Inorganic powder
By optimizing the physical properties of spherical alumina powder and spherical silica powder, the problem of insufficient fluidity of inorganic powder in resin is solved, more efficient mixing and operability are achieved, and the performance of the resin composition is improved.
Patent Information
- Application Number
- CN202380020963.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-09
- Filing Date
- 2023-02-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing inorganic powders have insufficient fluidity when blended with resin, making it difficult to meet the requirements for efficient mixing and operability.
By controlling the angle of repose, collapse angle, packing density and particle size distribution of spherical alumina powder and spherical silica powder, the physical properties of the inorganic powder are optimized to improve its fluidity and mixability with resin.
It significantly improves the fluidity and operability of inorganic powder and resin, enhances the compactness and mixing performance of the powder, and improves the strength and fluidity of the resin composition.
Smart Images

Figure BDA0004984604830000111 
Figure HDA0004984604850000011
Abstract
Description
Technical Field
[0001] The present invention relates to inorganic powders. Background Art
[0002] Various developments have been made on inorganic powders. As such a technology, for example, the technology described in Patent Document 1 is known. Patent Document 1 describes, as an inorganic powder, spherical alumina powder having a silica coating layer spheroidized by flame thermal spraying.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-014513 Summary of the invention
[0006] However, as a result of the present inventors' studies, they have found that the inorganic powder described in Patent Document 1 has room for improvement in terms of fluidity when mixed with a resin.
[0007] The present inventors have further studied and found that in an inorganic powder containing spherical alumina powder and spherical silica powder, by appropriately controlling the angle of repose, the fluidity when the inorganic powder is blended with a resin can be improved, thereby completing the present invention.
[0008] According to one aspect of the present invention, the following inorganic powder is provided.
[0009] 1. An inorganic powder comprising spherical alumina powder and spherical silica powder,
[0010] The repose angle measured by the following step A at a room temperature of 25°C and a humidity of 65% is 35° to 47°.
[0011] (Step A)
[0012] A funnel with an outlet diameter of 0.5 cm was installed at a height of 15 cm from a horizontal plate provided on the powder tester.
[0013] The inorganic powder is continuously supplied from a vertical direction onto the surface of the horizontal plate via a hopper to form a conical deposit that maintains a constant shape.
[0014] Using a protractor, the elevation angle between the side surface of the conical deposit and the surface of the horizontal plate was determined and taken as the repose angle (°).
[0015] Next, a weight of 110 g was dropped from a height of 18 cm three times to apply impact to the horizontal plate. Then, using a protractor, the elevation angle between the side surface of the conical deposit and the surface of the horizontal plate was determined and taken as the collapse angle (°).
[0016] 2. The inorganic powder according to 1., wherein
[0017] Under the conditions of room temperature of 25°C and humidity of 65%, the collapse angle measured according to the above step A is 20° to 37°.
[0018] 3. The inorganic powder according to 1. or 2., wherein
[0019] At room temperature of 25°C and humidity of 55%, the tapped bulk density measured according to step B below is 1.5 g / cm 3 ~2.3g / cm 3 .
[0020] (Step B)
[0021] The inorganic powder is naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup to prepare a full cup in the shape of a mountain.
[0022] Next, the portion of the cup that is filled in a mountain shape is scraped off without shaking it, and the mass (g) of the inorganic powder filled in the cup is measured to calculate the loose bulk density (g / cm 3 ).
[0023] On the other hand, for a cup filled with a mountain shape, after vibrating it 180 times in the up and down direction (stroke length 2 cm, 1 second / time), the part exceeding the upper surface of the cup was scraped off, and the mass (g) of the inorganic powder filled in the cup was measured to calculate the tapped bulk density (g / cm 3 ).
[0024] 4. The inorganic powder according to 1. to 3., wherein
[0025] When the loose bulk density measured in step B is defined as A and the tapped bulk density is defined as P,
[0026] The compression degree calculated based on ((P-A) / P)×100 is 30% to 44%.
[0027] 5. The inorganic powder according to any one of 1. to 4., wherein
[0028] In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 10% is defined as D 10 The particle size with a cumulative value of 50% is set as D 50 The particle size with a cumulative value of 97% is set as D 97 hour,
[0029] (D97 -D 10 ) / D 50 4 to 30.
[0030] 6. The inorganic powder according to any one of 1. to 5., wherein
[0031] In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 10% is defined as D 10 The particle size with a cumulative value of 50% is set as D 50 hour,
[0032] D 50 -D 10 0.5μm~17μm.
[0033] According to the present invention, there is provided an inorganic powder having excellent fluidity when mixed with a resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic cross-sectional view showing the structure of a thermal spraying device. DETAILED DESCRIPTION
[0035] The outline of the inorganic powder according to the present embodiment will be described.
[0036] The inorganic powder of the present embodiment contains spherical alumina powder and spherical silica powder, and has a repose angle of 35° to 47°.
[0037] The upper limit of the repose angle of the inorganic powder is 47° or less, preferably 46° or less, and more preferably 45° or less. This can improve the fluidity of the resin composition containing the inorganic powder.
[0038] The lower limit of the angle of repose of the inorganic powder is, for example, 35° or more, preferably 36° or more, and more preferably 37° or more. This can be expected to improve the handling properties of the powder.
[0039] The upper limit of the collapse angle of the inorganic powder is 37° or less, preferably 36° or less, and more preferably 35° or less. This can further improve the fluidity of the resin composition containing the inorganic powder.
[0040] The lower limit of the collapse angle of the inorganic powder is, for example, 20° or more, preferably 21° or more, and more preferably 22° or more. This can be expected to improve the handleability of the powder.
[0041] (Measurement of Angle of Repose and Angle of Collapse Step A)
[0042] The measurement procedure A of the angle of repose and the angle of collapse of the inorganic powder is as follows.
[0043] A funnel with an outlet diameter of 0.5 cm was installed at a height of 15 cm from a horizontal plate provided on the powder tester.
[0044] The inorganic powder is continuously supplied from a vertical direction onto the surface of the horizontal plate via a hopper to form a conical deposit that maintains a constant shape.
[0045] Using a protractor, the elevation angle between the side surface of the conical deposit and the surface of the horizontal plate was determined and taken as the repose angle (°).
[0046] Next, a weight of 110 g was dropped from a height of 18 cm three times to apply impact to the horizontal plate. Then, using a protractor, the elevation angle between the side surface of the conical deposit and the surface of the horizontal plate was determined and taken as the collapse angle (°).
[0047] The degree of compression of the inorganic powder was calculated based on ((P-A) / P)×100 using the loose bulk density (A) and the tapped bulk density (P) obtained according to the following procedure B.
[0048] The upper limit of the degree of compression of the inorganic powder is, for example, 44% or less, preferably 43% or less, and more preferably 42% or less. This can be expected to improve the mixing properties of the inorganic powder and the resin.
[0049] The lower limit of the degree of compression of the inorganic powder is, for example, 30% or more, preferably 31% or more, and more preferably 32% or more. This can be expected to improve the handling properties of the powder.
[0050] The upper limit of the tapped bulk density (P) of the inorganic powder is, for example, 2.3 g / cm 3 Below, preferably 2.2 g / cm 3 Below, more preferably 2.1 g / cm 3 Thereby, the compactness is improved, and it is possible to improve the strength of the resin composition.
[0051] The lower limit of the tapped bulk density (P) of the inorganic powder is, for example, 1.5 g / cm 3 Above, preferably 1.6 g / cm 3 More preferably, 1.7 g / cm 3 This makes it possible to improve the handleability of the powder.
[0052] (Measurement step B of tapped bulk density and loose bulk density)
[0053] The inorganic powder is naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup to prepare a full cup in the shape of a mountain.
[0054] Next, the portion of the cup that is filled in a mountain shape is scraped off without shaking it, and the mass (g) of the inorganic powder filled in the cup is measured to calculate the loose bulk density (g / cm 3 ).
[0055] On the other hand, for a cup filled with a mountain shape, after vibrating it 180 times in the up and down direction (stroke length 2 cm, 1 second / time), the part exceeding the upper surface of the cup was scraped off, and the mass (g) of the inorganic powder filled in the cup was measured to calculate the tapped bulk density (g / cm 3 ).
[0056] The volume frequency particle size distribution of the inorganic powder was measured by a wet laser diffraction scattering method, and in the volume frequency particle size distribution, the particle size at which the cumulative value was 10% was defined as D 10 The particle size with a cumulative value of 50% is set as D 50 The particle size with a cumulative value of 97% is set as D 97 .
[0057] (D 97 -D 10 ) / D 50 The lower limit of is, for example, 4 or more, preferably 5 or more, and more preferably 6 or more. If the particle size distribution becomes too narrow or D 50 If it becomes too large, the fluidity and filling properties of the powder itself may deteriorate.
[0058] (D 97 -D 10 ) / D 50 The upper limit of is, for example, 30 or less, preferably 25 or less, and more preferably 20 or less. 50 It will not become too small but will be in an appropriate range, which can improve the fluidity and filling properties of the powder itself.
[0059] D 50 -D 10 The upper limit of is, for example, 17 μm or less, preferably 16 μm or less, and more preferably 15 μm or less. This ensures appropriate fluidity, thermal conductivity, and the like.
[0060] D 50 -D 10 The lower limit of is, for example, 0.5 μm or more, preferably 1 μm or more, and more preferably 2 μm or more. Thus, filling properties can be ensured.
[0061] The particle size distribution of inorganic powder is a value based on particle size measurement using a laser diffraction light scattering method, and can be measured, for example, using "Model LS-13-230" (manufactured by Beckman Coulter) as a particle size distribution measuring machine. During the measurement, water is used as a solvent, and as a pretreatment, a homogenizer is used to apply an output of 200 W for dispersion treatment for 1 minute. In addition, it is prepared so that the PIDS (Polarization Intensity Differential Scattering) concentration is 45-55%. It should be noted that the refractive index of water used is 1.33, and the refractive index of the powder takes into account the refractive index of the material of the powder. For example, amorphous silica is measured at a refractive index of 1.50, and aluminum oxide is measured at a refractive index of 1.68.
[0062] In the present embodiment, the angle of repose, angle of collapse, bulk density and degree of compression can be controlled by, for example, appropriately selecting the type and amount of each component contained in the inorganic powder, the method for preparing the inorganic powder, etc. Among them, for example, appropriate storage treatment of the alumina powder and / or silica powder just after being captured, appropriate adjustment of the opening of these powders during classification treatment, and use of spherical alumina powder and spherical silica powder of different particle sizes can be cited as factors for setting the angle of repose, angle of collapse, bulk density and degree of compression to the desired numerical range.
[0063] The inorganic powder according to this embodiment will be described in detail.
[0064] The spherical alumina powder and spherical silica powder contained in the inorganic powder are also called molten spherical particles, and are produced by feeding the raw material powder into a high-temperature flame formed by the combustion reaction of the combustible gas and the combustion-supporting gas, and melting and sphericalizing at a temperature above the melting point. If necessary, the molten spherical particles obtained in this way can also be classified and sieved.
[0065] For example, the inorganic powder can be obtained by separately producing a spherical alumina powder and a spherical silica powder and mixing them.
[0066] An example of a schematic diagram of a thermal spraying apparatus for producing molten spherical particles is shown in FIG. Figure 1 .
[0067] Figure 1 The thermal spraying device 100 is composed of a melting furnace 2 provided with a burner 1, a cyclone separator 4 for classifying molten spherical particles generated by high-temperature exhaust gas of the flame through suction by a blower 9, and a bag filter 8 for recovering fine powder that cannot be captured by the cyclone separator 4.
[0068] The melting furnace 2 is constituted by a vertical furnace body, but is not limited thereto, and may be a so-called horizontal furnace or a tilted furnace which is placed horizontally and ejects flames in the horizontal direction.
[0069] The high-temperature exhaust gas is cooled by pipes 3 and 5 provided with water-cooling jackets.
[0070] The blower 9 may be connected to a suction gas amount control valve and a gas exhaust port (not shown).
[0071] A collected powder extraction device (not shown) may be connected to the lower parts of the melting furnace 2, the cyclone separator 4, and the bag filter 8.
[0072] The classification can be performed using known equipment such as a gravity settling chamber, a cyclone separator, a classifier having rotary blades, etc. The classification operation can be incorporated into the conveying process of the molten spheroidized product, or can be performed in another pipeline after collectively capturing the molten spheroidized product.
[0073] As the combustible gas, for example, one or more of acetylene, propane, butane, etc. can be used, but propane, butane, or a mixed gas thereof having a relatively low calorific value is preferred.
[0074] As the combustion-supporting gas, for example, a gas containing oxygen can be used. Generally speaking, it is cheap and most preferred to use pure oxygen of more than 99 mass %. In order to reduce the calorific value of the gas, an inert gas such as air or argon can also be mixed into the combustion-supporting gas.
[0075] The alumina raw material powder as the raw material powder may have an average particle size of 3 to 70 μm, for example. The aluminum hydroxide powder may be supplied to the high temperature flame in a dry process or in a wet process by slurrying with water or the like.
[0076] The silica raw material powder used as the raw material powder may be a powder obtained by adjusting a siliceous raw material such as crystal or natural silica to have a particle size composition in which particles of 1 μm or less account for 15 to 50% and particles of 5 μm or greater account for 50 to 80%.
[0077] The content of the spherical silica powder in the inorganic powder is, for example, 3 to 30 mass %, preferably 3 to 20 mass %, and more preferably 3 to 10 mass % in 100 mass % of the total of the spherical alumina powder and the spherical silica powder.
[0078] The spherical silicon dioxide powder may be amorphous and / or crystalline.
[0079] The amorphous rate of the spherical silica powder, for example, measured by the following method, is preferably 95% or more, and more preferably 97% or more. The amorphous rate is determined by the intensity ratio of a specific diffraction peak by using a powder X-ray diffraction device (e.g., RIGAKU company trade name "Model MiniFlex"), and performing X-ray diffraction analysis in the range of 26° to 27.5° of CuKα rays. In the case of siliceous powder, crystalline silica has a main peak at 26.7°, but there is no peak in amorphous silica. When amorphous silica and crystalline silica are mixed, a peak height of 26.7° corresponding to the proportion of crystalline silica can be obtained. Therefore, the crystalline silica mixing ratio is calculated based on the ratio of the X-ray intensity of the sample to the X-ray intensity of the crystalline silica standard sample (X-ray diffraction intensity of the sample / X-ray diffraction intensity of crystalline silica), and the amorphous rate is calculated by the formula Amorphous rate (%) = (1-crystalline silica mixing ratio) × 100.
[0080] As for the degree of "sphericity" of the spherical alumina powder and / or spherical silica powder, for example, it is preferred that the average sphericity of particles having a particle size smaller than 75% (d75) of the cumulative particle size distribution is 0.90 or more, and the average sphericity of particles having a particle size greater than d75 is 0.85 or more. Generally speaking, if the average sphericity of the spherical silica powder is increased, the fluidity tends to be improved, and in particular, by setting the average sphericity of coarse particles having a particle size greater than d75 to 0.85 or more, the effect of the present embodiment can be further improved.
[0081] The average sphericity can be measured by importing particle images taken with a stereo microscope (e.g., model "SMZ-10" manufactured by Nikon), a scanning electron microscope, etc. into an image analyzer (e.g., manufactured by Nippon Avionics, etc.) in the following manner. That is, the projected area (A) and circumference (PM) of the particle are measured from the photograph. If the area of the true circle corresponding to the circumference (PM) is set to (B), the true roundness of the particle can be expressed as A / B. Therefore, if a true circle with the same circumference as the circumference (PM) of the sample particle is assumed, then since PM = 2πr, B = πr 2 , so B = π × (PM / 2π) 2 The sphericity of each particle can be expressed as: sphericity = A / B = A × 4π / (PM) 2 The roundness of any 200 particles thus obtained is calculated, and the average value thereof is taken as the average sphericity.
[0082] It should be noted that as a method for measuring the circularity other than the above, the circularity of each particle can be quantitatively and automatically measured using a particle image analyzer (e.g., model "FPIA-1000" manufactured by Sysmex Corporation) and converted using the formula circularity = (circularity)2.
[0083] A material obtained by blending the inorganic powder of the present invention with a resin composition can be suitably used as a resin molding material.
[0084] Next, the resin composition according to the present embodiment will be described.
[0085] The resin composition contains a resin, a known resin additive, and the like in addition to the inorganic powder of the present invention.
[0086] In the resin composition, the inorganic powder can be used alone or mixed with other fillers. The resin composition can contain 10 to 99% by mass of the inorganic powder, or can contain 10 to 99% by mass of a mixed inorganic powder containing the inorganic powder and other fillers. In addition, in the mixed inorganic powder, the content of the other fillers is, for example, 1 to 20% by mass, or 3 to 15% by mass, relative to 100% by mass of the inorganic powder.
[0087] In addition, in this specification, unless otherwise specified, "to" means that the upper limit value and the lower limit value are included.
[0088] Examples of other fillers include titanium dioxide, silicon nitride, aluminum nitride, silicon carbide, talc, calcium carbonate, etc. The other fillers have an average particle size of about 5 to 100 μm, and there are no particular restrictions on the particle size composition and shape.
[0089] Examples of the resin include epoxy resins, silicone resins, phenolic resins, melamine resins, urea-formaldehyde resins, unsaturated polyesters, fluororesins, polyamides such as polyimide, polyamide-imide, and polyether-imide, polyesters such as polybutylene terephthalate and polyethylene terephthalate, polyphenylene sulfide, fully aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile acrylic rubber styrene) resins, and AES (acrylonitrile, ethylene, propylene, diene rubber-styrene) resins, etc. These resins may be used alone or in combination of two or more thereof.
[0090] The resin composition can be produced by, for example, mixing the raw material components in a predetermined quantitative ratio using a mixer, Henschel mixer or the like, kneading the mixture using a heating roll, a kneader, a single-screw or twin-screw extruder or the like, and then pulverizing the mixture after cooling.
[0091] The embodiments of the present invention have been described above, but these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are included in the present invention.
[0092] Example
[0093] Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited at all to the description of these Examples.
[0094] <Manufacturing of inorganic powder>
[0095] use Figure 1 The thermal spraying apparatus 100 shown is used to produce various spherical alumina powders and spherical silica powders.
[0096] Figure 1 The thermal spraying device 100 shown includes a melting furnace 2 , a burner 1 provided above the melting furnace 2 , and a collection system pipeline directly connected to a cyclone separator 4 and a bag filter 8 provided below the melting furnace 2 .
[0097] The burner 1 has a double-tube structure capable of forming an inner flame and an outer flame, and is disposed on the top of the melting furnace 2, and is connected to a combustible gas supply pipe 11, a combustion-supporting gas supply pipe 12, and a raw material supply pipe 13 respectively.
[0098] In the melting furnace 2, the raw material powder is supplied to the high temperature flame from the raw material supply pipe 13 to be melted, and spheroidized molten spherical particles can be formed. The molten spherical particles passing through the melting furnace 2 are sucked by the blower 9 together with the combustion exhaust gas, move with the air in the pipes 3 and 5, and are classified and captured by the cyclone separator 4 or the bag filter 8.
[0099] (Example 1)
[0100] ·Manufacturing of spherical alumina powder
[0101] Using the thermal spraying apparatus 100 , LPG as a combustible gas is supplied from the combustible gas supply pipe 11 , and air in the atmosphere is supplied from the combustion-supporting gas supply pipe 12 as a combustion-supporting gas. In the burner 1 , a high-temperature flame is formed by combustion of LPG and oxygen.
[0102] Secondary air is supplied to the cyclone 4 by a rotary valve (not shown) provided in the pipe 3. The secondary air is air heated in the melting furnace 2. The lower opening of the cyclone 4 is set to 100%.
[0103] As the raw material powder, an average particle size (D 50) Alumina powder having a maximum value in the range of 2 to 45 μm. The molten spherical particles captured by the bag filter 8 are recovered as spherical alumina powder.
[0104] ·Manufacturing of spherical silica powder
[0105] As the raw material powder, an average particle size (D 50 ) is a natural silica powder of 5 μm, and the carrier gas as the raw material is set to 10Nm 3 / hr, and the supply rate of combustible gas to the burner is set to 10Nm 3 / hr, and set the supply rate of combustion-supporting gas to 25Nm 3 / hr, except for this, the production process is the same as that of the spherical alumina powder.
[0106] The molten spherical particles collected by the bag filter 8 are taken as the average particle size (D 50 ) is recovered as spherical silica powder with a size of 0.3 μm.
[0107] ·Manufacturing of inorganic powder
[0108] The spherical silica powder was stored in an aluminum bag (manufactured by a Japanese company, LAMIZIP AL) at a humidity of 60 to 80% and a temperature of 20 to 30° C. for 28 days (storage treatment) immediately after being captured. The spherical silica powder just after the aluminum bag was opened and taken out was mixed with the spherical alumina powder just after being produced at a mass ratio of 90:10 to obtain an inorganic powder.
[0109] (Examples 2 to 4)
[0110] In the production of the spherical alumina powder, an inorganic powder was obtained by using the obtained spherical alumina powder in the same manner as in Example 1 except that the lower opening was changed to 20%, 25%, and 35%, respectively.
[0111] (Comparative Example 1)
[0112] The spherical silica powder was not mixed, and the above-mentioned spherical alumina powder was used as the inorganic powder.
[0113] (Comparative Example 2)
[0114] In the production of inorganic powders, the conditions of the classification process are changed to obtain the average particle size (D 50 The obtained spherical silica powder and the above-mentioned spherical alumina powder were mixed at a mass ratio of 90:10 to obtain an inorganic powder.
[0115] (Comparative Example 3)
[0116] The same procedure as in Example 1 was carried out except that no secondary air was supplied and the lower opening of the cyclone 4 was set to 0%, and an inorganic powder was obtained using the obtained spherical alumina powder.
[0117] (Comparative Example 4)
[0118] In the production of the spherical silica powder, an inorganic powder was obtained by using the obtained silica powder in the same manner as in Example 3 except that the spherical silica powder was not stored in an aluminum bag.
[0119]
[0120] <Loose bulk density, tapped bulk density>
[0121] The loose bulk density and tapped bulk density of the obtained inorganic powder were measured at room temperature of 25° C. and humidity of 55% using a powder tester (PT-E model, manufactured by Hosokawa Micron Co., Ltd.).
[0122] The specific steps are as follows.
[0123] The inorganic powder as the measurement sample is naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup to prepare a full cup in the shape of a mountain.
[0124] Next, the portion of the cup that is filled in a mountain shape is scraped off without shaking it, and the mass (g) of the inorganic powder filled in the cup is measured to calculate the loose bulk density (g / cm 3 ).
[0125] On the other hand, for the cup filled with a mountain shape, after vibrating 180 times in the up and down direction (stroke length 2 cm, 1 second / time), the part exceeding the upper surface of the cup was scraped off, and the mass (g) of the inorganic powder filled in the cup was measured to calculate the tapped bulk density (g / cm 3 ).
[0126] When the loose bulk density obtained by the above-mentioned procedure is defined as A and the tapped bulk density is defined as P, the compression degree (%) is determined based on the formula: ((P-A) / P)×100.
[0127] <Angle of repose, angle of collapse>
[0128] The obtained inorganic powder was measured for its repose angle and collapse angle using a powder tester (PT-E model, manufactured by Hosokawa Micron Co., Ltd.) at room temperature of 25° C. and humidity of 65%.
[0129] The specific steps are as follows.
[0130] A funnel with an outlet diameter of 0.5 cm was installed at a height of 15 cm from a horizontal plate provided on the powder tester.
[0131] The inorganic powder is continuously supplied from the vertical direction onto the surface of the horizontal plate via the hopper, forming a conical deposit that maintains a constant shape.
[0132] Using a protractor, the elevation angle between the side surface of the conical deposit and the surface of the horizontal plate was determined and taken as the repose angle (°).
[0133] Next, a weight of 110 g was dropped from a height of 18 cm three times to apply impact to the horizontal plate. Then, using a protractor, the elevation angle between the side surface of the conical deposit and the surface of the horizontal plate was determined and taken as the collapse angle (°).
[0134] <Particle size distribution>
[0135] The obtained inorganic powder was subjected to a volume frequency particle size distribution by a wet laser diffraction scattering method using a particle size distribution measuring device (manufactured by Beckman Coulter, LS-13-230). Water was used as a solvent, and as a pretreatment, a homogenizer was used to apply an output of 200 W for 1 minute for dispersion treatment. In addition, the PIDS (Polarization Intensity Differential Scattering) concentration was prepared and measured in a manner of 45 to 55%.
[0136] Based on the obtained volume frequency particle size distribution, calculate the particle size D with a cumulative value of X%. X .
[0137] <Flowability of resin composition>
[0138] 90 parts by mass of each of the obtained inorganic powders and a biphenyl epoxy resin (Japan Epoxy 5.5 parts by mass of phenolic resin (YX-4000HK manufactured by Resin Co., Ltd.), 4.8 parts by mass of phenolic resin (phenol aralkyl resin, MEHC-7800S manufactured by Meiwa Chemicals Co., Ltd.), 0.15 parts by mass of triphenylphosphine (manufactured by Hokuko Chemical Industry Co., Ltd.: TPP) and 0.35 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: KBM-573) were mixed under the conditions of room temperature and a rotation speed of 2000 rpm, and the obtained mixture was heated and kneaded in a co-rotating intermeshing twin-screw extruder (screw diameter D = 25 mm, L / D = 10.2, blade rotation speed 50 to 120 rpm, ejection amount 3.0 kg / Hr, kneaded material temperature 98 to 100°C) to obtain a resin composition.
[0139] The obtained resin composition was used and molded using a spiral flow mold according to EMMI-1-66 (Epoxy Molding Material Institute; Society of Plastic Industry) at a mold temperature of 175° C., a molding pressure of 7.4 MPa, and a holding time of 90 seconds.
[0140] The resin composition having a spiral flow of 200 cm or more was evaluated as good, and the resin composition having a spiral flow of less than 200 cm was evaluated as poor.
[0141] The inorganic powders of Examples 1 to 4 showed a result that the fluidity of the resin composition could be improved compared with Comparative Examples 1 to 4.
[0142] This application claims the benefit of priority based on Japanese patent application No. 2022-018507, filed on February 9, 2022, the disclosure of which is incorporated herein in its entirety.
[0143] Explanation of symbols
[0144] 1 Burner
[0145] 2 Melting furnace
[0146] 3Piping
[0147] 4 Cyclone separator
[0148] 5 piping
[0149] 8-Bag Filter
[0150] 9 Blower
[0151] 11 Combustible gas supply pipe
[0152] 12 Combustion-supporting gas supply pipe
[0153] 13Raw material supply pipe
[0154] 100 Thermal Spraying Equipment
Claims
1. An inorganic powder comprising spherical alumina powder and spherical silica powder, At room temperature of 25°C and humidity of 65%, the angle of repose measured according to step A below is 35° to 47°; Step A: Install a funnel with an outlet diameter of 0.5 cm at a height of 15 cm from the horizontal plate set on the powder tester; The inorganic powder is continuously supplied from a vertical direction onto the surface of the horizontal plate through a funnel to form a conical deposit that maintains a certain shape; Using a protractor, find the angle of elevation between the side of the conical deposit and the surface of the horizontal plate and use it as the angle of repose in degrees; Next, a weight of 110 g was dropped from a height of 18 cm three times to impact the horizontal plate, and then the angle of elevation between the side of the conical deposit and the surface of the horizontal plate was calculated using a protractor as the collapse angle in degrees.
2. The inorganic powder according to claim 1, Under the conditions of room temperature of 25°C and humidity of 65%, the collapse angle measured according to step A is 20° to 37°.
3. The inorganic powder according to claim 1 or 2, At room temperature of 25°C and humidity of 55%, the tapped bulk density measured according to step B below is 1.5 g / cm 3 ~2.3g / cm 3 ; Step B: The inorganic powder is naturally dropped from a height of 25 cm at a rate of 5 to 10 g per minute. 3 The inside of the measuring cup is filled with water until it overflows from the cup, and a full cup is prepared; Next, for the cup filled with a mountain shape, the part that exceeds the upper surface of the cup is scraped off without shaking it, and the mass of the inorganic powder filled in the cup is measured in g, and the loose bulk density is calculated in g / cm 3 ; On the other hand, for a cup filled with a mountain shape, after being vibrated 180 times in the up and down direction with a stroke length of 2 cm and 1 second per time, the part exceeding the upper surface of the cup was scraped off, and then the mass of the inorganic powder filled in the cup was measured in g, and the tapped bulk density was calculated in g / cm 3 .
4. The inorganic powder according to claim 3, When the loose bulk density measured in step B is defined as A and the tapped bulk density is defined as P, The compression degree calculated based on ((P-A) / P)×100 is 30% to 44%.
5. The inorganic powder according to any one of claims 1 to 4, In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 10% is defined as D 10 The particle size with a cumulative value of 50% is set as D 50 The particle size with a cumulative value of 97% is set as D 97 hour, (D 97 -D 10 ) / D 50 4 to 30.
6. The inorganic powder according to any one of claims 1 to 5, In the volume frequency particle size distribution measured by the laser diffraction scattering method based on the wet method, the particle diameter at which the cumulative value is 10% is defined as D 10 The particle size with a cumulative value of 50% is set as D 50 hour, D 50 -D 10 0.5μm~17μm.
Citation Information
Patent Citations
Spherical alumina powder
JP2013014513A