A preparation and purification process of modified quartz sand

Through crushing, grinding, roasting, pickling and magnetic separation, combined with acid solution treatment, high-purity, antibacterial modified quartz sand is prepared, which solves the problems of insufficient impurity removal and antibacterial properties of quartz sand in the prior art, and realizes the The efficient purification of quartz sand and the improvement of antibacterial ability.

CN118790996BActive Publication Date: 2024-12-03JIANGSU XINYIDING QUARTZ TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411276779.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-03
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The existing quartz sand purification methods are difficult to effectively remove impurities in quartz, especially Al elements, and fail to impart antibacterial properties to quartz sand, limiting its application in certain fields.

Method used

After crushing, grinding, sieving and calculating quartz fragments, the acid treatment and magnetic separation treatment are carried out to reduce the content of impurities and add composite antibacterial agent to the functionalized primary quartz sand to prepare modified quartz sand. . This process includes roasting, pickling and magnetic separation steps, combining the mixed acid solution and composite antibacterial agent to significantly reduce the content of impurity elements such as Fe, Al, K, Na, Ca, Ti, etc., and impart antibacterial ability to quartz sand.

Benefits of technology

High purity purification of quartz sand was achieved, the SiO2 purity reached 99.67%, the Fe element content decreased by 79.5%, and it had a significant inhibitory effect on E. coli and Staphylococcus aureus, expanding the application field of quartz sand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118790996B_ABST
    Figure CN118790996B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of quartz sand, and in particular to a preparation and purification process of modified quartz sand. The invention prepares a quartz sample by roasting, performs subsequent acid treatment and magnetic separation treatment, obtains primary quartz sand, and after functionalization, adds a composite antibacterial agent to prepare modified quartz sand. After roasting first, the content of impurity elements in the quartz sand can be reduced, thereby achieving the purpose of purifying the quartz sand. Through acid washing, the removal effect on aluminum is most obvious, and the removal rate reaches 71.1%. By controlling the mixed acid ratio, the SiO2 purity of the modified quartz sand can be 99.67%. After subsequent magnetic separation treatment, the Fe element content in the modified quartz sand is reduced by 79.5%. Finally, the prepared primary quartz sand is combined with the composite antibacterial agent to prepare modified quartz sand with antibacterial effect, which has an inhibitory effect on Escherichia coli and Staphylococcus aureus.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quartz sand, in particular to a preparation and purification process of modified quartz sand. Background Art

[0002] Quartz sand is a widely used industrial raw material, and its main chemical composition is SiO2. It has an irreplaceable position in the fields of glass, ceramics, building materials, semiconductor chips, optical fiber communications, etc. However, natural quartz sand contains a large amount of impurities, which limits its application in some fields. Therefore, it is of great significance to modify and purify quartz sand. Some of the impurities in quartz exist in the internal inclusions of quartz, and some exist in the quartz lattice, especially Al element, which has high abundance and atomic radius similar to Si. These impurities will greatly affect the properties and applications of quartz. The existing high-purity quartz purification methods mainly include the following: magnetic separation, flotation, high-temperature calcination and acid washing. Although some impurities in quartz sand can be removed to a certain extent, there are still technical barriers.

[0003] For example, in the literature Zijie Ren, Zhi Liu, Yuhang Liu, Huimin Gao, Feida Wu and Yuhan Song. The Effects of Calcination-Water Quenching on Quartz Purificationand Its Mechanism. Mining, Metallurgy & Exploration, 2023, 40, 2519–2527., quartz sand was purified by calcination and water quenching, and the different expansion rates of gangue minerals and quartz were used to produce cracks to remove fluid inclusions, and the position of calcination-water quenching in the gangue quartz purification process was adjusted. The results showed that the grinding-calcination-water quenching-classification-acid leaching process and the grinding-classification-acid leaching-calcination-water quenching process had better purification effects. Calcination-water quenching will cause cracks in quartz, and calcination-water quenching is located after grinding. The final prepared quartz sand has a large specific surface area, pore volume and pore size, and has a strong adsorption capacity for acidic solutions. However, there is no targeted removal of metal Al in this literature. Another document Yubiao Li, QiangMa, Zhangjie Xia, Wanqing Li, Shaomin Lei. Influences of Na2CO3 roasting andH3PO4 hot-pressure leaching on the purification of vein quartz to achievehigh-purity quartz. Hydrometallurgy, 2023, 218, 106065. produced high-purity quartz and established a combined process of Na2CO3 roasting and double H3PO4 hot-pressure leaching. The roasting pretreatment destroys the muscovite crystal structure, which is conducive to the dissolution of impurities in the subsequent H3PO4 hot-pressure leaching process. Finally, the selective removal of impurities in quartz is achieved. However, the purification method in this document lacks a magnetic separation step, and is not efficient for the removal of magnetic iron-containing impurities. Chinese invention patent CN202111445804.9 discloses a method for preparing high-purity quartz sand, which improves the problems of large amounts of exogenous impurities introduced by crushing and grinding, and high energy consumption of roasting and water quenching in traditional processes. However, the prepared high-purity quartz sand does not have antibacterial properties and its application is limited in some fields.

[0004] In addition, water or -OH in quartz sand will reduce the high temperature resistance of quartz sand, so consuming hydroxyl groups to achieve the modification of quartz sand has high application value. However, a single method cannot remove the internal inclusions and internal impurities of quartz.

[0005] Therefore, a preparation and purification process of modified quartz sand is proposed. Summary of the invention

[0006] The object of the present invention is to provide a preparation and purification process of modified quartz sand, wherein a quartz sample prepared by crushing, grinding, screening and roasting quartz fragments is subjected to subsequent acid treatment and magnetic separation treatment, and the surface of the obtained primary quartz sand is functionalized, and a composite antibacterial agent is added to form the modified quartz sand. After roasting first, the content of impurity elements in the quartz sand can be reduced, wherein the Fe content decreases by 22.8%, the Al content decreases by 33.9%, the K content decreases by 54%, the Na content decreases by 38.4%, the Ca content decreases by 58.1%, and the Ti content decreases by 46.7%. Through pickling, the removal effect on aluminum is most obvious, and the removal rate reaches 71.1%. By controlling the mixed acid ratio, the SiO2 purity of the modified quartz sand can be 99.67%. After subsequent magnetic separation treatment, the Fe element content in the modified quartz sand is reduced by 79.5%. Finally, the obtained primary quartz sand is coupled with the composite antibacterial agent to prepare modified quartz sand with antibacterial effect, which has an inhibitory effect on Escherichia coli and Staphylococcus aureus.

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solutions. On the one hand, the present invention provides a preparation and purification process of modified quartz sand, comprising the following steps: loading quartz fragments into a crusher to crush them into quartz particles and washing them with deionized water; grinding and screening the quartz particles to obtain a quartz sample; placing the quartz sample in a crucible, placing the crucible in the furnace of a pit furnace and roasting at 600-1000°C for 5 hours.

[0008] A mixed acid solution of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid is added to the calcined quartz sample, and the mixture is soaked at a temperature of 20-70°C for 2-8 hours to obtain a turbid solution; in the mixed acid solution, the hydrochloric acid accounts for 10%-20% of the total volume of the mixed acid solution; the sulfuric acid accounts for 25%-30% of the total volume of the mixed acid solution; the nitric acid accounts for 15%-30% of the total volume of the mixed acid solution; the hydrofluoric acid accounts for 10%-15% of the total volume of the mixed acid solution; and the oxalic acid accounts for 10%-20% of the total volume of the mixed acid solution; the turbid solution is centrifuged and the waste acid solution is recovered to obtain a quartz precipitate; the quartz precipitate is washed with deionized water until neutral, and then washed with ethanol, centrifuged, and dried to obtain pretreated quartz sand, which is stored for later use.

[0009] The pretreated quartz sand is placed in a magnetic separator for magnetic separation treatment; the magnetic field intensity of the magnetic separation treatment is 50-250mT, and after the treatment is completed, the primary quartz sand is dried.

[0010] Concentrated nitric acid is added to the primary quartz sand to obtain a quartz sand acid solution; the quartz sand acid solution is placed in a flask, heated to 85°C, and refluxed in an oil bath for 28 hours to obtain a suspension; the suspension is centrifuged to separate solids; the solids are washed with deionized water until neutral to obtain carboxyl quartz sand; the carboxyl quartz sand is dispersed in deionized water, 3-aminopropyltriethoxysilane is added thereto, and after stirring and reacting at 37°C for 14 hours, centrifugation and drying are performed to obtain amino quartz sand; a composite antibacterial agent, a surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution; the reaction solution is continuously stirred at 70°C for 16 hours, centrifuged and dried to obtain the modified quartz sand.

[0011] Preferably, the screening process is to screen out quartz samples with a particle size of 100-800um on an electric vibrating screen.

[0012] Preferably, the solid-liquid ratio of the calcined quartz sample to the acid solution is 1 g:1-10 mL.

[0013] Preferably, the concentration of the quartz sand acid solution is 0.1 g / mL.

[0014] Preferably, the molar ratio of the carboxy quartz sand to the 3-aminopropyltriethoxysilane is 1:1-1.5.

[0015] Preferably, the mass ratio of the amino quartz sand to the composite antibacterial agent is 100:1-10.

[0016] Preferably, the composite antibacterial agent is a combination of silver nitrate: quaternary ammonium salt: vanillin in a mass ratio of 1:1:1.

[0017] On the other hand, the present invention provides a modified quartz sand, characterized in that: the modified quartz sand is a quartz sample prepared by crushing, grinding, screening and calcining quartz fragments, and then subjected to acid treatment and magnetic separation treatment. After the surface of the obtained primary quartz sand is functionalized, a composite antibacterial agent is added. The modified quartz sand is prepared and purified by the preparation and purification process as described above; the content of impurity elements in the modified quartz sand is generally reduced, wherein the Fe content is reduced by 22.8%, the Al content is reduced by 33.9%, the K content is reduced by 54%, and the Na content is reduced by 1.3%. The content of Fe decreased by 38.4%, the content of Ca decreased by 58.1%, and the content of Ti decreased by 46.7%; during the purification of the modified quartz sand, the pickling temperature was 70°C, the pickling time was 5 hours, and the removal rate of metallic aluminum in the obtained modified quartz sand was 71.1%; the SiO2 purity of the modified quartz sand was 99.67%; the modified quartz sand was treated by magnetic separation to reduce the content of Fe by 79.5%; the modified quartz sand had antibacterial ability, with an inhibition rate of 99.8% on Escherichia coli and 99.7% on Staphylococcus aureus.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. In the present invention, the quartz fragments are crushed and rinsed with deionized water, and then ground and screened to screen out a quartz sample with a particle size of 300-500um and place it in a crucible, and then roasted at 900°C in a pit furnace for 5 hours. The quartz sample prepared by the roasting method is subsequently treated with acid and magnetic separation, and the surface of the obtained primary quartz sand is functionalized, and a composite antibacterial agent is added to prepare modified quartz sand. After roasting first, the content of impurity elements in quartz sand can be generally reduced, wherein the Fe content decreases by 22.8%, the Al content decreases by 33.9%, the K content decreases by 54%, the Na content decreases by 38.4%, the Ca content decreases by 58.1%, and the Ti content decreases by 46.7%, thereby achieving the purpose of purifying the original quartz. This is because quartz undergoes a phase transition when roasted at high temperature, which is manifested as the volume expansion of the quartz matrix, the internal inclusions bursting under heat, and some atomic impurities diffuse to the surface of the quartz particles due to thermal motion, which is convenient for purification by subsequent acid treatment. However, since the atomic structures of Al and Si are similar, some aluminum atoms are located inside the crystal lattice, making it difficult to remove them using a single method. Subsequent pickling can reduce the Al content.

[0019] 2. The present invention adds a mixed acid solution to the calcined quartz sample, the solid-liquid ratio of the quartz sample to the acid solution is 1g:8mL, soaks at a temperature of 70°C for 5 hours to obtain a turbid solution, centrifuges the turbid solution and recovers the waste acid solution to obtain a quartz precipitate, washes the quartz precipitate with deionized water to neutrality, and then washes it with ethanol, centrifuges it, and dries it to obtain pretreated quartz sand. The quartz sand obtained by the above pickling steps has the most obvious effect on the removal of metallic aluminum. In particular, when the pickling temperature is 70°C and the pickling time is 5 hours, the removal rate of metallic aluminum in the obtained quartz sand reaches 71.1%. The present invention removes most of the metal impurities on the surface of quartz by first roasting the initial quartz sand and then pickling it. The principle is that quartz does not react with acids other than hydrofluoric acid, and other impurity metals can be dissolved by acid and converted into ionic states, thereby further purifying the quartz sand. In addition, the present invention can improve the removal efficiency by controlling the temperature and time of pickling, and the maximum removal rate of aluminum can reach 71.1%. The removal effect of aluminum by roasting alone is poor, so the combination of roasting and pickling can remove the aluminum element in quartz sand to the greatest extent.

[0020] 3. In the mixed acid solution of the present invention, hydrochloric acid accounts for 15% of the total volume of the acid solution, sulfuric acid accounts for 25% of the total volume of the acid solution, nitric acid accounts for 30% of the total volume of the acid solution, hydrofluoric acid accounts for 15% of the total volume of the acid solution, and oxalic acid accounts for 15% of the total volume of the acid solution. By adopting the above-mentioned mixed acid ratio, the purity of SiO2 in the finally prepared modified quartz sand can reach 99.67%, meeting the refined quartz sand level (99.5% < SiO2 purity < 99.995%). The present invention can remove most of the impurity metals to obtain high-purity quartz sand by first roasting and then pickling. Moreover, the present invention adds organic acid oxalic acid to the mixed acid, and uses the -COOH group of oxalic acid to combine with transition metals to form complexes or coordination compounds, so as to achieve the purpose of removing impurity metal elements. Compared with a single type of acid, using a mixed acid solution and controlling the ratio of the mixed acid can play a synergistic effect, resulting in a higher impurity removal rate and a greater purity of the main body SiO2 in the quartz sand. The pickling method provided by the present invention can purify quartz ore to the refined quartz sand level.

[0021] 4. The present invention places the pretreated quartz sand in a magnetic separator for magnetic separation treatment. The magnetic field intensity of the magnetic separation treatment is 200 mT, and the number of magnetic separation times is 3 times. After the treatment, it is dried to obtain primary quartz sand. The primary quartz sand obtained by the above method is further modified. The content of Fe element in the finally prepared modified quartz sand decreases by 79.5%. The present invention utilizes the non-magnetic property of quartz and the magnetic property of iron-containing impurity minerals to remove the enriched magnetic impurity Fe in the quartz sand by magnetic separation. In addition, the number of magnetic separation times also affects the decrease in the content of Fe element. The more the number of magnetic separation times, the greater the decrease in the content of Fe element.

[0022] 5. The present invention adds concentrated nitric acid to the primary quartz sand, heats it to 85 °C, refluxes it in an oil bath for 28 hours, centrifuges and washes it to neutral to obtain carboxyl quartz sand. The carboxyl quartz sand is dispersed in deionized water, and 3-aminopropyltriethoxysilane is added. The molar ratio of carboxyl quartz sand to 3-aminopropyltriethoxysilane is 1:1.3. It is stirred and reacted at 37 °C for 13 hours, centrifuged and dried to obtain amino quartz sand; compound antibacterial agent, surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution. The mass ratio of amino quartz sand to the compound antibacterial agent is 100:5. The compound antibacterial agent is a combination of silver nitrate: quaternary ammonium salt: vanillin in a mass ratio of 1:1:1. The reaction solution is stirred at 70 °C for 16 hours, centrifuged and dried to obtain modified quartz sand. The modified quartz sand prepared by the above method has antibacterial ability, with an inhibition rate of 99.8% against Escherichia coli and an inhibition rate of 99.7% against Staphylococcus aureus. The present invention functionalizes the prepared primary quartz sand by refluxing it with concentrated nitric acid, consumes the -OH of the quartz sand, and combines it with the compound antibacterial agent to prepare modified quartz sand with antibacterial effects, which has inhibitory effects on common bacteria Escherichia coli and Staphylococcus aureus, enriching the application fields of quartz. Description of the Drawings

[0023] Figure 1 The invention discloses an effect of the ratio of mixed acid during pickling on the purity of the final quartz sand SiO2. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] See also Figure 1 The present invention provides a preparation and purification process of modified quartz sand, and the technical scheme is as follows.

[0026] Example 1

[0027] A preparation and purification process of modified quartz sand comprises the following steps.

[0028] The quartz fragments are put into a crusher to be crushed into quartz particles and rinsed with deionized water; the quartz particles are ground and screened, that is, quartz samples with a particle size of 100-300um are screened out on an electric vibrating screen; the quartz sample is placed in a crucible, and the crucible is placed in the furnace of a pit furnace and roasted at 600°C for 5 hours.

[0029] A mixed acid solution of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid is added to the calcined quartz sample, wherein the solid-liquid ratio of the calcined quartz sample to the acid solution is 1 g:1 mL; in the mixed acid solution, hydrochloric acid accounts for 20% of the total volume of the acid solution, sulfuric acid accounts for 30% of the total volume of the acid solution, nitric acid accounts for 20% of the total volume of the acid solution, hydrofluoric acid accounts for 10% of the total volume of the acid solution, and oxalic acid accounts for 20% of the total volume of the acid solution, and the mixture is soaked at a temperature of 20° C. for 2 hours to obtain a turbid solution; the turbid solution is centrifuged and the waste acid solution is recovered to obtain a quartz precipitate; the quartz precipitate is washed with deionized water until neutral, and then washed with ethanol, centrifuged, and dried to obtain pretreated quartz sand, which is stored for standby use.

[0030] The pretreated quartz sand is placed in a magnetic separator for magnetic separation treatment; the magnetic field intensity of the magnetic separation treatment is 50mT, and after the treatment is completed, the primary quartz sand is dried to obtain.

[0031] Concentrated nitric acid is added to primary quartz sand to obtain a quartz sand acid solution with a concentration of 0.1 g / mL; the quartz sand acid solution is placed in a flask, heated to 85°C, and refluxed in an oil bath for 28 hours to obtain a suspension; the suspension is centrifuged to separate solids; the solids are washed with deionized water until neutral to obtain carboxyl quartz sand; the carboxyl quartz sand is dispersed in deionized water, 3-aminopropyltriethoxysilane is added thereto, the molar ratio of the carboxyl quartz sand to the 3-aminopropyltriethoxysilane is 1:1, after stirring and reacting at 37°C for 13 hours, centrifugation and drying are performed to obtain amino quartz sand; a composite antibacterial agent, a surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution, the mass ratio of the amino quartz sand to the composite antibacterial agent is 100:1; the composite antibacterial agent is silver nitrate: quaternary ammonium salt: vanillin added in a mass ratio of 1:1:1; the reaction solution is continuously stirred at 70°C for 16 hours, centrifuged and dried to obtain modified quartz sand.

[0032] The quartz fragments used in the examples of the present invention were produced in Fengyang, Anhui Province. The remaining chemical reagents can be purchased through conventional channels. The purity of the solvents used was analytical grade.

[0033] Comparative Example 1

[0034] The calcination step was not performed, and the remaining reagents and operations were the same as in Example 5.

[0035] The particle size range of the quartz samples screened in Examples 2-8 and the calcination temperature of the pit furnace are shown in Table 1 below. The remaining reagents and operations are the same as in Example 1.

[0036] Table 1 Particle size range of quartz samples in Examples 2-8 and calcination temperature of pit furnace

[0037]

[0038] Example 9

[0039] For the modified quartz sand prepared in the above Examples 1-8 and Comparative Example 1, ICP-OES was used to detect common impurity elements and their contents in quartz. The results are shown in Table 2.

[0040] In Example 5, the quartz fragments are crushed and rinsed with deionized water, and then ground and screened. A quartz sample with a particle size of 300-500um is screened out on an electric vibrating screen and placed in a crucible. The crucible is placed in the furnace of a pit furnace and roasted at 900°C for 5 hours. The quartz sample prepared by the roasting method is subsequently treated with acid and magnetically separated. After the surface of the obtained primary quartz sand is functionalized, a composite antibacterial agent is added to prepare modified quartz sand. The removal rates of various metal impurities in the prepared modified quartz sand are shown in Table 2. It can be seen that the content of impurity elements in quartz sand can be generally reduced by calcining first. In the method of Example 5, the particle size of the quartz sample is in the range of 300-500um, and the calcination temperature is 900℃, which can make the Fe content of the modified quartz sand prepared finally reduced by 22.8% compared with the original sample without any treatment; the Al content is reduced by 33.9%; the K content is reduced by 54%; the Na content is reduced by 38.4%; the Ca content is reduced by 58.1%; and the Ti content is reduced by 46.7%, thereby achieving the purpose of purifying the original quartz. This is because quartz undergoes a phase transition when calcined at high temperature, which is manifested as the volume expansion of the quartz matrix, causing the internal inclusions to burst due to heat, and some atomic impurities will diffuse to the surface of the quartz particles due to thermal motion, which is convenient for purification by subsequent acid treatment. However, Comparative Example 1 does not undergo a calcination step, and the proportion of the reduction in the content of impurity elements in the prepared quartz sand is very small, indicating that the present invention can reduce the content of impurities in quartz by high-temperature calcination. However, since the atomic structures of Al and Si are similar, some aluminum atoms are located inside the crystal lattice, making it difficult to remove them using a single method. Subsequent pickling can reduce the Al content.

[0041] Table 2 Common impurity element contents in modified quartz sand prepared in Examples 1-8 and Comparative Example 1 (ppm)

[0042]

[0043] Example 10

[0044] A preparation and purification process of modified quartz sand comprises the following steps.

[0045] The quartz fragments are put into a crusher to be crushed into quartz particles and rinsed with deionized water; the quartz particles are ground and screened, that is, quartz samples with a particle size of 300-500um are screened out on an electric vibrating screen; the quartz sample is placed in a crucible, and the crucible is placed in the furnace of a pit furnace and roasted at 900°C for 5 hours.

[0046] A mixed acid solution of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid is added to the calcined quartz sample, wherein the solid-liquid ratio of the calcined quartz sample to the acid solution is 1 g:2 mL; in the mixed acid solution, hydrochloric acid accounts for 20% of the total volume of the acid solution, sulfuric acid accounts for 30% of the total volume of the acid solution, nitric acid accounts for 20% of the total volume of the acid solution, hydrofluoric acid accounts for 10% of the total volume of the acid solution, and oxalic acid accounts for 20% of the total volume of the acid solution, and the mixture is soaked at a temperature of 30° C. for 4 hours to obtain a turbid solution; the turbid solution is centrifuged and the waste acid solution is recovered to obtain a quartz precipitate; the quartz precipitate is washed with deionized water until neutral, and then washed with ethanol, centrifuged, and dried to obtain pretreated quartz sand, which is stored for standby use.

[0047] The pretreated quartz sand is placed in a magnetic separator for magnetic separation treatment; the magnetic field intensity of the magnetic separation treatment is 50mT, and after the treatment is completed, the primary quartz sand is dried to obtain.

[0048] Concentrated nitric acid is added to primary quartz sand to obtain a quartz sand acid solution with a concentration of 0.1 g / mL; the quartz sand acid solution is placed in a flask, heated to 85°C, and refluxed in an oil bath for 28 hours to obtain a suspension; the suspension is centrifuged to separate solids; the solids are washed with deionized water until neutral to obtain carboxyl quartz sand; the carboxyl quartz sand is dispersed in deionized water, 3-aminopropyltriethoxysilane is added thereto, the molar ratio of the carboxyl quartz sand to the 3-aminopropyltriethoxysilane is 1:1, after stirring and reacting at 37°C for 13 hours, centrifugation and drying are performed to obtain amino quartz sand; a composite antibacterial agent, a surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution, the mass ratio of the amino quartz sand to the composite antibacterial agent is 100:1; the composite antibacterial agent is silver nitrate: quaternary ammonium salt: vanillin added in a mass ratio of 1:1:1; the reaction solution is continuously stirred at 70°C for 16 hours, centrifuged and dried to obtain modified quartz sand.

[0049] The solid-to-liquid ratio of the calcined quartz sample to the acid solution, the immersion temperature and time in Examples 11-19 are shown in Table 3, and the remaining reagents and operations are the same as in Example 10.

[0050] Table 3 Solid-to-liquid ratio of quartz sample and acid solution after calcination, immersion temperature and time in Examples 11-19

[0051]

[0052] Comparative Example 2

[0053] No mixed acid solution immersion treatment is used, that is, the pickling step is removed, and the remaining reagents and operations are the same as in Example 18.

[0054] Embodiment 20

[0055] The modified quartz sand samples prepared in the above Examples 10-19 and Comparative Example 2 were tested for changes in aluminum content using an ICP-OES instrument, and the aluminum removal rate was calculated. The results are shown in Table 4.

[0056] In Example 18, a mixed acid solution is added to the calcined quartz sample, and the solid-liquid ratio of the quartz sample to the acid solution is 1g:8mL; a turbid solution is obtained by soaking at a temperature of 70°C for 5 hours, the turbid solution is centrifuged and the waste acid solution is recovered to obtain a quartz precipitate, the quartz precipitate is washed with deionized water to neutrality, and then washed with ethanol, centrifuged, and dried to obtain pretreated quartz sand. The quartz sand obtained by the above pickling steps has the most obvious removal effect on metallic aluminum. In particular, when the pickling temperature is 70°C and the pickling time is 5 hours, the removal of metallic aluminum in the obtained quartz sand can reach 71.1%. The present invention removes most of the metal impurities on the surface of quartz by first roasting the initial quartz sand and then pickling it. The principle is that quartz does not react with acids other than hydrofluoric acid, and other impurity metals can be dissolved by acid and converted into ionic states, thereby further purifying the quartz sand. In addition, the present invention can improve the removal efficiency by controlling the temperature and time of pickling, and the maximum removal rate of aluminum can reach 71.1%. In Comparative Example 2, the mixed acid solution immersion treatment is not used, that is, the pickling step is removed, and the aluminum removal rate in the prepared quartz sand is the lowest, which is 15.2%, and the purification effect is poor. It can be seen from the above that the removal effect of aluminum by roasting alone is poor, so roasting and pickling are combined to remove the aluminum element in quartz sand to the greatest extent.

[0057] Table 4 Removal rate of aluminum in modified quartz sand prepared in Examples 10-19 and Comparative Example 2

[0058]

[0059] Embodiment 21

[0060] A preparation and purification process of modified quartz sand comprises the following steps.

[0061] The quartz fragments are put into a crusher to be crushed into quartz particles and rinsed with deionized water; the quartz particles are ground and screened, that is, quartz samples with a particle size of 300-500um are screened out on an electric vibrating screen; the quartz sample is placed in a crucible, and the crucible is placed in the furnace of a pit furnace and roasted at 900°C for 5 hours.

[0062] A mixed acid solution of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid is added to the calcined quartz sample, wherein the solid-liquid ratio of the calcined quartz sample to the acid solution is 1 g:8 mL; in the mixed acid solution, hydrochloric acid accounts for 10% of the total volume of the acid solution, sulfuric acid accounts for 25% of the total volume of the acid solution, nitric acid accounts for 30% of the total volume of the acid solution, hydrofluoric acid accounts for 15% of the total volume of the acid solution, and oxalic acid accounts for 20% of the total volume of the acid solution, and the mixture is soaked at a temperature of 70° C. for 5 hours to obtain a turbid solution; the turbid solution is centrifuged and the waste acid solution is recovered to obtain a quartz precipitate; the quartz precipitate is washed with deionized water until neutral, and then washed with ethanol, centrifuged, and dried to obtain pretreated quartz sand, which is stored for standby use.

[0063] The pretreated quartz sand is placed in a magnetic separator for magnetic separation treatment; the magnetic field intensity of the magnetic separation treatment is 50mT, and after the treatment is completed, the primary quartz sand is dried to obtain.

[0064] Concentrated nitric acid is added to primary quartz sand to obtain a quartz sand acid solution with a concentration of 0.1 g / mL; the quartz sand acid solution is placed in a flask, heated to 85°C, and refluxed in an oil bath for 28 hours to obtain a suspension; the suspension is centrifuged to separate solids; the solids are washed with deionized water until neutral to obtain carboxyl quartz sand; the carboxyl quartz sand is dispersed in deionized water, 3-aminopropyltriethoxysilane is added thereto, the molar ratio of the carboxyl quartz sand to the 3-aminopropyltriethoxysilane is 1:1, after stirring and reacting at 37°C for 13 hours, centrifugation and drying are performed to obtain amino quartz sand; a composite antibacterial agent, a surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution, the mass ratio of the amino quartz sand to the composite antibacterial agent is 100:1; the composite antibacterial agent is silver nitrate: quaternary ammonium salt: vanillin added in a mass ratio of 1:1:1; the reaction solution is continuously stirred at 70°C for 16 hours, centrifuged and dried to obtain modified quartz sand.

[0065] Embodiment 22

[0066] In the mixed acid solution, hydrochloric acid accounts for 20% of the total volume of the acid solution, sulfuric acid accounts for 30% of the total volume of the acid solution, nitric acid accounts for 15% of the total volume of the acid solution, hydrofluoric acid accounts for 15% of the total volume of the acid solution, and oxalic acid accounts for 20% of the total volume of the acid solution. The remaining steps and operations are the same as Example 21.

[0067] Embodiment 23

[0068] In the mixed acid solution, hydrochloric acid accounts for 10% of the total volume of the acid solution, sulfuric acid accounts for 30% of the total volume of the acid solution, nitric acid accounts for 30% of the total volume of the acid solution, hydrofluoric acid accounts for 10% of the total volume of the acid solution, and oxalic acid accounts for 10% of the total volume of the acid solution. The remaining steps and operations are the same as Example 21.

[0069] Embodiment 24

[0070] In the mixed acid solution, hydrochloric acid accounts for 15% of the total volume of the acid solution, sulfuric acid accounts for 30% of the total volume of the acid solution, nitric acid accounts for 25% of the total volume of the acid solution, hydrofluoric acid accounts for 10% of the total volume of the acid solution, oxalic acid accounts for 20% of the total volume of the acid solution, and the remaining steps are the same as those in Operation and Example 21.

[0071] Example 25

[0072] In the mixed acid solution, hydrochloric acid accounts for 15% of the total volume of the acid solution, sulfuric acid accounts for 25% of the total volume of the acid solution, nitric acid accounts for 30% of the total volume of the acid solution, hydrofluoric acid accounts for 15% of the total volume of the acid solution, oxalic acid accounts for 15% of the total volume of the acid solution, and the remaining steps are the same as those in Operation and Example 21.

[0073] Example 26

[0074] Detect the influence of the mixed acid ratio on the purity of the main SiO2 in the finally purified modified quartz sand during pickling of the modified quartz sand prepared in Examples 21-25 above. The results are as Figure 1 shown.

[0075] In the mixed acid solution of Example 25 of the present invention, hydrochloric acid accounts for 15% of the total volume of the acid solution, sulfuric acid accounts for 25% of the total volume of the acid solution, nitric acid accounts for 30% of the total volume of the acid solution, hydrofluoric acid accounts for 15% of the total volume of the acid solution, and oxalic acid accounts for 15% of the total volume of the acid solution. By adopting the above-mentioned mixed acid ratio, the purity of SiO2 in the finally prepared modified quartz sand can reach 99.67%, which can reach the level of refined quartz sand (99.5% < SiO2 purity < 99.995%). Through roasting followed by pickling, the present invention can remove most of the impurity metals to obtain high-purity quartz sand. And in the mixed acid of the present invention, organic acid oxalic acid is added, and the -COOH group of oxalic acid is used to combine with transition metals to form complexes or coordination compounds, so as to achieve the purpose of removing impurity metal elements. Compared with a single type of acid, using a mixed acid solution and controlling the ratio of the mixed acid can play a synergistic effect, resulting in a higher impurity removal rate and a greater purity of the main SiO2 in the quartz sand. The pickling method provided by the present invention can purify quartz ore to the level of refined quartz sand.

[0076] Example 27

[0077] A preparation and purification process for modified quartz sand includes the following steps.

[0078] Load quartz fragments into a crusher to crush them into quartz particles and rinse them clean with deionized water; perform grinding and screening on the quartz particles, that is, screen out quartz samples with a particle size of 300-500 um on an electric vibrating sieve; place the quartz samples in a crucible, and place the crucible in the furnace of a pit furnace and roast it at 900 °C for 5 hours.

[0079] A mixed acid solution of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid is added to the calcined quartz sample, wherein the solid-liquid ratio of the calcined quartz sample to the acid solution is 1 g:8 mL; in the mixed acid solution, hydrochloric acid accounts for 15% of the total volume of the acid solution, sulfuric acid accounts for 25% of the total volume of the acid solution, nitric acid accounts for 30% of the total volume of the acid solution, hydrofluoric acid accounts for 15% of the total volume of the acid solution, and oxalic acid accounts for 15% of the total volume of the acid solution, and the mixture is soaked at a temperature of 70° C. for 5 hours to obtain a turbid solution; the turbid solution is centrifuged and the waste acid solution is recovered to obtain a quartz precipitate; the quartz precipitate is washed with deionized water until neutral, and then washed with ethanol, centrifuged, and dried to obtain pretreated quartz sand, which is stored for standby use.

[0080] The pretreated quartz sand is placed in a magnetic separator for magnetic separation treatment; the magnetic field intensity of the magnetic separation treatment is 100mT, and after the treatment is completed, the primary quartz sand is obtained by drying.

[0081] Concentrated nitric acid is added to primary quartz sand to obtain a quartz sand acid solution with a concentration of 0.1 g / mL; the quartz sand acid solution is placed in a flask, heated to 85°C, and refluxed in an oil bath for 28 hours to obtain a suspension; the suspension is centrifuged to separate solids; the solids are washed with deionized water until neutral to obtain carboxyl quartz sand; the carboxyl quartz sand is dispersed in deionized water, 3-aminopropyltriethoxysilane is added thereto, the molar ratio of the carboxyl quartz sand to the 3-aminopropyltriethoxysilane is 1:1, after stirring and reacting at 37°C for 13 hours, centrifugation and drying are performed to obtain amino quartz sand; a composite antibacterial agent, a surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution, the mass ratio of the amino quartz sand to the composite antibacterial agent is 100:1; the composite antibacterial agent is silver nitrate: quaternary ammonium salt: vanillin added in a mass ratio of 1:1:1; the reaction solution is continuously stirred at 70°C for 16 hours, centrifuged and dried to obtain modified quartz sand.

[0082] The magnetic field strength and magnetic separation times of the magnetic separation treatment in Examples 28-35 are shown in Table 5, and the remaining steps and operations are the same as those in Example 27.

[0083] Table 5 Magnetic field strength and magnetic separation times in magnetic separation treatment in Examples 28-35

[0084]

[0085] Comparative Example 3

[0086] No magnetic separation treatment is performed, and the remaining steps are the same as the operation in Example 34.

[0087] Embodiment 36

[0088] The Fe content in the modified quartz sand prepared in the above Examples 27-35 and Comparative Example 3 was detected by ICP-OES. The results are shown in Table 6.

[0089] In Example 34, the pretreated quartz sand is placed in a magnetic separator for magnetic separation treatment; the magnetic field intensity of the magnetic separation treatment is 200mT, the number of magnetic separations is 3 times, and the primary quartz sand is dried after the treatment. The primary quartz sand obtained by the method is further modified, and the Fe content in the final prepared quartz sand decreases by 79.5%. The present invention utilizes the fact that quartz is non-magnetic, while the iron-containing impurity minerals are magnetic, and the magnetic impurities enriched in the quartz sand are removed by a magnetic separation method. Comparative Example 3 does not undergo magnetic separation treatment, and the decrease in the Fe content in the final prepared quartz sand mainly depends on the pickling process, so the decrease is not obvious, only 31.5%. In addition, the number of magnetic separations will also affect the decrease in the Fe content. The more magnetic separations, the greater the decrease in the Fe content. The Fe content decrease rate in the modified quartz sand prepared in Examples 31-35 is generally high, at 69.1%-79.5%.

[0090] Table 6 Fe content in modified quartz sand prepared in Examples 27-35 and Comparative Example 3

[0091]

[0092] Embodiment 37

[0093] A preparation and purification process of modified quartz sand comprises the following steps.

[0094] The quartz fragments are put into a crusher to be crushed into quartz particles and rinsed with deionized water; the quartz particles are ground and screened, that is, quartz samples with a particle size of 300-500um are screened out on an electric vibrating screen; the quartz sample is placed in a crucible, and the crucible is placed in the furnace of a pit furnace and roasted at 900°C for 5 hours.

[0095] A mixed acid solution of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid is added to the calcined quartz sample, wherein the solid-liquid ratio of the calcined quartz sample to the acid solution is 1 g:8 mL; in the mixed acid solution, hydrochloric acid accounts for 15% of the total volume of the acid solution, sulfuric acid accounts for 25% of the total volume of the acid solution, nitric acid accounts for 30% of the total volume of the acid solution, hydrofluoric acid accounts for 15% of the total volume of the acid solution, and oxalic acid accounts for 15% of the total volume of the acid solution, and the mixture is soaked at a temperature of 70° C. for 5 hours to obtain a turbid solution; the turbid solution is centrifuged and the waste acid solution is recovered to obtain a quartz precipitate; the quartz precipitate is washed with deionized water until neutral, and then washed with ethanol, centrifuged, and dried to obtain pretreated quartz sand, which is stored for standby use.

[0096] The pretreated quartz sand is placed in a magnetic separator for three magnetic separation treatments; the magnetic field intensity of the magnetic separation treatment is 200mT, and after the treatment, the primary quartz sand is dried.

[0097] Concentrated nitric acid is added to primary quartz sand to obtain a quartz sand acid solution with a concentration of 0.1 g / mL; the quartz sand acid solution is placed in a flask, heated to 85°C, and refluxed in an oil bath for 28 hours to obtain a suspension; the suspension is centrifuged to separate solids; the solids are washed with deionized water until neutral to obtain carboxyl quartz sand; the carboxyl quartz sand is dispersed in deionized water, 3-aminopropyltriethoxysilane is added thereto, the molar ratio of the carboxyl quartz sand to the 3-aminopropyltriethoxysilane is 1:1.1, after stirring and reacting at 37°C for 13 hours, centrifugation and drying are performed to obtain amino quartz sand; a composite antibacterial agent, a surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution, the mass ratio of the amino quartz sand to the composite antibacterial agent is 100:1; the composite antibacterial agent is silver nitrate: quaternary ammonium salt: vanillin added in a mass ratio of 1:1:1; the reaction solution is continuously stirred at 70°C for 16 hours, centrifuged and dried to obtain modified quartz sand.

[0098] The molar ratio of carboxyl quartz sand to 3-aminopropyltriethoxysilane and the mass ratio of amino quartz sand to the composite antibacterial agent in Examples 38-46 are shown in Table 7, and the remaining reagents and operations are the same as in Example 37.

[0099] Table 7 The molar ratio of carboxyl quartz sand to 3-aminopropyltriethoxysilane and the mass ratio of amino quartz sand to composite antibacterial agent

[0100]

[0101] In Comparative Example 4, no composite antibacterial agent was added, and the remaining reagents and operations were the same as in Example 42.

[0102] Embodiment 47

[0103] The antibacterial properties of the modified quartz sand prepared in the above Examples 37-46 and Comparative Example 4 were tested, and the inhibition rates against Escherichia coli and Staphylococcus aureus are shown in Table 8.

[0104] In Example 42, concentrated nitric acid is added to primary quartz sand, heated to 85°C, refluxed in an oil bath for 28 hours, centrifuged, washed to neutrality, and carboxyl quartz sand is obtained. The carboxyl quartz sand is dispersed in deionized water, and 3-aminopropyltriethoxysilane is added. The molar ratio of carboxyl quartz sand to 3-aminopropyltriethoxysilane is 1:1.3. The reaction is stirred at 37°C for 13 hours, centrifuged, and dried to obtain amino quartz sand; a composite antibacterial agent, a surfactant, and deionized water are added to the amino quartz sand to obtain a reaction solution, wherein the mass ratio of amino quartz sand to the composite antibacterial agent is 100:5, and the composite antibacterial agent is silver nitrate: quaternary ammonium salt: vanillin according to the mass ratio of 1:1:1. The reaction solution is stirred at 70°C for 16 hours, centrifuged, and dried to obtain modified quartz sand. The modified quartz sand prepared by the method has antibacterial ability, and the inhibition rate of Escherichia coli is 99.8%, and the inhibition rate of Staphylococcus aureus is 99.7%. In comparative example 4, no composite antibacterial agent is added, and the modified quartz sand finally prepared does not have antibacterial properties. The present invention utilizes the prepared primary quartz sand and concentrated nitric acid reflux for functionalization, consumes the -OH of the quartz sand, and combines with the composite antibacterial agent to prepare modified quartz sand with antibacterial effect, which has an inhibitory effect on common bacteria Escherichia coli and Staphylococcus aureus, enriching the application field of quartz.

[0105] Table 8 Antibacterial properties of modified quartz sand prepared in Examples 37-46 and Comparative Example 4

[0106]

[0107] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing and purifying modified quartz sand, characterized in that: The following steps are involved: Putting quartz fragments into a crusher to crush them into quartz particles and washing them with deionized water; grinding and screening the quartz particles to obtain a quartz sample; placing the quartz sample in a crucible, placing the crucible in a furnace of a pit furnace and roasting at 600-1000° C. for 5 hours; Add a mixed acid solution of hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid and oxalic acid to the calcined quartz sample, and soak it at a temperature of 20-70°C for 2-8 hours to obtain a turbid solution; in the mixed acid solution, the hydrochloric acid accounts for 10%-20% of the total volume of the mixed acid solution; the sulfuric acid accounts for 25%-30% of the total volume of the mixed acid solution; the nitric acid accounts for 15%-30% of the total volume of the mixed acid solution; the hydrofluoric acid accounts for 10%-15% of the total volume of the mixed acid solution; and the oxalic acid accounts for 10%-20% of the total volume of the mixed acid solution; centrifuge the turbid solution and recover the waste acid solution to obtain a quartz precipitate; wash the quartz precipitate with deionized water until neutral, then wash it with ethanol, centrifuge it, and dry it to obtain pretreated quartz sand, which is stored for standby use; The pretreated quartz sand is placed in a magnetic separator for magnetic separation; the magnetic field intensity of the magnetic separation treatment is 50-250mT, and after the treatment is completed, the primary quartz sand is dried; Add concentrated nitric acid to the primary quartz sand to obtain a quartz sand acid solution; place the quartz sand acid solution in a flask, heat to 85° C., and reflux in an oil bath for 28 hours to obtain a suspension; centrifuge the suspension to separate solids; The solid is washed with deionized water until it is neutral to obtain carboxyl quartz sand; the carboxyl quartz sand is dispersed in deionized water, 3-aminopropyltriethoxysilane is added thereto, and after stirring and reacting at 37°C for 14 hours, centrifugation and drying are performed to obtain amino quartz sand; a composite antibacterial agent, a surfactant and deionized water are added to the amino quartz sand to obtain a reaction solution; the reaction solution is further stirred at 70°C for 16 hours, centrifuged and dried to obtain the modified quartz sand; the mass ratio of the amino quartz sand to the composite antibacterial agent is 100:1-10; the composite antibacterial agent is a combination of silver nitrate: quaternary ammonium salt: vanillin in a mass ratio of 1:1:

1.

2. A preparation and purification process of modified quartz sand according to claim 1, characterized in that: The screening process is to screen out quartz samples with a particle size of 100-800um on an electric vibrating screen.

3. The preparation and purification process of modified quartz sand according to claim 1, characterized in that: The solid-to-liquid ratio of the calcined quartz sample to the acid solution is 1 g:1-10 mL.

4. The preparation and purification process of modified quartz sand according to claim 1, characterized in that: The concentration of the quartz sand acid solution is 0.1 g / mL.

5. The preparation and purification process of modified quartz sand according to claim 1, characterized in that: The molar ratio of the carboxyl quartz sand to the 3-aminopropyltriethoxysilane is 1:1-1.

5.

6. A modified quartz sand, characterized in that: The modified quartz sand is a quartz sample prepared by crushing, grinding, screening and calcining quartz fragments, and then subjected to acid treatment and magnetic separation treatment. The surface of the obtained primary quartz sand is functionalized and coupled with a composite antibacterial agent. The modified quartz sand is prepared and purified by the preparation and purification process described in any one of claims 1 to 5. The content of impurity elements in the modified quartz sand is generally reduced, wherein the Fe content is reduced by 22.8%, the Al content is reduced by 33.9%, the K content is reduced by 54%, and the Na content is reduced by 38.4%. , the Ca content decreased by 58.1%, and the Ti content decreased by 46.7%; when the modified quartz sand was purified, the pickling temperature was 70°C, the pickling time was 5 hours, and the removal rate of metallic aluminum in the obtained modified quartz sand was 71.1%; the SiO2 purity of the modified quartz sand was 99.67%; the modified quartz sand was treated by magnetic separation, so that the Fe element content decreased by 79.5%; the modified quartz sand has antibacterial ability, with an inhibition rate of 99.8% on Escherichia coli and 99.7% on Staphylococcus aureus.