Coating process method of PCBN (polycrystalline cubic boron nitride) blade

By using high-temperature resistant thermal insulation materials and yttrium oxide in the PCBN blade coating process, combined with surface curing spray and alkaline galvanizing, the problem of surface blackening and stability after heat treatment in the coating process is solved, achieving high efficiency and environmental protection. The advanced coating process improves the high temperature resistance and aesthetics of the blade.

CN118788568APending Publication Date: 2024-10-18郑州华菱超硬材料有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410773753.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-16
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

PCBN blades have problems with blackening and discoloration of the surface after heat treatment during the coating process. The coating has poor stability and slow curing speed, which affects its appearance and efficiency.

Method used

Using a combination of high temperature resistant thermal insulation materials and yttrium oxide, a uniform coating is formed through physical vapor deposition technology or chemical vapor deposition technology, and surface curing spray and alkaline galvanizing are sprayed outside the coating to increase the high temperature resistance and stability of the coating To improve the performance and aesthetics, use detergents and anti-cracking agents to ensure the stability and adhesion of the coating.

Benefits of technology

It improves the high temperature resistance stability and aesthetics of PCBN blade coating, ensures the stability and adhesion effect of the coating, shortens the coating process time, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788568A_ABST
    Figure CN118788568A_ABST
Patent Text Reader

Abstract

The invention discloses a coating process method of a PCBN (Polycrystalline Cubic Boron Nitride) blade, which relates to the technical field of coating processes and comprises the following steps: cleaning the PCBN blade, removing oil stains and impurities on the surface of the PCBN blade, preparing a coating mixture, selecting a coating material, adding a high-temperature-resistant heat-insulating material, and uniformly mixing the high-temperature-resistant heat-insulating material with the coating mixture according to a weight ratio. A coating material and water are poured to be mixed, yttrium oxide is added, a coating reinforcing material is prepared, a detergent is poured into the coating mixture according to the weight proportion, the cleaned blade is placed into the coating reinforcing material, and the coating technological process of the PCBN blade is completed. According to the coating process method of the PCBN blade, high stability and high adiabaticity of high temperature resistance of the coating are improved, the situation that the surface of the blade is blackened and discolored due to fire baking after the PCBN blade is coated is avoided, the situation that the grain size of tungsten alloy is too large after multiple additives are mixed is avoided, and the coating process duration of the PCBN blade is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating technology, and in particular to a coating process method for a PCBN blade. Background Art

[0002] PCBN is polycrystalline cubic boron nitride. The production process of PCBN blades involves combining CBN material with a cemented carbide substrate. This combination method makes the PCBN blades have both the high hardness, high thermal stability and chemical stability of CBN materials and the strength and good weldability of cemented carbide. PCBN blades need to be coated with heat treatment during coating.

[0003] Patent No. CN 117070885 A discloses a PCBN tool with a nano-diamond thin film coating on the surface and a preparation method thereof, comprising a tool substrate and a multi-layer coating deposited on the substrate, wherein the composite reinforcement layer has an alternating stacking structure in which a first composite layer and a second composite layer are alternately repeated more than twice; the PCBN tool with a nano-diamond thin film coating on the surface provided by the present invention has high hardness, high wear resistance, strong adhesion, good high-temperature stability and high thermal conductivity, and the bonding strength between the coating and the substrate is high, the production process is simple, the production cost is low and the service life is long.

[0004] After searching the above patents, it was found that the coating process of PCBN blades has the following deficiencies: 1. Since the existing coating process of PCBN blades has high hardness, high wear resistance, strong adhesion, good high temperature stability and high thermal conductivity, but since the PCBN blades need to be heat treated after coating, the heat treatment can easily cause the blade surface to turn black and discolor, affecting the appearance of the PCBN blades. At the same time, in the coating process of PCBN blades, since multiple additives are required during the preparation of the coating, the multiple additives cannot ensure the stability of the coating while increasing the coating effect, and the tungsten alloy grains are prone to be too large, affecting the coating adhesion effect, and the PCBN blades cannot be quickly cured after coating, affecting the coating efficiency.

[0005] Therefore, a coating process method for a PCBN insert is proposed to solve the above problems. Summary of the invention

[0006] The main purpose of the present invention is to provide a coating process method for a PCBN blade which is resistant to high temperature, environmentally friendly and has a fast curing speed, and is applied to the coating preparation of the PCBN blade.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a coating process method for a PCBN blade, comprising the following steps:

[0008] Step 1: Pretreatment: Before coating the PCBN blade, the PCBN blade needs to be cleaned to remove oil and impurities on the surface;

[0009] Step 2: prepare a coating mixture, select a coating material, add a high temperature resistant heat insulating material, pour the high temperature resistant heat insulating material into the coating material and water according to the weight ratio, add yttrium oxide, stir for 30 minutes to 60 minutes, and prepare a coating mixture;

[0010] Step 3: Prepare a coating reinforcement material, pour a decontaminant in a weight ratio into the coating mixture, and add a thickener, a defoaming agent and an anti-cracking agent to prepare a coating reinforcement material with strong decontamination;

[0011] Step 4: Spray coating: Place the cleaned blade into the coating reinforcement material, form a uniform and fine coating on the blade surface by physical vapor deposition technology or chemical vapor deposition technology, and spray the spray material on the outer surface of the coating;

[0012] Step 5: Post-processing: heat-treating and cooling the coated blade to combine the coating with the PCBN blade, thus completing the coating process of the PCBN blade.

[0013] The coating material includes one or more combinations of TiN, Al2O3, AlTiN, TiCN, AlCrN and CVD diamond, and the ratio of the coating material to water is 5:2.

[0014] The high temperature resistant heat insulating material includes anti-oxidation material, wear resistant material and high temperature resistant material;

[0015] The antioxidant material includes one or more of polyurethane, silicone, alumina, silicate and perovskite, and the weight ratio of the antioxidant material is 1%-5% polyurethane, 1%-5% silicone, 1%-3% alumina, 2%-10% silicate and 5%-15% perovskite.

[0016] The wear-resistant material is a mixture of aluminum oxide, zirconium oxide and a resin base material, and the weight ratio of the wear-resistant material is 1%-5% of aluminum oxide, 2%-15% of zirconium oxide and 1%-10% of the resin base material.

[0017] The high temperature resistant material includes one or more of magnesium aluminum compound, mica, corundum, graphite, diamond, tungsten, silicon dioxide, silicon carbide, copper oxide, ferroferric oxide, iron powder and manganese dioxide;

[0018] The weight ratio of the high temperature resistant material is 1%-3% of magnesium aluminum compound, 2%-5% of mica, 2%-8% of corundum, 5%-12% of graphite, 3%-8% of diamond, 0.2%-3% of tungsten, 0.5%-3% of silicon dioxide, 0.4%-3% of silicon carbide, 1%-5% of copper oxide, 2%-4% of ferrosoferric oxide, 1%-3% of iron powder and 2%-8% of manganese dioxide.

[0019] The thickener includes one or more of cellulose derivatives such as methyl cellulose, carboxymethyl cellulose, polyanionic cellulose, starch derivatives, casein, sodium polyacrylate, polyethylene oxide, polyvinyl pyrrolidone, polyvinyl alcohol, low molecular polyethylene wax and polyacrylamide, and the weight ratio of the thickener is 2%-15%. The anti-cracking agent is mixed with 1%-3% clay, 10%-20% sand and gravel powder, 10%-20% aluminum powder, 10%-20% zirconium silicate, 2%-7% acetic acid and 10%-30% deionized water.

[0020] The defoaming agent is one or more of n-butanol, silicon dioxide powder, polylactic acid, starch, silicone polyester and siloxane, and the weight ratio of the defoaming agent is 0.5%-2% of n-butanol, 0.3%-1% of silicon dioxide powder, 0.5%-1% of silicone polyester and 0.5%-3% of siloxane;

[0021] The anti-cracking agent has the following weight components: one or more of 10-50 parts of 4-tert-butylphenol CAS, 20-100 parts of dehydroabietinamine, 15-30 parts of polyethylene glycol diacrylate, 20-30 parts of triethoxysilylpropyl maleic acid, 15-60 parts of N,N'methylenebisacrylamide copolymer, 10-50 parts of humic acid, 5-20 parts of pumice powder, 10-30 parts of shell powder, 120-250 parts of palygorskite powder, 100-250 parts of pearl stone powder, 100-150 parts of plant polysaccharides and 30-80 parts of choline glycerophosphate.

[0022] The detergent is a mixture of silica gel, alumina, natural clay, activated carbon powder, activated carbon powder, polylactic acid, starch, organosilicon and zeolite powder, wherein the weight ratio of the detergent is 5%-15% of silica gel, 2%-10% of alumina, 3%-15% of natural clay, 20%-30% of activated carbon powder, 2%-20% of activated carbon powder, 2%-20% of polylactic acid, 2%-20% of starch, 2%-20% of organosilicon and 5%-15% of zeolite powder;

[0023] The detergent comprises one or more of polylactic acid and starch.

[0024] The spray material includes surface curing spray and alkaline zinc plating, and the curing spray is made of polyurethane or liquid photosensitive resin.

[0025] The coating thickness is 2nm-30nm.

[0026] The present invention has the following beneficial effects:

[0027] 1. In the present invention, by adding high temperature resistant heat insulation material and adding yttrium oxide to the high temperature resistant heat insulation material, the coating used for the PCBN blade can increase the high stability and high thermal insulation of the coating. The alkaline galvanizing sprayed on the surface of the coating can prevent the coating of the PCBN blade from blackening and discoloring when it contacts fire, thereby increasing the beauty of the PCBN blade. The coating strength of the PCBN blade is further increased by adding yttrium oxide.

[0028] 2. In the present invention, by adding a detergent and yttrium oxide, the coating used for the PCBN blade can absorb harmful substances that appear after mixing with the additives, thereby avoiding the prepared PCBN blade coating material from polluting the environment, increasing the coating effect while ensuring the stability of the PCBN blade coating. At the same time, the added yttrium oxide can avoid the situation where the grain size of the tungsten alloy is too large after mixing multiple additives, making the coating more uniform and fine, and the adhesion effect of the coating is better.

[0029] 3. In the present invention, by spraying a spray material on the outer surface of the coating, the spray material includes a surface curing spray and alkaline galvanizing, and the curing spray is made of polyurethane or liquid photosensitive resin. The polyurethane and liquid photosensitive resin will cure quickly after encountering air, thereby shortening the coating process time of the PCBN blade and improving the coating process efficiency of the PCBN blade. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a schematic diagram of the overall process of a coating process method for a PCBN blade. DETAILED DESCRIPTION

[0031] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0032] Comparative Example

[0033] A coating process method for a PCBN blade, the coating process method for a PCBN blade comprising the following steps:

[0034] Step 1: Clean the PCBN blade to remove oil and impurities on the surface;

[0035] Step 2: Select coating material and stir for 30-60 minutes;

[0036] Step 3: Add thickener, defoamer and anti-cracking agent;

[0037] Step 4: Place the cleaned blade into the coating reinforcement material, and form a uniform and fine coating on the blade surface by physical vapor deposition technology or chemical vapor deposition technology;

[0038] Step 5: heat treat and cool the coated blade to combine the coating with the PCBN blade, thus completing the coating process of the PCBN blade.

[0039] Comparison 1:

[0040] S1: Before coating the PCBN insert, the PCBN insert needs to be cleaned to remove oil and impurities on the surface;

[0041] S2: Select coating materials, add high temperature resistant heat insulation materials, pour high temperature resistant heat insulation materials including antioxidant materials, wear resistant materials and high temperature resistant materials according to the weight ratio, mix coating materials including one or more combinations of TiN, Al2O3, AlTiN, TiCN, AlCrN and CVD diamond and water, add yttrium oxide, stir for 30min-60min, and prepare a coating mixture;

[0042] S3: pouring the detergent in the weight ratio into the coating mixture, and adding the thickener, defoaming agent and anti-cracking agent;

[0043] S4: placing the cleaned blade into the coating reinforcement material, and forming a uniform and fine coating on the blade surface by physical vapor deposition technology or chemical vapor deposition technology;

[0044] S5: heat-treating and cooling the coated blade to combine the coating with the PCBN blade, thus completing the coating process of the PCBN blade.

[0045] Comparison 2:

[0046] S1: Before coating the PCBN insert, the PCBN insert needs to be cleaned to remove oil and impurities on the surface;

[0047] S2: Select coating material and stir for 30-60 minutes;

[0048] S3: pouring a decontamination agent prepared by mixing silica gel, alumina, natural clay, activated carbon powder, activated carbon powder, polylactic acid, starch, silicone and zeolite powder according to a weight ratio into the coating mixture, and adding a thickener, a defoaming agent and an anti-cracking agent to prepare a coating reinforcement material with strong decontamination;

[0049] S4: placing the cleaned blade into the coating reinforcement material, and forming a uniform and fine coating on the blade surface by physical vapor deposition technology or chemical vapor deposition technology;

[0050] S5: heat-treating and cooling the coated blade to combine the coating with the PCBN blade, thus completing the coating process of the PCBN blade.

[0051] Comparison 3:

[0052] S1: Before coating the PCBN insert, the PCBN insert needs to be cleaned to remove oil and impurities on the surface;

[0053] S2: Select coating material and stir for 30-60 minutes;

[0054] S3: pouring the detergent in the weight ratio into the coating mixture, and adding the thickener, defoaming agent and anti-cracking agent;

[0055] S4: placing the cleaned blade into the coating reinforcement material, forming a uniform and fine coating on the blade surface by physical vapor deposition technology or chemical vapor deposition technology, and spraying a spray material on the outer surface of the coating, the spray material including surface curing spray and alkaline zinc plating;

[0056] S5: heat-treating and cooling the coated blade to combine the coating with the PCBN blade, thus completing the coating process of the PCBN blade.

[0057] Embodiment 1

[0058] Please refer to Figure 1 As shown: A coating process method for a PCBN blade comprises the following steps:

[0059] Step 1: Pretreatment: Before coating the PCBN blade, the PCBN blade needs to be cleaned to remove oil and impurities on the surface;

[0060] Step 2: prepare a coating mixture, select a coating material, add a high temperature resistant heat insulating material, pour the high temperature resistant heat insulating material into the coating material and water according to the weight ratio, add yttrium oxide, stir for 30 minutes to 60 minutes, and prepare a coating mixture;

[0061] Step 3: Prepare a coating reinforcement material, pour a decontaminant in a weight ratio into the coating mixture, and add a thickener, a defoaming agent and an anti-cracking agent to prepare a coating reinforcement material with strong decontamination;

[0062] Step 4: Spray coating: Place the cleaned blade into the coating reinforcement material, form a uniform and fine coating on the blade surface by physical vapor deposition technology or chemical vapor deposition technology, and spray the spray material on the outer surface of the coating;

[0063] Step 5: Post-processing: heat-treating and cooling the coated blade to combine the coating with the PCBN blade, thus completing the coating process of the PCBN blade.

[0064] High temperature resistant heat insulation materials include antioxidant materials, wear resistant materials and high temperature resistant materials;

[0065] The antioxidant material includes one or more of polyurethane, silicone, alumina, silicate and perovskite, and the weight ratio of the antioxidant material is 1%-5% polyurethane, 1%-5% silicone, 1%-3% alumina, 2%-10% silicate and 5%-15% perovskite.

[0066] The wear-resistant material is mixed with aluminum oxide, zirconium oxide and resin base material, and the weight ratio of the wear-resistant material is 1%-5% of aluminum oxide, 2%-15% of zirconium oxide and 1%-10% of resin base material.

[0067] The high temperature resistant material includes one or more of magnesium aluminum compound, mica, corundum, graphite, diamond, tungsten, silicon dioxide, silicon carbide, copper oxide, ferroferric oxide, iron powder and manganese dioxide;

[0068] The weight ratio of high temperature resistant materials is 1% - 3% of magnesium aluminum compound, 2% - 5% of mica, 2% - 8% of corundum, 5% - 12% of graphite, 3% - 8% of diamond, 0.2% - 3% of tungsten, 0.5% - 3% of silicon dioxide, 0.4% - 3% of silicon carbide, 1% - 5% of copper oxide, 2% - 4% of ferrosoferric oxide, 1% - 3% of iron powder and 2% - 8% of manganese dioxide.

[0069] The coating used on PCBN blades can increase the high stability and high thermal insulation of the coating at high temperatures, prevent the surface of the PCBN blade from turning black and discolored when the coating contacts fire, increase the appearance of the PCBN blade, and further increase the strength of the coating of the PCBN blade by adding yttrium oxide.

[0070] Embodiment 2

[0071] Please refer to Figure 1As shown: Based on Example 1, the thickener includes one or more of cellulose derivatives such as methyl cellulose, carboxymethyl cellulose, polyanionic cellulose, starch derivatives, casein, sodium polyacrylate, polyethylene oxide, polyvinyl pyrrolidone, polyvinyl alcohol, low molecular weight polyethylene wax and polyacrylamide, the weight ratio of the thickener is 2%-15%, and the anti-cracking agent is mixed with 1%-3% clay, 10%-20% sand and gravel powder, 10%-20% aluminum powder, 10%-20% zirconium silicate, 2%-7% acetic acid and 10%-30% deionized water.

[0072] The defoaming agent is one or more of n-butanol, silicon dioxide powder, polylactic acid, starch, silicone polyester and siloxane, and the weight ratio of the defoaming agent is 0.5%-2% of n-butanol, 0.3%-1% of silicon dioxide powder, 0.5%-1% of silicone polyester and 0.5%-3% of siloxane;

[0073] The weight components of the anti-cracking agent are as follows: one or more of 10-50 parts of 4-tert-butylphenol CAS, 20-100 parts of dehydroabietinamine, 15-30 parts of polyethylene glycol diacrylate, 20-30 parts of triethoxysilylpropyl maleic acid, 15-60 parts of N,N'methylenebisacrylamide copolymer, 10-50 parts of humic acid, 5-20 parts of pumice powder, 10-30 parts of shell powder, 120-250 parts of palygorskite powder, 100-250 parts of pearl stone powder, 100-150 parts of plant polysaccharides and 30-80 parts of choline glycerophosphate.

[0074] The detergent is a mixture of silica gel, alumina, natural clay, activated carbon powder, activated carbon powder, polylactic acid, starch, organosilicon and zeolite powder, wherein the weight ratio of the detergent is 5%-15% of silica gel, 2%-10% of alumina, 3%-15% of natural clay, 20%-30% of activated carbon powder, 2%-20% of activated carbon powder, 2%-20% of polylactic acid, 2%-20% of starch, 2%-20% of organosilicon and 5%-15% of zeolite powder;

[0075] The detergent includes one or more of polylactic acid and starch, which can degrade crystal particles, making the prepared coating more delicate and uniform.

[0076] The coating used for PCBN blades can absorb harmful substances that appear after mixing with additives, avoid polluting the environment with the prepared PCBN blade coating materials, increase the coating effect while ensuring the stability of the PCBN blade coating. At the same time, the added yttrium oxide can avoid the situation where the grain size of tungsten alloy is too large after mixing multiple additives, making the coating more uniform and fine, and the coating adhesion effect is better.

[0077] Embodiment 3

[0078] Please refer to Figure 1 As shown: Based on the first embodiment, the spray material includes surface curing spray and alkaline zinc plating, and the curing spray is made of polyurethane or liquid photosensitive resin.

[0079] The coating thickness is 2nm~30nm.

[0080] The curing spray is made of polyurethane or liquid photosensitive resin. The polyurethane and liquid photosensitive resin will cure quickly when they meet the air, which shortens the coating process time of the PCBN blade and improves the coating process efficiency of the PCBN blade.

[0081] The test results of high temperature resistance, thermal insulation and environmental protection performance are shown in Table 1 below:

[0082] Table 1: Tests on high temperature resistance, thermal insulation and environmental performance

[0083] High temperature resistance, heat insulation and thermal insulation performance (℃) Environmental performance (%) Embodiment 1 120—350 10—20 Embodiment 2 250—450 25—55 Embodiment 3 300—750 45—85

[0084] It can be seen from the test results in the above table that the high temperature resistance, heat insulation and environmental protection performance of the coating of the prepared PCBN insert are significantly enhanced.

[0085] The present invention provides a coating process method for a PCBN blade. When the method is operated, the PCBN blade needs to be cleaned before coating the PCBN blade to remove oil stains and impurities on the surface; a coating mixture is prepared, a coating material is selected, a high temperature resistant heat insulation material is added, the high temperature resistant heat insulation material is added according to a weight ratio, the coating material and water are poured into the mixture, yttrium oxide is added, and stirred for 30 minutes to 60 minutes to prepare a coating mixture; and the high temperature resistant heat insulation material is added, and yttrium oxide is added to the high temperature resistant heat insulation material. Yttrium makes the coating used in PCBN blades increase the high stability and high thermal insulation of the coating, avoids the blackening and discoloration of the blade surface when the coating of the PCBN blade contacts fire, increases the appearance of the PCBN blade, and further increases the coating strength of the PCBN blade by adding yttrium oxide; prepare the coating reinforcement material, pour the detergent according to the weight ratio into the coating mixture, and add the thickener, defoaming agent and anti-cracking agent to prepare the strong decontamination coating reinforcement material, by adding the detergent and yttrium oxide, the PC The coating used in the BN blade can absorb harmful substances after mixing with additives, avoid the prepared PCBN blade coating material from polluting the environment, increase the coating effect and ensure the stability of the PCBN blade coating. At the same time, the added yttrium oxide can avoid the situation where the grain size of tungsten alloy is too large after mixing multiple additives, making the coating more uniform and fine, and the coating adhesion effect is better; spray coating, put the cleaned blade into the coating reinforcement material, form a uniform and fine coating on the blade surface through physical vapor deposition technology or chemical vapor deposition technology, and spray the spray material on the outer surface of the coating, spray the spray material on the outer surface of the coating, the spray material includes surface curing spray and alkaline zinc plating, and the curing spray is made of polyurethane or liquid photosensitive resin. The characteristics of polyurethane and liquid photosensitive resin that they will quickly solidify after encountering air shorten the coating process time of the PCBN blade and improve the coating process efficiency of the PCBN blade; post-processing, heat treatment and cooling treatment are performed on the coated blade, the coating is combined with the PCBN blade to complete the coating process of the PCBN blade. The preparation of the coating process method of the entire PCBN blade is simple and easy to operate.

[0086] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A coating process for a PCBN insert, characterized in that: The coating process of the PCBN blade comprises the following steps: Step 1: Pretreatment: Before coating the PCBN blade, the PCBN blade needs to be cleaned to remove oil and impurities on the surface; Step 2: prepare a coating mixture, select a coating material, add a high temperature resistant heat insulating material, pour the high temperature resistant heat insulating material into the coating material and water according to the weight ratio, add yttrium oxide, stir for 30 minutes to 60 minutes, and prepare a coating mixture; Step 3: Prepare a coating reinforcement material, pour a decontaminant in a weight ratio into the coating mixture, and add a thickener, a defoaming agent and an anti-cracking agent to prepare a coating reinforcement material with strong decontamination; Step 4: Spray coating: Place the cleaned blade into the coating reinforcement material, form a uniform and fine coating on the blade surface by physical vapor deposition technology or chemical vapor deposition technology, and spray the spray material on the outer surface of the coating; Step 5: Post-processing: heat-treating and cooling the coated blade to combine the coating with the PCBN blade, thus completing the coating process of the PCBN blade.

2. The method according to claim 1, characterized in that The coating material includes one or more combinations of TiN, Al2O3, AlTiN, TiCN, AlCrN and CVD diamond, and the ratio of the coating material to water is 5:

2.

3. The method according to claim 1, characterized in that The high temperature resistant heat insulating material includes anti-oxidation material, wear resistant material and high temperature resistant material; The antioxidant material includes one or more of polyurethane, silicone, alumina, silicate and perovskite, and the weight ratio of the antioxidant material is 1%-5% polyurethane, 1%-5% silicone, 1%-3% alumina, 2%-10% silicate and 5%-15% perovskite.

4. The method according to claim 3, characterized in that The wear-resistant material is a mixture of aluminum oxide, zirconium oxide and a resin base material, and the weight ratio of the wear-resistant material is 1%-5% of aluminum oxide, 2%-15% of zirconium oxide and 1%-10% of the resin base material.

5. The method according to claim 4, characterized in that The high temperature resistant material includes one or more of magnesium aluminum compound, mica, corundum, graphite, diamond, tungsten, silicon dioxide, silicon carbide, copper oxide, ferroferric oxide, iron powder and manganese dioxide; The weight ratio of the high temperature resistant material is 1%-3% of magnesium aluminum compound, 2%-5% of mica, 2%-8% of corundum, 5%-12% of graphite, 3%-8% of diamond, 0.2%-3% of tungsten, 0.5%-3% of silicon dioxide, 0.4%-3% of silicon carbide, 1%-5% of copper oxide, 2%-4% of ferrosoferric oxide, 1%-3% of iron powder and 2%-8% of manganese dioxide.

6. The method according to claim 1, characterized in that The thickener includes one or more of cellulose derivatives such as methyl cellulose, carboxymethyl cellulose, polyanionic cellulose, starch derivatives, casein, sodium polyacrylate, polyethylene oxide, polyvinyl pyrrolidone, polyvinyl alcohol, low molecular polyethylene wax and polyacrylamide, and the weight ratio of the thickener is 2%-15%. The anti-cracking agent is mixed with 1%-3% clay, 10%-20% sand and gravel powder, 10%-20% aluminum powder, 10%-20% zirconium silicate, 2%-7% acetic acid and 10%-30% deionized water.

7. The method according to claim 1, characterized in that The defoaming agent is one or more of n-butanol, silicon dioxide powder, polylactic acid, starch, silicone polyester and siloxane, and the weight ratio of the defoaming agent is 0.5%-2% of n-butanol, 0.3%-1% of silicon dioxide powder, 0.5%-1% of silicone polyester and 0.5%-3% of siloxane; The anti-cracking agent has the following weight components: one or more of 10-50 parts of 4-tert-butylphenol CAS, 20-100 parts of dehydroabietinamine, 15-30 parts of polyethylene glycol diacrylate, 20-30 parts of triethoxysilylpropyl maleic acid, 15-60 parts of N,N'methylenebisacrylamide copolymer, 10-50 parts of humic acid, 5-20 parts of pumice powder, 10-30 parts of shell powder, 120-250 parts of palygorskite powder, 100-250 parts of pearl stone powder, 100-150 parts of plant polysaccharides and 30-80 parts of choline glycerophosphate.

8. The method according to claim 1, characterized in that The detergent is mixed with silica gel, alumina, natural clay, activated carbon powder, activated carbon powder, polylactic acid, starch, silicone and zeolite powder, and the weight ratio of the detergent is 5%-15% of silica gel, 2%-10% of alumina, 3%-15% of natural clay, 20%-30% of activated carbon powder, 2%-20% of activated carbon powder, 2%-20% of polylactic acid, 2%-20% of starch, 2%-20% of silicone and 5%-15% of zeolite powder.

9. The method according to claim 1, characterized in that: The spray material includes surface curing spray and alkaline zinc plating, and the curing spray is made of polyurethane or liquid photosensitive resin.

10. The method according to claim 1, characterized in that The coating thickness is 2nm-30nm.

Citation Information

Patent Citations

  • PCBN cutter with nano diamond film coating on surface and preparation method of PCBN cutter

    CN113403602A

  • PCBN (Polycrystalline Cubic Boron Nitride) cutter with nano diamond film coating on surface and preparation method of PCBN cutter

    CN117070885A

  • CVD coating scheme including alumina and / or titanium-containing materials and method of making the same

    US20070298232A1