Method for selectively depositing high-conductivity metal film
Selective deposition of ruthenium seed layers and metal-containing precursors through oxygen-free ruthenium precursors solves the problem of non-selective coverage of high-resistivity materials in microelectronic devices, achieves selective deposition of low resistivity, and reduces through-hole resistance , improving the performance of microelectronic devices.
Patent Information
- Application Number
- CN202380024537.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-03
- Filing Date
- 2023-01-27
- Publication Date
- 2024-10-15
AI Technical Summary
In the manufacturing of microelectronic devices, it is difficult to selectively deposit low-resistivity crystal nucleation layers with existing technology, resulting in high-resistivity metal covering the sidewalls during the non-selective pulse growth process, increasing the overall resistance-capacitance delay of the device. .
Oxygen-free ruthenium precursors are used for selective ruthenium seed layer deposition, and then metal precursors containing tungsten, molybdenum, cobalt, ruthenium or copper are deposited, and vapor deposition technology is used to form a highly conductive ruthenium seed layer at 300°C, and Minimize coverage of insulating surfaces through selective deposition methods.
A highly selective deposition of conductive parts is achieved, significantly reducing through-hole resistance, reducing sidewall coverage of high-resistivity materials, and improving the overall performance of the microelectronic device.
Smart Images

Figure CN118786240A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates generally to the field of vapor deposition. In particular, the present invention relates to the selective deposition of ruthenium-containing precursors followed by bulk deposition of various metals onto microelectronic device substrates.
[0002] Priority claim
[0003] The present invention claims priority to U.S. Provisional Patent No. 63 / 306,287, filed on February 3, 2022, which is incorporated herein by reference. Background Art
[0004] In the manufacture of microelectronic devices, tungsten is typically deposited on titanium nitride barriers. The method involves a nucleation layer deposition using tungsten hexafluoride and a silicon or boron source, followed by a bulk deposition using tungsten hexafluoride and hydrogen as a reducing gas. Disadvantageously, the material in such a nucleation layer is typically very fine-grained and exhibits high resistivity. Additionally, this growth step is non-selective, and as a result, the sidewalls of the device are often also covered with this high-resistivity metal.
[0005] In the process of depositing molybdenum-containing films onto microelectronic device substrates, molybdenum pentachloride and molybdenum oxychloride have been developed for chemical vapor deposition of high purity and low resistivity molybdenum metal. However, molybdenum also generally requires similar non-selective pulsed crystal growth techniques to be deposited onto titanium nitride surfaces at temperatures below about 500°C.
[0006] Therefore, there remains a need to be able to deposit low resistivity nucleus (i.e., seed) layers onto metal surfaces such as titanium nitride with high selectivity to the surrounding dielectric, and thus to enable bulk deposition of materials such as tungsten, molybdenum, cobalt, ruthenium or copper containing metal films.
[0007] For the scaling of integrated semiconductor devices, the resistance of the conductive vias connecting the wiring layers has become an important part of the overall resistance-capacitance (RC) delay in the communication within the integrated device. In order to minimize the resistance of the via, it is necessary to minimize the volume consumed by the higher resistivity barrier, adhesion layer and nucleation layer. One of the methods to fill the entire volume of the via with low resistivity metal is to grow and grow from the metal contact at the bottom of the via to the top instead of growing from the dielectric sidewalls of the via. Therefore, selective deposition is required at these metal contacts. Summary of the invention
[0008] In summary, the present invention provides a method comprising selective ruthenium seed layer deposition using an oxygen-free ruthenium precursor, followed by a bulk deposition of a metal-containing precursor, such as a tungsten, molybdenum, cobalt, ruthenium and / or copper-containing precursor. The ruthenium seed layer deposition is highly selective to the conductive portion of a microelectronic device substrate while minimizing deposition onto insulating surfaces of the microelectronic device substrate. In certain embodiments, the conductive portion of the substrate is selected from titanium nitride, tungsten nitride, tantalum nitride (all conductive nitrides), tungsten, cobalt, molybdenum, aluminum and copper (metal 1 in FIG. 6 ). In certain embodiments, the insulating surface is selected from silicon oxide, silicon nitride and other dielectrics, as well as low-k dielectrics.
[0009] Ruthenium seed layer at 300 °C for the synthesis of p-cymene cyclohexadiene precursor on titanium nitride substrate The thick ruthenium film exhibits an as-deposited resistivity of about 450 μΩ-cm. As shown, this method is also highly selective, thus exhibiting selectivity for conductive portions of the substrate relative to insulating portions of the substrate. This highly conductive seed layer enables bulk deposition of the metals described above. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 Graph showing the self-limiting deposition and deposition selectivity of titanium nitride relative to SiO2 as described in Example 1. The deposition selectivity was shown to be 94% at 5 angstroms of ruthenium.
[0011] Figure 2 Graph showing the as-deposited resistivity of ruthenium films on titanium nitride at various thicknesses.
[0012] Figure 3 Deposited on a titanium nitride substrate Scanning electron micrograph (SEM) top view of a thick ruthenium layer. (10 minutes, 446.1 μΩ-cm)
[0013] Figure 4 To illustrate the self-limiting deposition and selectivity of titanium nitride relative to silicon dioxide for the deposition of ethylbenzyl(1-ethyl-1,4-cyclohexadienyl)Ru with H2 as a co-reactant as described in Example 2.
[0014] Figure 5 Graph showing the as-deposited resistivity of ruthenium on titanium dioxide and silicon dioxide at various thicknesses according to Example 2.
[0015] Figure 6a is an illustration of a problem addressed in the art, where non-selective deposition often creates voids when filling vias with "Metal 2" as depicted. Figure 6bis a diagrammatic representation of a solution to this problem that is believed to be achievable by the method of the present invention, namely a through-hole structure without such voids. Figure 6c In order to selectively deposit Metal 2 onto “Metal 1 ” in a highly selective manner, an illustration of filling the via with Metal 2 from the bottom up is thus achieved. DETAILED DESCRIPTION
[0016] As used in this specification and the following claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. As used in this specification and the following claims, the term "or" is generally employed in its sense including "and / or" unless the context clearly dictates otherwise.
[0017] The term "about" generally refers to a numerical range that is considered equivalent to the recited value (eg, having the same function or result). In many cases, the term "about" may include numbers that are rounded to the nearest significant figure.
[0018] The recitation of numerical ranges using endpoints includes all numbers subsumed within that range (eg, 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, and 5).
[0019] In a first aspect, the present invention provides a method of depositing a metal-containing film onto a microelectronic device substrate, wherein the metal is selected from the group consisting of tungsten, molybdenum, cobalt, ruthenium, and copper, and wherein the substrate is selected from the group consisting of titanium nitride, tungsten nitride, tantalum nitride, niobium nitride, tungsten, molybdenum, cobalt, and copper, the method comprising:
[0020] a. In the presence of a reducing gas and under vapor deposition conditions, introducing an oxygen-free ruthenium precursor material into a reaction zone containing the substrate until the thickness of the ruthenium-containing film is about 3 to about then
[0021] b. Under vapor deposition conditions, introducing a tungsten-, molybdenum-, cobalt-, ruthenium- or copper-containing metal precursor into the reaction zone until a tungsten-, molybdenum-, cobalt-, ruthenium- or copper-containing metal film having a desired thickness is obtained.
[0022] The method of the present invention enables the bulk deposition of certain metal-containing films onto a substrate that already has a highly conductive ruthenium seed layer (step a). This selective formation and highly conductive ruthenium layer can be deposited using the methods described in U.S. Patent Publications 2020 / 0149155 and 2020 / 0157680 (which are incorporated herein by reference). As noted, in this step a., an oxygen-free ruthenium precursor material is utilized. In one embodiment, this oxygen-free ruthenium precursor is selected from:
[0023]
[0024] They are referred to herein as "para-isopropylbenzene CHD Ru" and "EBECHD Ru", respectively.
[0025] In the formation of a thickness of about 3 to about After forming a ruthenium seed layer, a metal precursor containing tungsten, molybdenum, cobalt, ruthenium or copper is introduced using step b. At this point, the ruthenium precursor used in step b can be an oxygen-free ruthenium precursor or an oxygen-containing ruthenium precursor selected from known ruthenium precursor materials in either case. In the case where the ruthenium precursor contains oxygen, it may be necessary to utilize a reducing gas as a co-reactant in order to properly deposit the desired metal (i.e., in a zero oxidation state). Exemplary reducing gases include hydrogen, ammonia, hydrazine, methylhydrazine, tert-butylhydrazine, 1,2-dimethylhydrazine, and 1,1-dimethylhydrazine.
[0026] In certain embodiments, vapor deposition conditions include reaction conditions known as chemical vapor deposition, pulsed chemical vapor deposition, and atomic layer deposition. In the case of pulsed chemical vapor deposition, a series of alternating pulses of a precursor composition and a co-reactant may be used to increase the film thickness to a desired index with or without an intermediate (inert gas) purge step.
[0027] In certain embodiments, the pulse time of the precursor compound described above (i.e., the duration of exposure of the precursor to the substrate) is in the range of between about 1 second and 30 seconds. When a purge step is utilized, the duration is about 1 to 20 seconds or 1 to 30 seconds. In other embodiments, the pulse time of the co-reactant is in the range of 5 to 60 seconds.
[0028] In one embodiment, vapor deposition conditions for step a, deposition of a ruthenium seed layer, include a temperature of about 100°C to about 400°C or about 200°C to about 350°C in the reaction zone, and at a pressure of about 1 Torr to about 100 Torr.
[0029] Step b. Bulk deposition of metal films depends on the specific metal precursor chosen and will involve a variety of temperatures, pressures, and co-reactant gases.
[0030] For example, U.S. Patent Publication No. 2021 / 0062331, incorporated herein by reference, describes temperatures of about 250°C to about 750°C for molybdenum hexacarbonyl and tungsten carbonyl.
[0031] For precursors such as MoCl5, MoOCl4, MoO2Cl2, WCl6, WCl5, WOCl4, and WO2Cl3, U.S. Patent Publication No. 2020 / 0199743 describes temperatures below about 480°C and pressures less than about 100 Torr.
[0032] For various ruthenium precursors, the vapor deposition temperature is typically from about 100°C to about 500°C, and the pressure is typically from about 10 mTorr to about 30 Torr.
[0033] For various cobalt precursors, the vapor deposition temperature is typically from about 70°C to about 480°C, and the pressure is typically from about 0.2 Torr to about 760 Torr.
[0034] For various copper precursors, the vapor deposition temperature is typically from about 40°C to about 200°C, and the pressure is typically from about 0.2 to about 30 Torr.
[0035] In one embodiment, the ruthenium-containing precursor compound in step a or step b is selected from one or more compounds selected from the following:
[0036]
[0037]
[0038]
[0039] Wherein R is selected from C1-C4 alkyl.
[0040] In one embodiment, R is tert-butyl.
[0041] The precursor composition comprising at least one compound selected from the above can be used to form a low resistivity ruthenium seed film on various surfaces. In one embodiment, in the above step (a), the ruthenium seed layer is formed using a chemical vapor deposition technique.
[0042] In one embodiment, the tungsten, molybdenum, cobalt, ruthenium or copper metal precursor in step (b) is selected from
[0043] a. Molybdenum precursors, such as MoCl5, MoOCl4 and MoO2Cl2; Mo(CO)6, MoH2( i PrCp)2;( i Pr = isopropyl; Cp = cyclopentadienyl)
[0044] b. Tungsten precursors, such as WF6 and W(tert-butyl-N)2(N(CH3)2)2; WCl5 and WCl6, WOCl4; W(CO)6, WH2( i PrCp)2;
[0045] c. Cobalt precursors such as Co(tert-butyl-NCHCHN-tert-butyl)2, Co2(CO)6(HCCCF3) and Co2(CO)6(HCC(CH3)3). Additional cobalt precursors can be found in Alain E. Kaloyeros et al., "Cobalt Thin Films: Trends in Processing Technologies and Emerging Applications", ECS Journal of Solid State Science and Technology, 8(2) P119-P152 (2019); and Seong Ho Han et al., "New Heteroleptic Cobalt Precursors for Deposition of Cobalt-based Thin Films", ACS Omega, http: / / pubs.acs.org / journal / acsodf ; and U.S. Patent No. 10,872,770 and U.S. Patent Publication No. 2018 / 044788 (incorporated herein by reference); and
[0046] d. Copper precursors, such as copper (I) amidine and copper (I) guanidine precursors, such as 2-methoxy-1,3-diisopropyl copper (I) amidine; 2-ethoxy-1,3-diisopropyl copper (I) amidine; 2-butoxy-1,3-diisopropyl copper (I) amidine; 2-isopropyl-1,3-diisopropyl copper (I) amidine; 2-dimethylamino-1,3-diisopropyl copper (I) amidine; (see U.S. Patent Publication Nos. 2005 / 0281952 and WO2007 / 1422700, which are incorporated herein by reference). In one embodiment, the copper precursor is N',N"-diisopropyl-N,N-dimethylguanidine copper (I), which is referred to as "CuDMAPA" hereinafter. See also Peter G. Gordon et al. 2015 ECS J. Solid State Sci. Technol. 4N3188; and U.S. Pat. Nos. 7,964,746 and 7,858,525 and U.S. Pat. Publication No. 2008 / 0281476, which are incorporated herein by reference.
[0047] The desired microelectronic device substrate can be placed in the reaction zone in any suitable manner, such as in single wafer CVD or ALD, or in a furnace containing multiple wafers.
[0048] In an alternative, the process of the present invention may be performed as an ALD or ALD-like process. As used herein, the term "ALD or ALD-like" refers to a process in which (i) each reactant, including a precursor composition containing a compound described herein, a co-reactant is sequentially introduced into a reactor, such as a single wafer ALD reactor, a semi-batch ALD reactor, or a batch furnace ALD reactor, or (ii) each reactant is exposed to the substrate or microelectronic device surface by moving or rotating the substrate to a different part of the reactor, and each part is separated by an inert gas curtain, i.e., a spatial ALD reactor or a roll-to-roll ALD reactor. In certain embodiments, the thickness of the resulting bulk ALD metal film may be from about 0.5 nm to about 40 nm.
[0049] The deposition method disclosed herein may involve one or more purge gases. The purge gas used to purge unconsumed reactants and / or reaction byproducts is an inert gas or counter-reactant that does not react with the precursor composition. Exemplary purge gases include, but are not limited to, argon, nitrogen, helium, neon, and mixtures thereof. In certain embodiments, a purge gas such as Ar is supplied to the reactor at a flow rate of about 10 sccm to about 2000 sccm for about 0.1 to 1000 seconds to purge unreacted materials and any byproducts that may remain in the reactor. Such purge gases may also be used as an inert carrier gas for either or both of the precursor composition and the co-reactant.
[0050] Energy is applied to the precursor composition and co-reactants in the reaction zone to induce a reaction and form a film on the surface of the microelectronic device. Such energy may be provided by, but is not limited to, heat, pulsed heat, plasma, pulsed plasma, helicon plasma, high density plasma, inductively coupled plasma, X-ray, electron beam, photon, remote plasma methods, and combinations thereof. In certain embodiments, a secondary RF frequency source may be used to modify the plasma characteristics at the substrate surface. In embodiments where deposition involves plasma, the plasma generation process may include a direct plasma generation process, in which the plasma is generated directly in the reactor; or alternatively, a remote plasma generation process, in which the plasma is generated 'remotely' from the reaction zone and substrate, and the plasma is supplied to the reactor.
[0051] As used herein, the term "microelectronic device" corresponds to a semiconductor substrate fabricated for microelectronic, integrated circuit or computer chip applications, including 3D NAND structures, flat panel displays, and microelectromechanical systems (MEMS). It should be understood that the term "microelectronic device" is not intended to be limiting in any way and includes any substrate that includes negative channel metal oxide semiconductor (nMOS) and / or positive channel metal oxide semiconductor (pMOS) transistors and will eventually become a microelectronic device or microelectronic assembly. Such a microelectronic device contains at least one substrate which may be selected from, for example, tin, SiO2, Si3N4, OSG, FSG, tin carbide, hydrogenated tin carbide, tin nitride, hydrogenated tin nitride, tin carbonitride, hydrogenated tin carbonitride, boron nitride, antireflective coatings, photoresists, germanium, germanium-containing, boron-containing, Ga / As, flexible substrates, porous inorganic materials, metals (such as copper and aluminum), and diffusion barrier layers such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W, or WN.
[0052] Example -
[0053] Example 1 - CVD Deposition of p-Isopropylbenzene (1,3-cyclohexadiene)Ru and H2 Co-Reactant
[0054] Ru metal was deposited using 4 μmol / min cymene CHD Ru and 0.4 liters / min (lpm) H2 at 300°C and 30 Torr.
[0055] In this example, ruthenium metal was deposited at 300°C and 30 Torr. Figure 1 The data for this example are presented in , illustrating the excellent selectivity of deposition on titanium nitride compared to silicon dioxide.
[0056] Example 2 - Ethylbenzyl (1-ethyl-1,4-cyclohexadienyl) Ru [EBECHD Ru] and H2 co-reactant CVD deposition
[0057] Ruthenium films were deposited at 300° C. and 30 Torr using ethylbenzyl(1-ethyl-1,4-cyclohexadienyl)Ru (4 μmol / min flow rate) as a precursor and 0.4 lpm H 2 co-reactant. Figure 4 The data for this example are presented in , demonstrating the self-limiting deposition and selectivity for titanium nitride relative to silicon dioxide.
[0058] Example 3 (Second step is prophetic)
[0059] In the first step, under the following conditions Ru was selectively deposited onto the TiN region of the substrate at 300°C and 30 Torr using 4 μmol / min CHD Ru in cymene and 0.4 liters / min (lpm) H2 for 3 minutes of deposition time. (The surrounding dielectric surface has < Ru. )
[0060] In the second step, the substrate was held at 400°C in 60 Torr H2 flowing at 2 standard liters per minute (slm). MoCl5 vapor was delivered from a ProE-Vap ampoule held at 105°C with 300 sccm Ar carrier gas. The deposition was completed in about 10 minutes. Mo metal, where the resistivity is <30 microohm-cm (μΩ-cm).
[0061] Example 4a (Ru deposition)
[0062] In this example, under the following conditions Ru was selectively deposited onto the TiN region of the substrate at 300°C and 30 Torr using 4 μmol / min CHD Ru in cymene and 0.4 liters / min (lpm) H2 for 3 minutes of deposition time. (The surrounding dielectric surface has < Ru. )
[0063] Example 4b (Cu deposition on sputtered Ru surface)
[0064] In this example, under the following conditions Cu was selectively deposited onto the Ru layer: The substrate was maintained at 65°C with the process pressure controlled at 1 Torr. There was a constant flow of 470 sccm H2 and 490 sccm Ar. CuDMAPA vapor was delivered in pulses 18 s long from a ProE-Vap ampoule maintained at 95°C with 95 Torr Ar carrier gas upstream. The Cu precursor flow was stopped for a purge time of 0.5 s. A 150 W DC plasma was ignited for 1.5 s, followed by a 0.05 s post plasma purge. After 550 cycles, the film was Thick, with a resistivity of 5.1 micro-ohm-cm (μΩ-cm).
[0065] Example 5a (Ru deposition)
[0066] In this example, under the following conditions Ru was selectively deposited onto the TiN region of the substrate at 300°C and 30 Torr using 4 μmol / min CHD Ru in cymene and 0.4 liters / min (lpm) H2 for 3 minutes of deposition time. (The surrounding dielectric surface has < Ru. )
[0067] Example 5b (Co deposition on sputtered Ru surface)
[0068] In this example, the substrate was held at 200°C in 30 Torr H2 flowing at 0.5 slm. Ten (10) micromoles / minute of Co(tert-butyl-NCHCHN-tert-butyl)2 vapor was delivered from a vaporizer held at 130°C with 100 sccm He carrier gas. The selective deposition of Co metal, wherein the resistivity is about 12 micro-ohm-centimeters (μΩ-cm).
[0069] aspect
[0070] In a first aspect, the present invention provides a method of depositing a metal-containing film onto a microelectronic device substrate, wherein the metal is selected from the group consisting of tungsten, molybdenum, cobalt, ruthenium, and copper, and wherein the substrate is selected from the group consisting of titanium nitride, tungsten nitride, tantalum nitride, niobium nitride, tungsten, molybdenum, cobalt, and copper, the method comprising:
[0071] a. In the presence of a reducing gas, under vapor deposition conditions, introducing an oxygen-free ruthenium precursor material into a reaction zone containing the substrate until the thickness of the ruthenium-containing film is about 3 to about then
[0072] b. Under vapor deposition conditions, introducing a tungsten-, molybdenum-, cobalt-, ruthenium- or copper-containing metal precursor into the reaction zone until a tungsten-, molybdenum-, cobalt-, ruthenium- or copper-containing metal film having a desired thickness is obtained.
[0073] In a second aspect, the present invention provides the method of the first aspect, wherein the ruthenium precursor material in (a) is introduced into the reaction zone under chemical vapor deposition conditions.
[0074] In a third aspect, the present invention provides the method of the first aspect, wherein a metal precursor containing tungsten, molybdenum, cobalt, ruthenium or copper is introduced into the reaction zone under chemical vapor deposition conditions.
[0075] In a fourth aspect, the present invention provides the method of the first aspect, wherein a metal precursor containing tungsten, molybdenum, cobalt, ruthenium or copper is introduced into the reaction zone under atomic layer deposition or pulsed CVD conditions.
[0076] In a fifth aspect, the present invention provides the method of any one of the first to fourth aspects, wherein the metal precursor containing tungsten, molybdenum, cobalt, ruthenium or copper is selected from
[0077] MoCl5, MoOCl4, MoO2Cl2; Mo(CO)6, MoH2( i PrCp)2;
[0078] WF6, W(tert-butyl-N)2(N(CH3)2)2, WCl5, WCl6 and WOCl4; W(CO)6, WH2( i PrCp)2;
[0079] Co(tert-butyl-NCHCHN-tert-butyl)2, Co2(CO)6(HCCCF3) and Co2(CO)6(HCC(CH3)3);
[0080] 2-Methoxy-1,3-diisopropyl amidine copper(I); 2-ethoxy-1,3-diisopropyl amidine copper(I); 2-tert-butoxy-1,3-diisopropyl amidine copper(I); 2-isopropyl-1,3-diisopropyl amidine copper(I); and 2-dimethylamino-1,3-diisopropyl amidine copper(I).
[0081] In a sixth aspect, the present invention provides a method of any one of the first to fifth aspects, wherein the molybdenum-containing metal precursor is selected from MoCl5, MoOCl4 or MoO2Cl2.
[0082] In a seventh aspect, the present invention provides the method of any one of the first to fourth aspects, wherein the tungsten-containing metal precursor is selected from WF6 and W(tert-butyl-N)2(N(CH3)2)2.
[0083] In an eighth aspect, the present invention provides the method of any one of the first to fourth aspects, wherein the copper-containing metal precursor is N',N"-diisopropyl-N,N-dimethylguanidine copper (I).
[0084] In a ninth aspect, the present invention provides the method of any one of the first to fourth aspects, wherein the ruthenium-containing metal precursor comprises one or more compounds selected from the group consisting of:
[0085]
[0086]
[0087] as well as
[0088]
[0089] Wherein R is selected from C1-C4 alkyl.
[0090] In a tenth aspect, the present invention provides the method of the ninth aspect, wherein R is tert-butyl.
[0091] In an eleventh aspect, the present invention provides the method of any one of the first to tenth aspects, wherein the oxygen-free ruthenium precursor comprises a compound selected from the following formula:
[0092]
[0093] In a twelfth aspect, the present invention provides the method of any one of the first to fourth or ninth aspects, wherein the ruthenium-containing metal precursor comprises a compound selected from the group consisting of:
[0094]
[0095]
[0096] as well as
[0097]
[0098] Wherein R is selected from C1-C4 alkyl.
[0099] In a thirteenth aspect, the present invention provides the method of any one of the first to fourth or ninth aspects, wherein the ruthenium-containing metal precursor comprises one or more compounds selected from the group consisting of:
[0100] as well as
[0101]
[0102] In a fourteenth aspect, the present invention provides the method of any one of the first to twelfth aspects, wherein the ruthenium-containing film of step a. is about A film with a thickness of 1000 Å exhibits a resistivity of about 450 μΩ-cm.
[0103] Therefore, based on the several illustrative embodiments of the present disclosure described, it will be readily apparent to those skilled in the art that other embodiments may be made and used within the scope of the appended claims. The numerous advantages of the present disclosure covered by this document have been set forth in the foregoing description. However, it will be understood that the present disclosure is in many respects merely illustrative. Of course, the scope of the present disclosure is defined in the language in which the appended claims are expressed.
Claims
1. A method of depositing a metal-containing film onto a microelectronic device substrate, wherein the metal is selected from the group consisting of tungsten, molybdenum, cobalt, ruthenium, and copper, and wherein the substrate is selected from the group consisting of titanium nitride, tungsten nitride, tantalum nitride, niobium nitride, tungsten, molybdenum, cobalt, and copper, the method comprising: a. In the presence of a reducing gas and under vapor deposition conditions, introducing an oxygen-free ruthenium precursor material into a reaction zone containing the substrate until the thickness of the ruthenium-containing film is about 3 to about then b. Under vapor deposition conditions, introducing a tungsten-, molybdenum-, cobalt-, ruthenium- or copper-containing metal precursor into the reaction zone until a tungsten-, molybdenum-, cobalt-, ruthenium- or copper-containing metal film having a desired thickness is obtained.
2. The method of claim 1, wherein the ruthenium precursor material in (a) is introduced into a reaction zone under chemical vapor deposition conditions.
3. The method of claim 1, wherein the tungsten-, molybdenum-, cobalt-, ruthenium- or copper-containing metal precursor is introduced into the reaction zone under chemical vapor deposition conditions.
4. The method of claim 1, wherein the metal precursor containing tungsten, molybdenum, cobalt, ruthenium or copper is introduced into the reaction zone under atomic layer deposition or pulsed CVD conditions.
5. The method according to claim 1, wherein the metal precursor containing tungsten, molybdenum, cobalt, ruthenium or copper is selected from a.MoCl5, MoOCl4, MoO2Cl2; Mo(CO)6, MoH2( i PrCp)2; b. WF6, W(tert-butyl-N)2(N(CH3)2)2, WCl5, WCl6 and WOCl4; W(CO)6, WH2( i PrCp)2; c. Co(tert-butyl-NCHCHN-tert-butyl)2, Co2(CO)6(HCCCF3) and Co2(CO)6(HCC(CH3)3); and d. 2-methoxy-1,3-diisopropyl amidine copper(I); 2-ethoxy-1,3-diisopropyl amidine copper(I); 2-tert-butoxy-1,3-diisopropyl amidine copper(I); 2-isopropyl-1,3-diisopropyl amidine copper(I); and 2-dimethylamino-1,3-diisopropyl amidine copper(I).
6. The method according to claim 1, wherein the molybdenum-containing metal precursor is selected from MoCl5, MoOCl4 or MoO2Cl2.
7. The method of claim 1, wherein the tungsten-containing metal precursor is selected from WF6 and W(tert-butyl-N)2(N(CH3)2)2.
8. The method of claim 1, wherein the copper-containing metal precursor is N',N"-diisopropyl-N,N-dimethylguanidine copper (I).
9. The method of claim 1, wherein the ruthenium-containing metal precursor comprises one or more compounds selected from the group consisting of: Wherein R is selected from C1-C4 alkyl.
10. The method according to claim 9, wherein R is tert-butyl.
11. The method of claim 1, wherein the oxygen-free ruthenium precursor comprises a compound selected from the following formula:
12. The method of claim 1, wherein the ruthenium-containing metal precursor comprises a compound selected from the group consisting of: Wherein R is selected from C1-C4 alkyl.
13. The method of claim 7, wherein the ruthenium-containing metal precursor comprises one or more compounds selected from the group consisting of:
14. The method of claim 1, wherein the ruthenium-containing film of step a. has a thickness of about A film with a thickness of 1000 Å exhibits a resistivity of about 450 μΩ-cm.
Citation Information
Patent Citations
New organo-Ruthenium compound, the process for its preparation and its use as a ruthenium precursor to manufacture ruthenium based film coated metal electrodes
EP1935897A1
METHOD OF FORMING Ru FILM AND METAL WIRING STRUCTURE
JP2008124464A
Chemical vapor deposition raw material composed of an organoruthenium compound and chemical vapor deposition method using the chemical vapor deposition raw material
JP6043851B1
Copper (I) compounds useful as deposition precursors of copper thin films
US20050283012A1
Process for electroless copper deposition
US20070004201A1