid (step S22).
[0086] The gas (hereinafter referred to as "permeable substance") derived from the outer peripheral surface of the support body 11 is introduced into the second recovery unit 28 via the second discharge port 223 as shown by the arrow 253, and is cooled in the second recovery unit 28 and recovered in the form of liquid. The pressure of the gas recovered by the second recovery unit 28 via the second discharge port 223 (i.e., the permeation pressure) is, for example, about 6.67 kPa (about 50 Torr). In addition to the above-mentioned high permeability substances, the permeable substance may also include a low permeability substance that permeates through the zeolite membrane 12.
[0087] In addition, the liquid in the mixed liquid other than the substance that permeates the zeolite membrane 12 and the support body 11 (hereinafter referred to as "non-permeable substance") passes through the through holes 111 of the support body 11 from the left side to the right side in the figure, and is recovered by the first recovery unit 27 via the first discharge port 222 as shown by the arrow 252. The pressure of the liquid recovered by the first recovery unit 27 via the first discharge port 222 is, for example, a pressure substantially the same as the introduction pressure. In addition to the above-mentioned low-permeability substances, the non-permeable substances may also include high-permeability substances that do not permeate the zeolite membrane 12. The non-permeable substance recovered by the first recovery unit 27 can be circulated to the supply unit 26 and supplied to the housing 22 again.
[0088] Next, Examples 1 to 5 and Comparative Examples 1 to 3 of the zeolite membrane composite are described.
[0089] (Fabrication of Seed Crystal Attachment Support)
[0090] A porous alumina support having a multilayer structure is prepared in the same manner as the manufacturing method described in International Publication No. 2017 / 169591 (the above-mentioned document 4). In addition, a seed crystal as a DDR type zeolite crystal powder is prepared in the same manner as the manufacturing method described in Japanese Patent Publication No. 2004-83375 (the above-mentioned document 5). Thereafter, the alumina support is contacted with a solution in which the seed crystal is dispersed so that the seed crystal is attached to the alumina support.
[0091] (Preparation of raw material solution)
[0092] After distilled water [a]g was placed in a wide-mouth bottle made of fluororesin, 1-adamantanamine (1-ADA, manufactured by Sigmaaldrich) [b]g, sodium hydroxide (NaOH, manufactured by Sigmaaldrich) [c]g, 30 wt% silica sol (trade name: SNOWTEX S, manufactured by Nissan Chemical Co., Ltd.) [d]g, sodium aluminate (manufactured by Wako Pure Chemical Industries, Ltd.) [e]g, and boehmite powder (AlO(OH), trade name: C20, manufactured by Daming Chemical Co., Ltd.) [f]g were added and stirred to prepare a raw material solution as a sol for film formation. The masses a to f of the raw materials in Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1.
[0093] [Table 1]
[0094]
[0095] (Synthesis of Zeolite Membrane)
[0096] After the alumina support is arranged in a fluororesin inner cylinder (internal volume 300 ml) of a stainless steel pressure-resistant container, the prepared raw material solution is placed therein and subjected to a heat treatment (hydrothermal synthesis) to form a DDR type zeolite membrane. During the hydrothermal synthesis, it is maintained at 130°C for [g] hours, and then maintained at 150°C for [h] hours. The holding times g and h at each temperature in Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1. Next, the alumina support is cleaned and dried at 80°C for more than 12 hours. Thereafter, the alumina support is heated to 450°C in an electric furnace and maintained for 50 hours to thereby burn and remove 1-adamantanamine. Through the above treatment, the zeolite membrane composites of Examples 1 to 5 and Comparative Examples 1 to 3 having a DDR type zeolite membrane are obtained.
[0097] (Si / Al ratio measurement)
[0098] Using X-ray photoelectron spectroscopy (XPS), the composition of the zeolite membrane after cleaning (1 nm sputtering to remove the surface contamination layer) was analyzed in depth to determine the change in the Si / Al ratio in the thickness direction. The measurement conditions are as follows: X-ray source: monochromatized AlKα ray (1486.6 eV), X-ray beam diameter: 100 μm, photoelectron extraction angle: 45° relative to the normal of the sample, sputtering: Ar monomer ions. In addition, the sputtering spacing, acceleration voltage, sputtering speed and sputtering end point during cleaning and measurement are shown in Table 2. It should be noted that the sputtering speed and depth are values converted to SiO2.
[0099] [Table 2]
[0100]
[0101] FIG. 8A to FIG. 8E is a graph showing the results of measuring the Si / Al ratio of the zeolite membrane composites of Examples 1 to 5. 9A to 9C This is a diagram showing the results of measuring the Si / Al ratio of the zeolite membrane composites of Comparative Examples 1 to 3. FIG. 8A to FIG. 8E as well as 9A to 9C The change of Si / Al ratio in the thickness direction is shown. In addition, the Si / Al ratio of the surface part is represented by a white triangle, and the position of the interface (here, the position where the Si / Al ratio is less than 1) is represented by a black triangle. Table 3 shows the Si / Al ratio of the surface part in the zeolite membrane composite of Examples 1 to 5 and Comparative Examples 1 to 3, the ratio of the length La of the high Si / Al ratio range to the thickness T of the zeolite membrane 12 (La / T), the maximum Si / Al ratio, and the ratio of the length Lb of the range of interest on the interface side to the thickness T of the zeolite membrane 12 (Lb / T) (refer to Figure 3 ). These values are based on FIG. 8A to FIG. 8Eas well as 9A to 9C It should be noted that, in the variation of the Si / Al ratio in the thickness direction, the range in the thickness direction where the Si / Al ratio is less than 1 is the alumina support. When the support is a material other than alumina, the point where the molar ratio of Si / (the total amount of elements constituting the support other than oxygen) is less than 1 is set as the interface.
[0102] [Table 3]
[0103]
[0104] In the zeolite membrane composites of Examples 1 to 5, FIG. 8A to FIG. 8E As shown in FIG. 1 , the Si / Al ratio increases from the interface toward the inside of the membrane, and decreases from the inside of the membrane toward the surface. On the other hand, in the zeolite membrane composites of Comparative Examples 1 and 2, as Fig. 9A and Fig. 9B As shown in FIG. 1 , the Si / Al ratio of the surface portion is larger than that of the inner portion of the membrane. Fig. 9C As shown, the Si / Al ratio at the interface is the same as that inside the film.
[0105] (Membrane performance evaluation)
[0106] Using the above-mentioned separation device 2, a water-ethanol mixture (mass ratio 50:50) was separated by pervaporation at a temperature of 60°C, and the permeation amount of the liquid recovered by the second recovery unit 28 was measured. Using a density hydrometer, the density of the liquid was calculated and the water / ethanol ratio was measured. Then, based on the permeation amount of the liquid and the water / ethanol ratio, the water permeation flux and the separation coefficient were calculated. The separation coefficient is the value obtained by dividing the water concentration (mass %) by the ethanol concentration. In Table 3, the water permeation flux is 2.5 kg / m 2 The case with a water permeation flux of less than 2.5 kg / m 2 h and 2.0kg / m 2 If the water permeation flux is less than 2.0 kg / m 2 The case of h was evaluated as "×".
[0107] In the zeolite membrane composites of Examples 1 to 5 and Comparative Examples 2 and 3, the water permeation flux was 2.0 kg / m 2 In particular, in the zeolite membrane composites of Examples 1, 2, 4, 5 and Comparative Examples 2 and 3, where the Si / Al ratio of the surface portion was 120 or less, the water permeation flux was 2.5 kg / m 2 In Comparative Example 1, the water permeation flux is relatively low (less than 2.0 kg / m 2 h).
[0108] (Evaluation of water and heat resistance)
[0109] In the evaluation of water and heat resistance, Figure 6 Similarly, the vacuum degree is measured using the housing 22 containing the zeolite membrane composite 1. In the measurement of the vacuum degree, Fig.10 As shown, a vacuum pump 291 (a direct-connected oil rotary vacuum pump manufactured by ULVAC KIKO Co., Ltd., model: G-20DA, exhaust speed 24L / min, reaching pressure 1.3Pa, 2-stage type) is connected to a port 221 at one end in the length direction of the housing 22 to perform vacuuming. In addition, a vacuum gauge 292 (a calibrator manufactured by GE Sensing, model: DPI800) is connected to a port 222 at the other end of the housing 22 to measure the reaching vacuum degree. At this time, a port 223 provided on the side of the housing 22 is open to the atmosphere. Next, the zeolite membrane composite taken out from the housing 22 is immersed in high-temperature water (180°C) for 12 hours, washed with ion exchange water, and dried at room temperature for more than 12 hours. Thereafter, the vacuum degree is measured again, and the ratio of the vacuum degree after immersion to the vacuum degree before immersion (hereinafter referred to as "the ratio of the vacuum degree before and after immersion") is set as an index of water heat resistance. In Table 3, the case where the ratio of the vacuum degree before and after immersion was 95% or more was evaluated as "0", the case where the ratio was less than 95% and 90% or more was evaluated as "△", and the case where the ratio was less than 90% was evaluated as "×".
[0110] In the zeolite membrane composites of Examples 1 to 5 and Comparative Examples 1 and 3, the ratio of the degree of vacuum before and after immersion was 90% or more, and high hydrothermal resistance was obtained. In particular, in the zeolite membrane composites of Examples 1 to 3 and Comparative Example 3, in which the ratio of the length La of the high Si / Al ratio range (La / T) was 25% or more and the maximum Si / Al ratio was 180 or more, the ratio of the degree of vacuum before and after immersion was 95% or more. In Comparative Example 2, the ratio of the degree of vacuum before and after immersion was less than 90%, and the hydrothermal resistance was low.
[0111] (Adhesion Evaluation)
[0112] The tape specified in JIS Z 1522 was attached to the surface of the zeolite membrane, and the surface of the zeolite membrane after the tape was peeled off was observed using a scanning electron microscope (SEM). In Table 3, the case where no membrane peeling was confirmed was evaluated as "○", the case where a small membrane peeling with a maximum width of less than 10 μm was confirmed was evaluated as "△", and the case where a large membrane peeling with a maximum width of more than 10 μm was confirmed was evaluated as "×".
[0113] In the zeolite membrane composites of Examples 1 to 5 and Comparative Examples 1 and 2, no significant membrane peeling was observed, and a zeolite membrane with improved adhesion was obtained. In addition, in the zeolite membrane composites of Examples 1, 3 to 5 and Comparative Examples 1 and 2, where the ratio of the length Lb of the range of interest on the interface side (Lb / T) was 30% or more, no membrane peeling occurred at all. In Comparative Example 3, significant membrane peeling was observed, and the adhesion was low.
[0114] As described above, the zeolite membrane composite 1 includes: a porous support 11, and a zeolite membrane 12 provided on the support 11. In the zeolite membrane 12, the Si / Al ratio increases in molar ratio from the interface portion 121 with the support 11 toward the inside of the membrane, and decreases from the inside of the membrane toward the surface portion 122 on the opposite side of the support 11. Thus, as in the above-mentioned Examples 1 to 5, a zeolite membrane composite 1 having high water permeation flux and hydrothermal resistance and suppressed membrane peeling can be realized.
[0115] Preferably, in the variation of the Si / Al ratio in the thickness direction of the zeolite membrane 12, the length of the range where the Si / Al ratio is twice or more of the Si / Al ratio of the surface portion 122 is at least 25% of the thickness of the zeolite membrane 12. By including a large amount of zeolites having a large Si / Al ratio in the zeolite membrane 12 in this manner, the hydrothermal resistance of the zeolite membrane 12 can be more reliably improved.
[0116] Preferably, the maximum Si / Al ratio in the thickness direction of the zeolite membrane 12 is not less than 180. When the zeolite membrane 12 includes zeolite having a sufficiently large Si / Al ratio, the hydrothermal resistance of the zeolite membrane 12 can be further improved.
[0117] Preferably, the Si / Al ratio at the surface portion 122 of the zeolite membrane 12 is not more than 120. This can improve the hydrophilicity of the surface portion 122 and more reliably improve the water permeation flux.
[0118] Preferably, in the change of the Si / Al ratio in the thickness direction of the zeolite membrane 12, the length of the range between the initial position where the Si / Al ratio is 1 / 2 of the maximum Si / Al ratio of the zeolite membrane 12 and the support 11 from the interface 121 toward the inside of the membrane is 25% or more of the thickness of the zeolite membrane 12. By making the Si / Al ratio small in a wide range near the interface 121 in this way, membrane peeling can be more reliably suppressed, thereby improving the adhesion of the zeolite membrane 12.
[0119] In addition, the zeolite constituting the zeolite membrane 12 is preferably an 8-membered ring zeolite. This allows the zeolite membrane composite 1 to achieve good selective permeation of a permeation target substance having a relatively small molecular diameter (particularly water).
[0120] Here, a comparative example of a method for manufacturing a zeolite membrane complex is described. In the manufacturing method of the comparative example, a zeolite membrane with a multilayer structure is formed. Specifically, a first zeolite layer with a relatively small Si / Al ratio is formed on a support using a raw material solution, a second zeolite layer with a relatively large Si / Al ratio is formed on the first zeolite layer using another raw material solution, and further, a third zeolite layer with a relatively small Si / Al ratio is formed on the second zeolite layer using yet another raw material solution. Thus, a multilayer zeolite membrane with a relatively small Si / Al ratio at the interface and surface is obtained. In the multilayer zeolite membrane, the Si / Al ratio is discontinuous at the boundary between adjacent zeolite layers. In the manufacturing method of the comparative example, since the formation of the zeolite layer is repeated, the manufacture of the zeolite membrane complex requires a long time.
[0121] In contrast, the method for manufacturing the above-mentioned zeolite membrane complex 1 includes the following steps: preparing a raw material solution by mixing a Si source and two Al sources having different solubility in water in water (step S13); immersing a porous support 11 in the raw material solution (step S14); and heating the raw material solution to form a zeolite membrane 12 on the support 11 (step S15). In step S15, hydrothermal synthesis is performed at a temperature at which one of the two Al sources contained in the raw material solution is substantially completely dissolved and at least a portion of the other Al source is not dissolved, and then hydrothermal synthesis is performed at a temperature higher than the temperature. Accordingly, the above-mentioned zeolite membrane 12 having a relatively small Si / Al ratio at the interface portion 121 and the surface portion 122 can be easily formed without repeatedly forming a zeolite layer as in the comparative example, thereby enabling the zeolite membrane complex 1 to be manufactured efficiently.
[0122] The above separation method includes the following steps: preparing a zeolite membrane complex 1 (step S21); and supplying a mixed substance containing a plurality of gases or liquids to the zeolite membrane complex 1, so that a highly permeable substance in the mixed substance passes through the zeolite membrane complex 1, thereby separating it from other substances (step S22). In this separation method, by using a zeolite membrane complex 1 having high water permeation flux and hydrothermal resistance and suppressed membrane peeling, various mixed substances can be separated efficiently and stably. The separation method using the zeolite membrane complex 1 is particularly suitable for the separation of mixed substances containing water.
[0123] The above-mentioned zeolite membrane composite 1 , the method for producing the zeolite membrane composite 1 , and the separation method may be modified in various ways.
[0124] As long as a zeolite membrane composite 1 having high water permeation flux and hydrothermal resistance and suppressed membrane peeling can be realized, the ratio (La / T) of the length La of the high Si / Al ratio range in the zeolite membrane 12 can be less than 25%, and the maximum Si / Al ratio can be less than 180. Similarly, the Si / Al ratio of the surface portion 122 can be greater than 120, and the ratio (Lb / T) of the length Lb of the interface side focus range can be less than 25%.
[0125] The maximum number of rings in the zeolite constituting the zeolite membrane 12 may be less than eight or greater than eight.
[0126] The zeolite membrane composite 1 may further include a functional film and a protective film laminated on the zeolite membrane 12 in addition to the support 11 and the zeolite membrane 12. Such a functional film and a protective film may be an inorganic film such as a zeolite membrane, a silicon dioxide film or a carbon film, or an organic film such as a polyimide film or an organic silicon film. In addition, a substance that easily absorbs water may be added to the functional film and the protective film laminated on the zeolite membrane 12.
[0127] Figure 4 In the manufacture of the zeolite membrane composite 1, the process of attaching the seed crystals to the support 11 (steps S11 and S12) may be omitted, and the zeolite membrane 12 may be directly formed on the support 11 in the process of step S15. Figure 4 Manufacturing by a method other than the manufacturing method of .
[0128] In the separation method, in addition to the separation of the mixed substance by the pervaporation method exemplified in the above description, the mixed substance can also be separated by a steam permeation method, a reverse osmosis method, a gas permeation method, etc. In addition, substances other than the substances exemplified in the above description can be separated from the mixed substance.
[0129] The configurations in the above-described embodiment and each modified example may be appropriately combined unless they are mutually contradictory.
[0130] Although the invention has been described in detail, the above description is illustrative and not restrictive. Therefore, it can be said that various modifications and solutions can be adopted without departing from the scope of the present invention.
[0131] Industrial Applicability
[0132] The zeolite membrane composite of the present invention can be utilized as, for example, a dehydration membrane, and can also be utilized as a separation membrane for various substances other than water or an adsorption membrane for various substances in various fields utilizing zeolite.
[0133] Explanation of symbols
[0134] 1 Zeolite membrane composite
[0135] 11 Support
[0136] 12 Zeolite membrane
[0137] 121 Interface Department
[0138] 122 Surface
[0139] Steps S11 to S15, S21, S22
Claims
1. A zeolite membrane composite, wherein: The invention comprises: a porous support and a zeolite membrane provided on the support, In the zeolite membrane, the Si / Al ratio in terms of molar ratio increases from the interface with the support toward the inside of the membrane, and decreases from the inside of the membrane toward the surface on the opposite side to the support.
2. The zeolite membrane composite according to claim 1, wherein In the variation of the Si / Al ratio in the zeolite membrane in the thickness direction, the length of the range where the Si / Al ratio is twice or more of the Si / Al ratio of the surface portion is 25% or more of the thickness of the zeolite membrane.
3. The zeolite membrane composite according to claim 1, wherein Among the changes in the Si / Al ratio in the thickness direction of the zeolite membrane, the maximum Si / Al ratio is 180 or more.
4. The zeolite membrane composite according to claim 1, wherein The Si / Al ratio at the surface portion of the zeolite membrane is 120 or less.
5. The zeolite membrane composite according to claim 1, wherein In the change of the Si / Al ratio in the zeolite membrane in the thickness direction, the length of the range between the initial position where the Si / Al ratio is 1 / 2 of the maximum Si / Al ratio of the zeolite membrane and the support body from the interface toward the inside of the membrane is more than 25% of the thickness of the zeolite membrane.
6. The zeolite membrane composite according to claim 1, wherein The zeolite constituting the zeolite membrane is an 8-membered ring zeolite.
7. A method for producing a zeolite membrane composite, wherein: Including the following processes: a) preparing a raw material solution by mixing a Si source and two Al sources having different solubility in water into water; b) immersing a porous support into the raw material solution; c) heating the raw material solution to form a zeolite film on the support, In the step c), hydrothermal synthesis is performed at a temperature at which substantially all of one of the two Al sources contained in the raw material solution is dissolved and at least a portion of the other Al source is not dissolved, and then hydrothermal synthesis is performed at a temperature higher than the temperature.
8. A separation method, wherein: Including the following processes: a) preparing the zeolite membrane composite according to any one of claims 1 to 6; b) supplying a mixed substance containing a plurality of gases or liquids to the zeolite membrane composite, allowing a substance with high permeability in the mixed substance to permeate through the zeolite membrane composite, thereby separating the substance from other substances.
Citation Information
Patent Citations
Method for manufacturing DDR type zeolite
JP2004083375A
Stopper structure for glove compartment
JP2022029614A
Porous support, method for manufacturing porous support, separation membrane structure, and method for manufacturing separation membrane structure
WO2017169591A1
Dewatering method and dewatering device
WO2018225787A1