An easy-to-cut eleven-layer co-extruded high-barrier packaging film and preparation method thereof

Through the composite technology of organic-inorganic hybrid opening agent, the problem of difficult cutting and adhesion of polyethylene films on high-speed packaging production lines is solved, and the easy cutting and excellent barrier properties of eleven layers of co-extruded high-barrier packaging films are achieved. Suitable for high-speed packaging production lines.

CN118789912BActive Publication Date: 2024-12-06SUZHOU ZIJIN PLASTIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411259760.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

On the high-speed packaging production line, polyethylene films are difficult to cut and easily stick, which affects production efficiency due to their strong adhesion.

Method used

Using organic-inorganic hybrid opening agent, the compound of zero-dimensional and two-dimensional inorganic opening agent and organic opening agent is formed to form an easily cut eleven-layer coextruded high-barrier packaging film, which is improved by hydrogen bonding and Schiff base reaction. The opening and barrier properties of the membrane.

Benefits of technology

It realizes easy cutting, anti-adhesion, excellent barrier properties and good heat sealing strength of polyethylene films, and is suitable for industrial automatic high-speed packaging production lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789912B_ABST
    Figure CN118789912B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of easy-to-cut packaging films for high-speed packaging production lines, and discloses an easy-to-cut eleven-layer co-extruded high-barrier packaging film and a preparation method thereof. The preparation method of the packaging film comprises the following steps: modifying a silane coupling agent containing a phenolic hydroxyl functional group and an aldehyde functional group on the surface of a zero-dimensional inorganic opening agent at the same time; modifying a silane coupling agent KH540 and a silane cross-linking agent containing a phenolic hydroxyl functional group on the surface of a two-dimensional inorganic opening agent at the same time; compounding the zero-dimensional inorganic opening agent with the two-dimensional inorganic opening agent through a Schiff base reaction, and then compounding with an organic opening agent through a hydrogen bond to obtain an organic-inorganic hybrid opening agent, which is introduced into the eleventh layer of the eleven-layer co-extruded film to obtain an easy-to-cut eleven-layer co-extruded high-barrier packaging film, which is not only easy to cut and does not produce adhesion, but also has excellent barrier properties and heat sealing strength, and is very suitable for use on an industrial automatic high-speed packaging production line.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of easy-to-cut packaging films for high-speed packaging production lines, in particular to an easy-to-cut eleven-layer co-extruded high-barrier packaging film and a preparation method thereof. Background Art

[0002] On industrial automatic packaging production lines, due to the high speed of film pulling, the opening performance and smoothness of the film used to package food, magazines, textiles, sanitary products and other products on high-speed production lines are required to be high. Polyethylene film has excellent tear strength, impact strength and puncture resistance, and is widely used in food packaging, medical packaging, cultural product packaging, heavy packaging bags, shopping bags and agricultural films. Due to the small polarity of polyethylene molecules, during the blow molding process, the films are easily bonded under vacuum and difficult to separate, resulting in difficulty in being cut on the packaging production line and easy to cause adhesion.

[0003] In order to improve the opening property of polyethylene film, an opening agent is usually added before producing blown film to improve the opening property. Opening agents can be divided into inorganic opening agents and organic opening agents. Common inorganic opening agents on the market include talcum powder, hydrated magnesium silicate, silicon dioxide, diatomaceous earth, calcium carbonate, calcium sulfate, sodium hydrogen phosphate, calcium hydrogen phosphate, hydrotalcite, bentonite, etc. Common organic opening agents include high carbon esters, amides, ammonium oxide, etc. When the inorganic opening agent is evenly dispersed in the plastic film, it can form many uneven spots on the surface of the film, reducing the contact area between the films and making the plastic film easy to open; when the organic opening agent is evenly dispersed in the plastic film, the organic opening agent gradually migrates from the inside of the plastic film to the surface of the film, and gathers into a protective film on the surface of the film, making the surface of the film smooth, which can reduce the friction coefficient between the films, making it easy to slide between the films, and preventing the molecular chains from entangled with each other, so as to achieve the purpose of anti-adhesion of polyethylene film. Usually, organic opening agents and inorganic opening agents need to work together to achieve the best opening property.

[0004] In addition, nylon (polyamide, PA) has a wide operating temperature range, from -60°C to 200°C. Ethylene-vinyl alcohol copolymer has always been the most widely used high-barrier material. Summary of the invention

[0005] The present invention develops an eleven-layer co-extruded packaging film which is very suitable for use on an industrial automatic high-speed packaging production line. The packaging film is not only easy to cut and does not produce adhesion, but also has excellent barrier properties and heat-sealing strength.

[0006] A method for preparing an eleven-layer co-extruded high-barrier packaging film that is easy to cut, comprising the following steps:

[0007] Step 1: preparing an organic-inorganic hybrid type opening agent, the organic-inorganic hybrid type opening agent is an organic-inorganic hybrid type opening agent I or an organic-inorganic hybrid type opening agent II, and the specific process is as follows:

[0008] preparing a silane coupling agent containing a phenolic hydroxyl functional group, a silane coupling agent containing an aldehyde functional group and a silane crosslinking agent containing a phenolic hydroxyl functional group;

[0009] The method for preparing the organic-inorganic hybrid opening agent I is:

[0010] Modifying the surface of the hydroxyl-functionalized zero-dimensional inorganic opening agent SiO2 with a silane coupling agent containing a phenolic hydroxyl functional group to obtain a phenolic hydroxylated zero-dimensional inorganic opening agent SiO2;

[0011] The phenolic hydroxylated zero-dimensional inorganic opening agent SiO2 was compounded with the organic opening agent stearic acid amide through hydrogen bonding to prepare the organic-inorganic hybrid opening agent Ⅰ;

[0012] The method for preparing the organic-inorganic hybrid type opening agent II is:

[0013] Simultaneously modifying the surface of the hydroxyl-functionalized zero-dimensional inorganic opening agent SiO2 with a silane coupling agent containing a phenolic hydroxyl functional group and a silane coupling agent containing an aldehyde functional group, thereby obtaining an aldehyde-functionalized phenolic hydroxyl-functionalized zero-dimensional inorganic opening agent SiO2;

[0014] The silane coupling agent KH540 and the silane crosslinking agent containing phenolic hydroxyl functional groups are simultaneously modified on the surface of the two-dimensional inorganic opening agent MgAl-LDH rich in hydroxyl functional groups to obtain the amino-phenolic hydroxylated two-dimensional inorganic opening agent MgAl-LDH;

[0015] The aldehyde-hydroxylated phenolic zero-dimensional inorganic opening agent SiO2 and the amino-hydroxylated phenolic two-dimensional inorganic opening agent MgAl-LDH are compounded by Schiff base reaction to prepare a composite inorganic opening agent.

[0016] The composite inorganic anti-blocking agent is compounded with the organic anti-blocking agent stearic acid amide through hydrogen bonding to prepare an organic-inorganic hybrid anti-blocking agent II;

[0017] Step 2: Set up the film structure of the eleven-layer co-extruded film, introduce the organic-inorganic hybrid anti-blocking agent into the eleventh layer of the eleven-layer co-extruded film, the eleventh layer is a PE layer, and adopt the eleven-layer co-extrusion blow molding film forming process to prepare an easy-to-cut eleven-layer co-extruded high barrier packaging film.

[0018] Preferably, the formula of the organic-inorganic hybrid opening agent I is: the mass ratio of the silane coupling agent containing a phenolic hydroxyl functional group, the inorganic opening agent SiO2 and the organic opening agent is (0.1~2):1:(0.1~2);

[0019] Preferably, the formula of the aldehyde-hydroxylated phenolic hydroxylated zero-dimensional inorganic opening agent SiO2 is: the mass ratio of the silane coupling agent containing the phenolic hydroxyl functional group, the silane coupling agent containing the aldehyde functional group and the inorganic opening agent SiO2 is (0.1~1): (0.1~1): 1;

[0020] Preferably, the formula of the aminophenol hydroxylated two-dimensional inorganic opening agent MgAl-LDH is: the mass ratio of the silane coupling agent KH540, the silane crosslinking agent containing the phenolic hydroxyl functional group and the inorganic opening agent MgAl-LDH is (0.1~1): (0.1~1): 1;

[0021] Preferably, the formula of the composite inorganic opening agent is: the mass ratio of the inorganic opening agent SiO2 to the inorganic opening agent MgAl-LDH is 1:(0.5~2);

[0022] Preferably, the formula of the organic-inorganic hybrid opening agent II is: the mass ratio of the composite inorganic opening agent to the organic opening agent is 1:(0.1-2).

[0023] Preferably, the eleven-layer co-extruded high barrier packaging film has an asymmetric structure, and the formula and dosage of each film layer are as follows:

[0024] The first layer is a PE layer: its raw material formula is 40~80wt% LDPE and 20~60wt% LLDPE, and its usage is 5~15 parts by weight;

[0025] The second layer is a PE layer: its raw material formula is 20~60wt% HDPE and 40~80wt% LLDPE, and its usage is 3~10 parts by weight;

[0026] The third layer is a PE layer: its raw material formula is 20~60wt% LDPE and 40~80wt% LLDPE, and its usage is 5~15 parts by weight;

[0027] The fourth layer is a bonding layer: its raw material formula is 100wt% PE-g-MAH, and its usage is 2-8 parts by weight;

[0028] The fifth layer is a PA layer: its raw material formula is 100wt% PA, and its usage is 5-15 parts by weight;

[0029] The sixth layer is a barrier layer: its raw material formula is 100wt% EVOH, and its usage is 5-15 parts by weight;

[0030] The seventh layer is a PA layer: its raw material formula is 100wt% PA, and its usage is 5-15 parts by weight;

[0031] The eighth layer is a bonding layer: its raw material formula is 100wt% PE-g-MAH, and its usage is 2-8 parts by weight;

[0032] The ninth layer is a PE layer: its raw material formula is 20-60wt% LDPE and 40-80wt% LLDPE, and its usage is 5-15 parts by weight;

[0033] The tenth layer is a PE layer: its raw material formula is 20-60wt% HDPE and 40-80wt% LLDPE, and its usage is 3-10 parts by weight;

[0034] The eleventh layer is a PE layer: its raw material formula is 40-70wt% LDPE, 20-40wt% LLDPE and 5-20wt% organic-inorganic hybrid opening agent, and its usage is 10-30 parts by weight.

[0035] Preferably, the preparation method of the silane coupling agent containing a phenolic hydroxyl functional group is: utilizing a nucleophilic substitution reaction mechanism, wherein p-toluenesulfonic acid catalyzes a thioesterification reaction between the carboxyl functional group of homovanillic acid and the mercapto functional group of 3-mercaptopropyltrimethoxysilane to prepare a silane coupling agent containing a phenolic hydroxyl functional group.

[0036] Preferably, the preparation method of the silane coupling agent containing an aldehyde functional group is:

[0037] Based on the Markovnikov rule of oriented electrophilic addition reaction of olefins, the strong acid catalyst catalyzes the addition reaction of homovanillic acid and citronellal to generate phenolic hydroxyl aldehyde monomers.

[0038] The phenolic hydroxyl aldehyde monomer is used as a nucleophilic reagent, and the bromine functional group of 3-bromopropyltrimethoxysilane reacts with the phenolic hydroxyl functional group of the phenolic hydroxyl aldehyde monomer to produce a nucleophilic substitution reaction, so as to prepare a silane coupling agent containing an aldehyde functional group.

[0039] Preferably, the strong acid catalyst is one of sulfuric acid, p-toluenesulfonic acid and fluoroboric acid.

[0040] Preferably, the preparation method of the silane crosslinking agent containing phenolic hydroxyl functional groups is: utilizing the nucleophilic substitution reaction mechanism, under the promotion of an activator, an acylation reaction between the carboxyl functional group of homovanillic acid and the secondary amine group of di(3-trimethoxysilylpropyl)amine is catalyzed by an organic base to prepare the silane crosslinking agent containing phenolic hydroxyl functional groups.

[0041] Preferably, the activator is one of N,N'-dicyclohexylcarbodiimide (DCC), 1-hydroxybenzotriazole (HOBT), N-hydroxy-7-azabenzotriazole (HOAT), and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC).

[0042] Preferably, the organic base is one of pyridine, triethylamine, tributylamine and imidazole.

[0043] The eleven-layer co-extruded high-barrier packaging film that is easy to cut and prepared according to the above method is used in an industrial automatic high-speed packaging production line.

[0044] Beneficial effects: The present invention firstly uses bio-based compounds homovanillic acid and citronellal and silane coupling agent as raw materials, designs and synthesizes aldehyde trimethoxy silane coupling agent, phenolic hydroxy di (trimethoxy) silane crosslinking agent, and phenolic hydroxy trimethoxy silane coupling agent;

[0045] Then, the present invention uses phenolic hydroxy trimethoxy silane coupling agent to perform surface modification on the zero-dimensional inorganic opening agent, and then compounds it with the organic opening agent through hydrogen bonding to prepare the first organic-inorganic hybrid opening agent;

[0046] On the other hand, the zero-dimensional inorganic opening agent is surface-modified by using a phenolic hydroxy trimethoxy silane coupling agent and an aldehyde trimethoxy silane coupling agent, and the two-dimensional inorganic opening agent is surface-modified by using a silane coupling agent KH540 and a phenolic hydroxy di(trimethoxy) silane crosslinking agent. The aldehyde functional group obtained by surface modification of the zero-dimensional inorganic opening agent reacts with the amino functional group obtained by surface modification of the two-dimensional inorganic opening agent to produce a Schiff base reaction to prepare a composite inorganic opening agent. The composite inorganic opening agent is compounded with the organic opening agent through hydrogen bonding to prepare a second organic-inorganic hybrid opening agent.

[0047] An organic-inorganic hybrid opening agent is added during the production of polyethylene packaging film, and the opening performance of the polyethylene material is improved by using the organic-inorganic hybrid opening agent. An eleven-layer co-extrusion high-barrier packaging film is prepared by adopting an eleven-layer co-extrusion blow molding film-forming process.

[0048] The experimental results show that the eleven-layer co-extruded high barrier packaging film prepared by the present invention not only exhibits excellent anti-adhesion performance, is a highly smooth and easy-to-cut material, but also has excellent barrier properties and good heat-sealing strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 These are the performance test results of eleven-layer co-extruded high barrier packaging film. DETAILED DESCRIPTION

[0050] The main raw materials used in the present invention are as follows:

[0051] Low-density polyethylene resin (LDPE), brand LD 150DW, purchased from Jiangsu Rantai Plastics Co., Ltd.;

[0052] Linear low-density polyethylene resin (LLDPE), brand 2045G, purchased from Yuyao Hongyang Plastics Co., Ltd.;

[0053] High-density polyethylene resin (HDPE), brand FB5600, purchased from Dongguan Longhuang Plastic Raw Materials Co., Ltd.;

[0054] Ethylene vinyl alcohol copolymer resin (EVOH), brand ET3803RB, purchased from Guangzhou Best New Material Technology Co., Ltd.;

[0055] Maleic anhydride grafted polyethylene resin (PE-g-MAH), brand 4288, purchased from Dongguan Taotao Plastic Raw Materials Co., Ltd.;

[0056] Nylon resin (PA), brand XCGA035, was purchased from Zhuzhou Times New Materials Technology Co., Ltd.;

[0057] Nano-silicon dioxide zinc powder, item number 100361, particle size 10-20 nm, purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.;

[0058] Nano-MgAl-LDH powder, item number 102911, with a flake diameter of 1-4 μm, was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.

[0059] Experimental Example 1:

[0060] Synthesis of phenolic hydroxy trimethoxy silane coupling agent: Using the nucleophilic substitution reaction mechanism, p-toluenesulfonic acid catalyzes the carboxyl functional group of homovanillic acid and the mercapto functional group of 3-mercaptopropyl trimethoxy silane to undergo a thioesterification reaction to generate phenolic hydroxy trimethoxy silane coupling agent;

[0061] Among them, the chemical structure of homovanillic acid is:

[0062] ;

[0063] The chemical structure of 3-mercaptopropyltrimethoxysilane is:

[0064] ;

[0065] The chemical structure of phenolic hydroxy trimethoxy silane coupling agent is:

[0066] ;

[0067] The specific experimental steps for preparing the phenolic hydroxy trimethoxy silane coupling agent are as follows: 1.8 g of homovanillic acid, 2.0 g of 3-mercaptopropyl trimethoxy silane, 1.0 g of p-toluenesulfonic acid and 50 mL of acetone are added to a three-necked flask with a water separator, heated to 70° C. for reflux reaction for 5 h under mechanical stirring, and the solvent is removed by rotary evaporation, and washed with saturated sodium bicarbonate aqueous solution and deionized water in turn until neutral, filtered, and vacuum dried at 40° C. for 12 h to obtain the phenolic hydroxy trimethoxy silane coupling agent;

[0068] The nuclear magnetic resonance hydrogen spectrum of phenolic hydroxy trimethoxy silane coupling agent is characterized as follows: 1 H NMR (CDCl3, 400MHz) δ: 0.79-0.82 (t, 2H), 1.77-1.84 (m, 2H), 2.98-3.01 (t, 2H), 3.56 (s, 9H), 3.85 (s, 3H), 4.04 (s, 2H), 6.80-6.85 (m, 3H).

[0069] Experimental Example 2:

[0070] Synthesis of phenolic hydroxybis(trimethoxy)silane crosslinker: Using the nucleophilic substitution reaction mechanism, under the promotion of 1-hydroxybenzotriazole, the carboxyl functional group of homovanillic acid and the secondary amine group of di(3-trimethoxysilylpropyl)amine are acylated by triethylamine to generate phenolic hydroxybis(trimethoxy)silane crosslinker;

[0071] Among them, the chemical structural formula of di(3-trimethoxysilylpropyl)amine is:

[0072] ;

[0073] The chemical formula of phenolic hydroxybis(trimethoxy)silane crosslinker is:

[0074] ;

[0075] The specific experimental steps for preparing the phenolic hydroxybis(trimethoxy)silane crosslinker are as follows: under the protection of nitrogen, 1.8 g of homovanillic acid, 3.4 g of bis(3-trimethoxysilylpropyl)amine, 1.0 g of triethylamine and 80 mL of anhydrous dichloromethane are added to a three-necked flask with a water separator, stirred and dissolved at room temperature for 30 min, then 20 mL of anhydrous dichloromethane solution dissolved with 1.5 g of 1-hydroxybenzotriazole is added dropwise to the three-necked flask, stirred and reacted at room temperature for 18 h, poured into deionized water, filtered, extracted with dichloromethane, dried over anhydrous magnesium sulfate, rotary evaporated to remove the solvent, and dried in vacuo at 40° C. for 12 h to obtain the phenolic hydroxybis(trimethoxy)silane crosslinker;

[0076] The nuclear magnetic resonance hydrogen spectrum of phenolic hydroxybis(trimethoxy)silane crosslinker is characterized as follows:1 H NMR (CDCl3, 400MHz) δ: 0.76-0.79 (t, 4H), 1.65-1.72 (m, 4H), 3.30-3.34 (t, 4H), 3.57 (s, 18H), 3.68 (s, 2H), 3.82 (s, 3H), 6.73-6.82 (m, 3H).

[0077] Experimental Example 3:

[0078] The synthesis steps of the aldehyde trimethoxysilane coupling agent are as follows:

[0079] Step 1: p-Toluenesulfonic acid catalyzes the addition reaction of homovanillic acid and citronellal, which is based on the Markovnikov rule to generate phenolic hydroxyl aldehyde monomers;

[0080] Among them, the chemical structural formula of citronellal is:

[0081] ;

[0082] The chemical formula of phenolic hydroxy aldehyde monomer is:

[0083] ;

[0084] Step 2: Using the phenolic hydroxyl aldehyde monomer as a nucleophilic reagent, a nucleophilic substitution reaction occurs between the bromine functional group of 3-bromopropyltrimethoxysilane and the phenolic hydroxyl functional group of the phenolic hydroxyl aldehyde monomer to generate an aldehyde trimethoxysilane coupling agent;

[0085] Among them, the chemical structural formula of 3-bromopropyltrimethoxysilane is:

[0086] ;

[0087] The chemical structure of aldehyde trimethoxysilane coupling agent is:

[0088] ;

[0089] The specific experimental steps for preparing aldehyde trimethoxysilane coupling agent are as follows:

[0090] Under nitrogen protection, 1.8 g of homovanillic acid, 1.5 g of citronellal and 50 mL of N, N-dimethylformamide were added to a three-necked flask, heated to 30°C to dissolve, and then 10 mL of N, N-dimethylformamide solution containing 0.5 g of p-toluenesulfonic acid was added dropwise to the three-necked flask, heated to 70°C and stirred for reaction for 5 h, cooled to room temperature, and the solvent was removed by rotary evaporation, and a phenolic hydroxy aldehyde monomer was obtained after drying;

[0091] 1.7 g of phenolic hydroxyl aldehyde monomer, 1.4 g of potassium carbonate and 50 mL of acetone were added to a three-necked flask, heated to 30°C for dissolution for 1 h under nitrogen protection and mechanical stirring, and then 1 mL of 3-bromopropyltrimethoxysilane was added dropwise to the three-necked flask, heated to 70°C for reflux reaction for 8 h, filtered after cooling, washed with acetone and deionized water in turn, and dried in vacuo at 40°C for 12 h to obtain an aldehyde trimethoxysilane coupling agent;

[0092] The nuclear magnetic resonance hydrogen spectrum of the aldehyde trimethoxysilane coupling agent is characterized as follows: 1 H NMR (CDCl3, 400MHz) δ: 0.74-0.88(m, 2H), 0.92-0.94(d, 3H), 1.32-1.91(m, 15H), 2.22-2.40(m, 2H), 3 .56(s, 9H), 3.59-3.66(t, 2H), 3.80(s, 3H), 4.02-4.06(t, 2H), 6.82-6.87(m, 3H). Embodiment 1:

[0093] The preparation process of organic-inorganic hybrid anti-blocking agent I is as follows:

[0094] Modified SiO2 nanoparticles I are prepared, and the preparation method is as follows: SiO2 nanoparticles are modified by using phenolic hydroxy trimethoxy silane coupling agent, and the silanol functional groups obtained by hydrolysis reaction of the hydrolysis functional groups of the phenolic hydroxy trimethoxy silane coupling agent react with the hydroxyl functional groups on the surface of hydroxylated SiO2 nanoparticles (the preparation method is as follows) to undergo dehydration condensation reaction to prepare modified SiO2 nanoparticles I. The specific experimental steps are as follows: 5g of hydroxylated SiO2 nanoparticles, 20mL of deionized water and 80mL of anhydrous ethanol are added to a three-necked flask, stirred and dissolved at room temperature for 30min, and ultrasonically dispersed for 30min, and then 20mL of anhydrous ethanol solution dissolved with 3g of phenolic hydroxy trimethoxy silane coupling agent is added dropwise to the three-necked flask, and after the addition is complete, 2 drops of glacial acetic acid are added, the temperature is raised to 60°C and stirred for reaction for 4h, and the modified SiO2 nanoparticles I are obtained by repeated washing and suction filtration with anhydrous ethanol, and vacuum drying at 60°C for 10h.

[0095] The preparation method of hydroxylated SiO2 nanoparticles is as follows: 20g of nano-silicon dioxide zinc powder and 200mL of hydrogen peroxide aqueous solution (30wt%) are added to a round-bottom flask, and the mixture is uniformly dispersed by ultrasonication for 10min, and the mixture is heated to 105°C for reflux reaction for 6h under mechanical stirring, and then centrifuged at 5000rpm for 5min after cooling, and then washed with deionized water for 3 times, and finally dried under vacuum at 80°C for 5h to obtain hydroxylated SiO2 nanoparticles.

[0096] An organic-inorganic hybrid anti-blocking agent I was prepared. The preparation method was as follows: the phenolic hydroxyl functional group on the surface of the modified SiO2 nanoparticle I was hydrogen bonded with the amide functional group of stearic acid amide to compound the modified SiO2 nanoparticle I with stearic acid amide to prepare the organic-inorganic hybrid anti-blocking agent I. The specific experimental steps were as follows: 8 g of the modified SiO2 nanoparticle I, 20 mL of deionized water and 80 mL of anhydrous ethanol were added to a three-necked flask, stirred and dissolved at room temperature for 30 min, ultrasonically dispersed for 1 h, 20 mL of anhydrous ethanol solution containing 4 g of stearic acid amide was added dropwise to the three-necked flask, the temperature was raised to 60°C and stirred for reaction for 8 h, and the solvent was removed by rotary evaporation to obtain the organic-inorganic hybrid anti-blocking agent I. Embodiment 2:

[0097] The preparation process of organic-inorganic hybrid anti-blocking agent II is as follows:

[0098] Modified SiO2 nanoparticles II are prepared by the following preparation method: SiO2 nanoparticles are modified by using phenolic hydroxy trimethoxy silane coupling agent and aldehyde trimethoxy silane coupling agent together, and the silanol functional groups obtained by hydrolysis reaction of the hydrolyzed functional groups of the phenolic hydroxy trimethoxy silane coupling agent and the aldehyde trimethoxy silane coupling agent react with the hydroxyl functional groups on the surface of the hydroxylated SiO2 nanoparticles to prepare the modified SiO2 nanoparticles II. The specific experimental steps are referred to the preparation experiment of the modified SiO2 nanoparticles I, and the only difference is that 3g of the phenolic hydroxy trimethoxy silane coupling agent is replaced by 1.5g of the phenolic hydroxy trimethoxy silane coupling agent and 1.5g of the aldehyde trimethoxy silane coupling agent;

[0099] The modified MgAl-LDH nanosheets are prepared by a preparation method comprising: using a silane coupling agent KH540 and a phenolic hydroxyl di(trimethoxy)silane crosslinking agent to modify the MgAl-LDH nanosheets; a silanol functional group obtained by a hydrolysis reaction of the hydrolyzed functional groups of the silane coupling agent KH540 and the phenolic hydroxyl di(trimethoxy)silane crosslinking agent and a hydroxyl functional group on the surface of the MgAl-LDH nanosheets undergo a dehydration condensation reaction to prepare the modified MgAl-LDH nanosheets; and the specific experimental steps are: 5 g of the nanosheets are added to the MgAl-LDH nanosheets; and 10 g of the nanosheets are added to the MgAl-LDH nanosheets. MgAl-LDH powder, 20 mL of deionized water and 80 mL of anhydrous ethanol were added to a three-necked flask, stirred and dissolved at room temperature for 30 min, and ultrasonically dispersed for 1 h. Then, 20 mL of anhydrous ethanol solution containing 1.5 g of silane coupling agent KH540 and 1.5 g of phenolic hydroxybis(trimethoxy)silane crosslinking agent was added dropwise to the three-necked flask. After the addition was complete, 2 drops of glacial acetic acid were added, the temperature was raised to 60 ° C, stirred and reacted for 4 h, and the mixture was repeatedly washed and filtered with anhydrous ethanol, and vacuum dried at 60 ° C for 10 h to obtain modified MgAl-LDH nanosheets.

[0100] A MgAl-LDH / SiO2 composite material is prepared. The preparation method is as follows: the aldehyde functional group on the surface of the modified SiO2 nanoparticle II reacts with the amino functional group on the surface of the modified MgAl-LDH nanosheet to modify the SiO2 nanoparticle on the surface of the MgAl-LDH nanosheet to prepare the MgAl-LDH / SiO2 composite material. The specific experimental steps are as follows: 5g of the modified MgAl-LDH nanosheet, 20mL of deionized water and 80mL of anhydrous ethanol are added to a three-necked flask, stirred and dissolved at room temperature for 30min, and ultrasonically dispersed for 1h, then 4g of the modified SiO2 nanoparticle II is added to the three-necked flask, the temperature is raised to 60°C and stirred for reaction for 10h, the anhydrous ethanol is repeatedly washed and centrifuged, and the MgAl-LDH / SiO2 composite material is obtained.

[0101] An organic-inorganic hybrid anti-blocking agent II is prepared by hydrogen bonding the phenolic hydroxyl functional groups on the surface of the MgAl-LDH / SiO2 composite material with the amide functional groups of stearic acid amide, thereby compounding the modified SiO2 nanoparticles I with stearic acid amide, and compounding the MgAl-LDH / SiO2 composite material with stearic acid amide to obtain an organic-inorganic hybrid anti-blocking agent II. The specific experimental steps refer to the preparation experiment of the organic-inorganic hybrid anti-blocking agent I, and the only difference is that the modified SiO2 nanoparticles I are replaced by the MgAl-LDH / SiO2 composite material. Embodiment three:

[0102] (1) Preparing an eleven-layer co-extruded high barrier packaging film I, comprising the following steps:

[0103] Step 1: Set the eleven-layer co-extruded high barrier packaging film I to be an eleven-layer asymmetric film structure, and the formula and dosage of each film layer are as follows:

[0104] The first layer is a PE layer: its raw material formula is 60wt% LDPE and 40wt% LLDPE, and its usage is 10 parts by weight;

[0105] The second layer is a PE layer: its raw material formula is 40wt% HDPE and 60wt% LLDPE, and its usage is 5 parts by weight;

[0106] The third layer is a PE layer: its raw material formula is 40wt% LDPE and 60wt% LLDPE, and its usage is 10 parts by weight;

[0107] The fourth layer is a bonding layer: its raw material formula is 100wt% PE-g-MAH, and its usage is 5 parts by weight;

[0108] The fifth layer is a PA layer: its raw material formula is 100wt% PA, and its usage is 10 parts by weight;

[0109] The sixth layer is a barrier layer: its raw material formula is 100wt% EVOH, and its usage is 10 parts by weight;

[0110] The seventh layer is a PA layer: its raw material formula is 100wt% PA, and its usage is 10 parts by weight;

[0111] The eighth layer is a bonding layer: its raw material formula is 100wt% PE-g-MAH, and its usage is 5 parts by weight;

[0112] The ninth layer is a PE layer: its raw material formula is 40wt% LDPE and 60wt% LLDPE, and its usage is 10 parts by weight;

[0113] The tenth layer is a PE layer: its raw material formula is 40wt% HDPE and 60wt% LLDPE, and its usage is 5 parts by weight;

[0114] The eleventh layer is a PE layer: its raw material formula is 60wt% LDPE, 30wt% LLDPE and 10wt% organic-inorganic hybrid type opening agent I, and its usage is 20 parts by weight;

[0115] Step 2, respectively putting the raw materials in step 1 into the hoppers of eleven screw extruders of the eleven-layer co-extrusion film blow molding unit, after stirring and mixing, the molten resin is converged at the head of the die through a diverter, extruded and blown through a die head, cooled, and rolled to obtain an eleven-layer co-extruded high barrier packaging film I with a thickness of 100 μm;

[0116] Among them, the process parameters of the screw extruder corresponding to the PE layer are set as follows: the temperatures of zones 1-3 are 130°C, 150°C, and 180°C, respectively, the flow channel temperature is 175°C, and the speed is 30r / min;

[0117] The process parameters of the screw extruder corresponding to the bonding layer were set as follows: the temperatures of zones 1-3 were 125°C, 150°C, and 165°C, respectively, the flow channel temperature was 160°C, and the rotation speed was 15 r / min;

[0118] The process parameters of the screw extruder corresponding to the barrier layer were set as follows: the temperatures of zones 1-3 were 170°C, 180°C, and 210°C, respectively, the flow channel temperature was 205°C, and the rotation speed was 40r / min;

[0119] The process parameters of the screw extruder corresponding to the PA layer were set as follows: the temperatures of zones 1-3 were 200°C, 230°C, and 270°C, respectively, the flow channel temperature was 265°C, and the rotation speed was 60 r / min;

[0120] (2) Preparation of eleven-layer co-extruded high barrier packaging film II: Compared with the eleven-layer co-extruded high barrier packaging film I, the only difference is that the organic-inorganic hybrid type opening agent II replaces the organic-inorganic hybrid type opening agent I;

[0121] (3) Preparation of eleven-layer co-extruded high-barrier packaging film a: Compared with the eleven-layer co-extruded high-barrier packaging film I, the only difference is that the organic-inorganic hybrid anti-blocking agent I is not used, and it is used as a comparative example.

[0122] Performance Test:

[0123] (1) Use the MXD-01 friction coefficient tester to test the friction performance of the sample in accordance with GB / T 10006-2021 and record the friction coefficient of the sample;

[0124] (2) Test the anti-adhesion performance of the sample in accordance with GB / T 39935-2021. Place the sample in an oven and load it with 5.4 kg to ensure a uniform pressure of 7 kPa. Keep it at 50 °C for 24 h. After that, remove the load and observe whether the sample is separated after 4 h.

[0125] (3) Use the Y110 oxygen permeability tester to test the oxygen barrier properties of the sample in accordance with GB / T 1038-2000 and record the oxygen permeability of the sample;

[0126] (4) Use TC-03 water vapor transmission tester to test the water barrier properties of the sample in accordance with GB / T 1037-2021 and record the water vapor transmission rate of the sample;

[0127] (5) The sample was heat-sealed using an HSG-C heat sealer with a sealing area of ​​15 cm × 1 cm, a heat-sealing temperature of 135 °C, a heat-sealing pressure of 0.2 MPa, and a heat-sealing time of 2.0 s.

[0128] According to QB / T 2358-1998 "Test Method for Heat Seal Strength of Plastic Film Packaging Bags", the heat seal performance of the heat seal sample was tested at a test speed of 300mm / min and a clamp spacing of 50mm. The heat seal strength of the sample was recorded.

[0129] (6) The mechanical properties of the samples were tested using an Instron 5565 universal tensile testing machine. The specific test steps are as follows: a 150 mm × 20 mm sample was fixed on the tensile testing machine, and a tensile test was performed at a tensile rate of 5 mm / min. The longitudinal and transverse tensile strengths of the samples were recorded.

[0130] The above experimental results are shown in Tables 1 and 2 below.

[0131] Table 1 Experimental results of friction and barrier properties of eleven-layer coextruded high barrier packaging film

[0132]

[0133] Table 2 Experimental results of heat sealing and mechanical properties of eleven-layer coextruded high barrier packaging film

[0134]

[0135] According to the friction performance test data in Table 1, Figure 1 , through comprehensive analysis of the above experimental results, we can draw the following conclusions:

[0136] Conclusion 1: The organic-inorganic hybrid anti-blocking agent developed by the present invention significantly reduces the friction coefficient of the eleven-layer co-extruded high barrier packaging film. The eleven-layer co-extruded high barrier packaging film prepared thereby exhibits excellent anti-adhesion performance and is a highly slippery and easy-to-cut material.

[0137] Conclusion 2: The organic-inorganic hybrid anti-blocking agent developed by the present invention can improve the barrier properties of the eleven-layer co-extruded high-barrier packaging film;

[0138] The heat sealing strength of the eleven-layer co-extruded high barrier packaging film prepared by the present invention is significantly greater than the requirement of JB / T9086-2007 "Plastic Bag Hot Press Sealing Machine" regarding the sealing strength ≥ 15N (material thickness R, 0.08mm≤R<0.18mm);

[0139] Conclusion 3: Compared with organic-inorganic hybrid anti-blocking agent I, organic-inorganic hybrid anti-blocking agent II has a more significant improvement on the comprehensive performance of the eleven-layer co-extruded high barrier packaging film.

Claims

1. A method for preparing an eleven-layer co-extruded high-barrier packaging film that is easy to cut, characterized in that: The following steps are involved: Step 1: preparing an organic-inorganic hybrid type opening agent, the organic-inorganic hybrid type opening agent is an organic-inorganic hybrid type opening agent I or an organic-inorganic hybrid type opening agent II, and the specific process is as follows: preparing a silane coupling agent containing a phenolic hydroxyl functional group, a silane coupling agent containing an aldehyde functional group and a silane crosslinking agent containing a phenolic hydroxyl functional group; The chemical structural formula of the silane coupling agent containing a phenolic hydroxyl functional group is: ; The preparation method of the silane coupling agent containing a phenolic hydroxyl functional group comprises: utilizing a nucleophilic substitution reaction mechanism, using p-toluenesulfonic acid to catalyze a carboxyl functional group of homovanillic acid and a mercapto functional group of 3-mercaptopropyltrimethoxysilane to cause a thioesterification reaction, thereby preparing the silane coupling agent containing a phenolic hydroxyl functional group; The chemical structural formula of the silane coupling agent containing an aldehyde functional group is: ; The preparation method of the silane coupling agent containing the aldehyde functional group is: Based on the Markovnikov rule of oriented electrophilic addition reaction of olefins, the strong acid catalyst catalyzes the addition reaction of homovanillic acid and citronellal to generate phenolic hydroxyl aldehyde monomers. A silane coupling agent containing an aldehyde functional group is prepared by using a phenolic hydroxyl aldehyde monomer as a nucleophilic reagent and reacting the bromine functional group of 3-bromopropyltrimethoxysilane with the phenolic hydroxyl functional group of the phenolic hydroxyl aldehyde monomer to undergo a nucleophilic substitution reaction; The chemical structural formula of the silane crosslinking agent containing phenolic hydroxyl functional groups is: ; The preparation method of the silane crosslinking agent containing phenolic hydroxyl functional groups comprises: utilizing a nucleophilic substitution reaction mechanism, under the promotion of an activator, catalyzing an acylation reaction between a carboxyl functional group of homovanillic acid and a secondary amine group of di(3-trimethoxysilylpropyl)amine by an organic base, and preparing the silane crosslinking agent containing phenolic hydroxyl functional groups; The method for preparing the organic-inorganic hybrid opening agent I is: Modifying the surface of the hydroxyl-functionalized zero-dimensional inorganic opening agent SiO2 with a silane coupling agent containing a phenolic hydroxyl functional group to obtain a phenolic hydroxylated zero-dimensional inorganic opening agent SiO2; The phenolic hydroxylated zero-dimensional inorganic opening agent SiO2 was compounded with the organic opening agent stearic acid amide through hydrogen bonding to prepare the organic-inorganic hybrid opening agent Ⅰ; The method for preparing the organic-inorganic hybrid type opening agent II is: Simultaneously modifying the surface of the hydroxyl-functionalized zero-dimensional inorganic opening agent SiO2 with a silane coupling agent containing a phenolic hydroxyl functional group and a silane coupling agent containing an aldehyde functional group, thereby obtaining an aldehyde-functionalized phenolic hydroxyl-functionalized zero-dimensional inorganic opening agent SiO2; The silane coupling agent KH540 and the silane crosslinking agent containing phenolic hydroxyl functional groups are simultaneously modified on the surface of the two-dimensional inorganic opening agent MgAl-LDH rich in hydroxyl functional groups to obtain the amino-phenolic hydroxylated two-dimensional inorganic opening agent MgAl-LDH; The aldehyde-hydroxylated phenolic zero-dimensional inorganic opening agent SiO2 and the amino-hydroxylated phenolic two-dimensional inorganic opening agent MgAl-LDH are compounded by Schiff base reaction to prepare a composite inorganic opening agent. The composite inorganic anti-blocking agent is compounded with the organic anti-blocking agent stearic acid amide through hydrogen bonding to prepare an organic-inorganic hybrid anti-blocking agent II; Step 2: Set up the film structure of the eleven-layer co-extruded film, introduce the organic-inorganic hybrid anti-blocking agent into the eleventh layer of the eleven-layer co-extruded film, the eleventh layer is a PE layer, and adopt the eleven-layer co-extrusion blow molding film forming process to prepare an easy-to-cut eleven-layer co-extruded high barrier packaging film.

2. The method for preparing an easy-to-cut eleven-layer co-extruded high-barrier packaging film according to claim 1, characterized in that: The formula of the organic-inorganic hybrid opening agent I is: the mass ratio of the inorganic opening agent SiO2 to the organic opening agent is 1: (0.1-2); The formula of the organic-inorganic hybrid opening agent II is as follows: the mass ratio of the composite inorganic opening agent to the organic opening agent is 1:(0.1-2), and the mass ratio of the inorganic opening agent SiO2 to the inorganic opening agent MgAl-LDH in the composite inorganic opening agent is 1:(0.5-2).

3. The method for preparing an easy-to-cut eleven-layer co-extruded high-barrier packaging film according to claim 1, characterized in that: The eleven-layer co-extruded high barrier packaging film has an asymmetric structure, and the formula and dosage of each film layer are as follows: The first layer is a PE layer: its raw material formula is 40~80wt% LDPE and 20~60wt% LLDPE, and its usage is 5~15 parts by weight; The second layer is a PE layer: its raw material formula is 20~60wt% HDPE and 40~80wt% LLDPE, and its usage is 3~10 parts by weight; The third layer is a PE layer: its raw material formula is 20~60wt% LDPE and 40~80wt% LLDPE, and its usage is 5~15 parts by weight; The fourth layer is a bonding layer: its raw material formula is 100wt% PE-g-MAH, and its usage is 2-8 parts by weight; The fifth layer is a PA layer: its raw material formula is 100wt% PA, and its usage is 5-15 parts by weight; The sixth layer is a barrier layer: its raw material formula is 100wt% EVOH, and its usage is 5-15 parts by weight; The seventh layer is a PA layer: its raw material formula is 100wt% PA, and its usage is 5-15 parts by weight; The eighth layer is a bonding layer: its raw material formula is 100wt% PE-g-MAH, and its usage is 2-8 parts by weight; The ninth layer is a PE layer: its raw material formula is 20-60wt% LDPE and 40-80wt% LLDPE, and its usage is 5-15 parts by weight; The tenth layer is a PE layer: its raw material formula is 20-60wt% HDPE and 40-80wt% LLDPE, and its usage is 3-10 parts by weight; The eleventh layer is a PE layer: its raw material formula is 40-70wt% LDPE, 20-40wt% LLDPE and 5-20wt% organic-inorganic hybrid opening agent, and its usage is 10-30 parts by weight.

4. The method for preparing an eleven-layer co-extruded high barrier packaging film that is easy to cut according to claim 1, characterized in that: The strong acid catalyst is one of sulfuric acid, p-toluenesulfonic acid and fluoroboric acid.

5. The method for preparing an easy-to-cut eleven-layer co-extruded high-barrier packaging film according to claim 1, characterized in that: The activator is one of N,N'-dicyclohexylcarbodiimide, 1-hydroxybenzotriazole, N-hydroxy-7-azabenzotriazole, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride.

6. The method for preparing an eleven-layer co-extruded high barrier packaging film that is easy to cut according to claim 1, characterized in that: The organic base is one of pyridine, triethylamine, tributylamine and imidazole.

7. An easy-to-cut eleven-layer co-extruded high-barrier packaging film prepared by the method according to any one of claims 1 to 6, characterized in that: The eleven-layer co-extruded high-barrier packaging film is applied on an industrial automatic high-speed packaging production line.