Organotin dendritic compound and photoresist composition thereof
By combining organotin dendrimers with free radical quenchers and photoresist solvents, a negative photoresist composition is formed, which solves the problems of low resolution and poor sensitivity of existing photoresists and achieves high resolution. High efficiency and high sensitivity lithography effect, suitable for nanoimprint and electron beam lithography.
Patent Information
- Application Number
- CN202410789349.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-19
AI Technical Summary
Existing photoresists have low resolution and poor sensitivity, especially when using shorter wavelength light sources. It is difficult to meet the requirements for high resolution and high sensitivity, and the synthesis method of polymer-based photoresists has stability and uniformity issues. .
Using an organotin dendrimer compound and its photoresist composition, the organotin dendrimer compound is prepared through a thiol-ene click reaction, and is combined with a free radical quencher and a photoresist solvent to form a negative photoresist composition. Used in applications such as nanoimprinting and electron beam lithography.
It achieves high-resolution and high-sensitivity photolithography effects, with a definite molecular structure and low molecular weight. The tin element has high absorption efficiency of extreme ultraviolet light. It is suitable for industrial production and shows excellent photolithography performance under electron beam exposure. .
Smart Images

Figure CN118791518A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photoresists, and specifically relates to a photoresist composition, in particular to a photoresist composition of an organic tin dendrite compound. Background Art
[0002] Photoresist, also known as photoetchant, is a patterned material that can change its solubility under the irradiation of light. Photoresist is a key material in chip manufacturing. Through the photolithography process, it can transfer the pre-designed pattern to the substrate material such as silicon wafer after the steps of pre-baking, exposure and development. During the photolithography process, the photoresist undergoes a photochemical reaction after exposure, resulting in a change in solubility. If the exposed area is soluble in the developer, positive photolithography occurs, and if the exposed area is insoluble in the developer, negative photolithography occurs.
[0003] In order to meet the needs of chip miniaturization and integration, the wavelength used in photolithography has gradually decreased from visible light (436nm) to deep ultraviolet (193nm) and even extreme ultraviolet (13.5nm) to achieve an increase in photolithography resolution from microns to nanometers. Therefore, the development of new high-sensitivity and high-resolution (<100nm) photoresists that meet the requirements of shorter wavelength light sources has become the current research focus. In order to quickly screen photoresists that meet the requirements, electron beam exposure has become the main verification method.
[0004] At present, polymer compounds are the main photoresist materials, but their synthesis methods have huge limitations. The molecular weight of polymer compounds is usually large, the chain segments are prone to entanglement, and the molecular weight distribution is difficult to ensure to be 1. This makes it difficult to ensure the stability and uniformity of polymer photoresists, resulting in inevitable low resolution. Among them, PMMA type photoresist is the most important photoresist. Although the ultimate resolution can reach tens of nanometers, it often requires a higher exposure dose (>1000μC / cm 2 ), and because it is mainly composed of carbon, hydrogen, and oxygen elements, PMMA has extremely low absorption efficiency for extreme ultraviolet light, resulting in its poor sensitivity and unsuitable for large-scale chip production. Summary of the invention
[0005] The present invention aims to solve the problems of low resolution and poor sensitivity of existing photoresists, provide a class of organic tin dendrite compounds and photoresist compositions thereof, and also provide a method for using the photoresist composition. The compounds and photoresist compositions provided by the present invention can be used in nanoimprint lithography, electron beam lithography, 248nm lithography, 193nm lithography or extreme ultraviolet lithography.
[0006] The technical solution adopted by the present invention is:
[0007] A class of organic tin dendrite compounds has a structure shown in the following formula (I):
[0008]
[0009] in:
[0010] In the structural formula, R a1 -R a4 are the same and are selected from hydrogen, methyl, isopropyl or ethoxy; R b1 -R b4 The same is selected from a hydrogen atom, a methyl group or an ethoxy group; n-Bu represents a n-butyl group.
[0011] Preferably, the organotin dendrimer compound is selected from the following compounds:
[0012]
[0013]
[0014] Here, n-Bu represents a normal butyl group.
[0015] The present invention also provides a method for preparing the compound represented by the above formula (I).
[0016] The preparation method of the organotin dendrimer compound comprises the following steps:
[0017]
[0018] wherein Ra1-Ra4 and Rb1-Rb4 are as defined above, Ra' represents a hydrogen atom, a methyl group, an isopropyl group or an ethoxy group, Rb' represents a hydrogen atom, a methyl group or an ethoxy group, and n-Bu represents a n-butyl group.
[0019] The organic tin dendrimer compound is obtained by reacting the compound of formula (II) with the compound of formula (III) through a thiol-ene click reaction.
[0020] The present invention also provides a photoresist composition, which is a negative photoresist composition and comprises the organic tin dendrite compound of the above formula (I), a free radical quencher, and a photoresist solvent.
[0021] Further preferably, the mass of the organic tin dendrite compound accounts for 1 wt%-10 wt% of the total mass of the negative photoresist composition, the free radical quencher accounts for 0.01 wt%-1 wt%, and the rest is photoresist solvent.
[0022] Further preferably, the free radical quencher can be selected from one or more of 2,2,6,6-tetramethylpiperidinyloxy, 4-hydroxy-2,2,6,6-tetramethylpiperidinyloxy, 1,1-diphenyl-2-trinitrophenylhydrazine (DPPH), benzoquinone or hydroquinone.
[0023] Further preferably, the photoresist solvent is selected from one or more of ethyl acetate, tetrahydrofuran (THF), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, ethyl lactate, methyl ethyl ketone, 4-methyl-2-pentanone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or acetonitrile.
[0024] Further preferably, the photoresist composition can use the following developers: one or more of ethyl acetate, tetrahydrofuran (THF), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, ethyl lactate, methyl ethyl ketone, 4-methyl-2-pentanone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or acetonitrile.
[0025] Advantages and beneficial effects of the present invention:
[0026] Based on the above technical solutions and the technical problems solved, the present invention achieves the following technical effects:
[0027] 1. The present invention provides an organic tin dendrite compound. The organic tin dendrite compound is simple to synthesize, and the final product can be separated from the system by precipitation, and is suitable for industrial production.
[0028] 2. The organic tin dendrite compound of the present invention has a definite molecular structure, a low molecular weight, and a single molecular size, and can well meet the requirements of high-resolution lithography.
[0029] 3. The organic tin dendrite compound of the present invention contains numerous tin atoms. Since the absorption cross-sectional area of tin element to extreme ultraviolet light is more than ten times that of carbon, hydrogen, oxygen and other elements, the organic tin dendrite compound can well meet the requirements of high-sensitivity lithography. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is an atomic force microscope (AFM) image of stripes obtained by electron beam lithography of a negative photoresist using compound I-1 as an organic tin dendrite compound in Comparative Example 1 of the present invention;
[0031] Figure 2 This is an atomic force microscope (AFM) image of stripes obtained by electron beam lithography of a negative photoresist using Compound I-1 as an organic tin dendrite compound in Example 10 of the present invention. DETAILED DESCRIPTION
[0032] Embodiment 1:
[0033] The synthesis route of compound I-1 is as follows:
[0034]
[0035] Tetrahydrofuran (60 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tributyl vinyl tin (4 mmol, 1.268 g), Irgacure 184 (1-hydroxycyclohexyl phenyl ketone, 0.05 g) were added to a 150 ml round-bottom flask in sequence and reacted under ultraviolet light at a wavelength of 365 nm for 2 hours. After the reaction, water / ethyl acetate was used for extraction and rotary evaporation was performed at 40°C to obtain a light yellow viscous liquid, namely, 1.231 g of compound I-1 product, with a yield of 72.4%. 1 H NMR(400MHz,Chloroform-d)δ2.79(t,J=6.9Hz,1H),2.59(t,J=6.9Hz,1H),2.46 (t,J=6.9Hz,1H),1.65(d,J=13.7Hz,0H),1.35–1.23(m,6H),0.94–0.80(m,8H).
[0036] Embodiment 2:
[0037] The synthesis route of compound I-1 is as follows:
[0038]
[0039] Tetrahydrofuran (5 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tributyl vinyl tin (4 mmol, 1.268 g), TBD (1,5,7-triazabicyclo [4.4.0] dec-5-ene, 27.8 mg) were added to a 10 ml round-bottom flask in sequence. After the addition of TBD, an exothermic reaction occurred, and the colorless solution turned yellow and became viscous. After 1 minute, the viscous solution was diluted with 5 mL of tetrahydrofuran, extracted with water / ethyl acetate, and rotary evaporated at 40 ° C to obtain a light yellow viscous liquid, namely, compound I-1 product 1.547 g, with a yield of 91.1%. 1 H NMR(400MHz,Chloroform-d)δ2.79(t,J=6.9Hz,1H),2.59(t,J=6.9Hz,1H),2.46 (t,J=6.9Hz,1H),1.65(d,J=13.7Hz,0H),1.35–1.23(m,6H),0.94–0.80(m,8H).
[0040] Embodiment 3:
[0041] Compound I-2 was prepared by the following synthetic route:
[0042]
[0043] Tetrahydrofuran (60 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tributyl isopropenyltin (4 mmol, 1.324 g), Irgacure 184 (1-hydroxycyclohexyl phenyl ketone, 0.05 g) were added to a 150 ml round-bottom flask in sequence and reacted under ultraviolet light at a wavelength of 365 nm for 2 hours. After the reaction, water / ethyl acetate was used for extraction and rotary evaporation was performed at 40°C to obtain a light yellow viscous liquid, namely, compound I-2 product 1.261 g, with a yield of 71.8%. 1 HNMR(400MHz,Chloroform-d)δ2.88–2.75(m,1H),2.60(t,J=7.1Hz,1H),2.48–2.37(m ,1H),1.70–1.61(m,0H),1.45–1.25(m,6H),1.05–0.91(m,5H),0.90(t,J=6.6Hz,4H).
[0044] Embodiment 4:
[0045] Compound I-2 was prepared by the following synthetic route:
[0046]
[0047] Tetrahydrofuran (5 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tributyl isopropenyltin (4 mmol, 1.324 g), TBD (1,5,7-triazabicyclo [4.4.0] dec-5-ene, 27.8 mg) were added to a 10 ml round-bottom flask in sequence. After the addition of TBD, an exothermic reaction occurred, and the colorless solution turned yellow and became viscous. After 1 minute, the viscous solution was diluted with 5 mL of tetrahydrofuran, extracted with water / ethyl acetate, and rotary evaporated at 40 ° C to obtain a light yellow viscous liquid, namely, compound I-2 product 1.528 g, with a yield of 86.9%. 1 H NMR(400MHz,Chloroform-d)δ2.88–2.75(m,1H),2.60(t,J=7.1Hz,1H),2.48–2.37(m ,1H),1.70–1.61(m,0H),1.45–1.25(m,6H),1.05–0.91(m,5H),0.90(t,J=6.6Hz,4H).
[0048] Embodiment 5:
[0049] Compound I-3 was prepared by the following synthetic route:
[0050]
[0051] Tetrahydrofuran (60 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tri-n-butyl (1-propenyl) tin (4 mmol, 1.324 g), Irgacure 184 (1-hydroxycyclohexyl phenyl ketone, 0.05 g) were added to a 150 ml round-bottom flask in sequence and reacted under ultraviolet light at a wavelength of 365 nm for 2 hours. After the reaction, water / ethyl acetate was used for extraction and rotary evaporation was performed at 40°C to obtain a light yellow viscous liquid, namely, compound I-3 product 1.036 g, with a yield of 59%. 1 H NMR (400MHz, Chloroform-d) δ2.86 (td, J = 7.1, 1.9Hz, 1H), 2.70–2.47 (m, 1H), 1.36–1.19 (m, 6H), 0.93–0.82 (m, 5H).
[0052] Embodiment 6:
[0053] Compound I-3 was prepared by the following synthetic route:
[0054]
[0055] Tetrahydrofuran (5 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tri-n-butyl (1-propenyl) tin (4 mmol, 1.324 g), TBD (1,5,7-triazabicyclo [4.4.0] dec-5-ene, 27.8 mg) were added to a 10 ml round-bottom flask in sequence. After the addition of TBD, an exothermic reaction occurred, and the colorless solution turned yellow and became viscous. After 1 minute, the viscous solution was diluted with 5 mL of tetrahydrofuran, extracted with water / ethyl acetate, and rotary evaporated at 40 ° C to obtain a light yellow viscous liquid, namely, compound I-3 product 1.493 g, with a yield of 85.0%. 1 H NMR(400MHz,Chloroform-d)δ2.88–2.75(m,1H),2.60(t,J=7.1Hz,1H),2.48–2.37(m ,1H),1.70–1.61(m,0H),1.45–1.25(m,6H),1.05–0.91(m,5H),0.90(t,J=6.6Hz,4H).
[0056] Embodiment 7:
[0057] Compound I-4 was prepared by the following synthetic route:
[0058]
[0059] Tetrahydrofuran (60 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tributyl (2-methylprop-1-ene) stannane (4 mmol, 1.381 g), Irgacure 184 (1-hydroxycyclohexylphenyl ketone, 0.05 g) were added to a 150 ml round-bottom flask in sequence and reacted under ultraviolet light at a wavelength of 365 nm for 2 hours. After the reaction, water / ethyl acetate was used for extraction and rotary evaporation was performed at 40°C to obtain a light yellow viscous liquid, namely, compound I-4 product 1.142 g, with a yield of 63%. 1 HNMR (400MHz, Chloroform-d) δ2.88 (t, J = 6.8 Hz, 1H), 2.63 (t, J = 6.8 Hz, 1H), 1.37–1.25 (m, 9H), 0.94–0.80 (m, 8H).
[0060] Embodiment 8:
[0061] Compound I-5 was prepared by the following synthetic route:
[0062]
[0063] Tetrahydrofuran (60 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tributyl (1-ethoxyethylene) tin (4 mmol, 1.445 g), Irgacure 184 (1-hydroxycyclohexyl phenyl ketone, 0.05 g) were added to a 150 ml round-bottom flask in sequence and reacted under ultraviolet light at a wavelength of 365 nm for 2 hours. After the reaction, water / ethyl acetate was used for extraction and rotary evaporation was performed at 40°C to obtain a light yellow viscous liquid, namely, compound I-5 product 1.288 g, with a yield of 69%. 1 HNMR(400MHz,Chloroform-d)δ3.57–3.48(m,1H),2.94–2.77(m,1H),2.66–2.52(m,2H ),1.45–1.25(m,6H),1.15(t,J=5.7Hz,1H),1.01–0.91(m,3H),0.90(t,J=6.6Hz,4H).
[0064] Embodiment 9:
[0065] Compound I-6 was prepared by the following synthetic route:
[0066]
[0067] Tetrahydrofuran (60 ml), pentaerythritol tetrathioglycolate (1 mmol, 0.433 g), tributyl (2-ethoxyethylene) tin (4 mmol, 1.445 g), Irgacure 184 (1-hydroxycyclohexyl phenyl ketone, 0.05 g) were added to a 150 ml round-bottom flask in sequence and reacted under ultraviolet light at a wavelength of 365 nm for 2 hours. After the reaction, water / ethyl acetate was used for extraction and rotary evaporation was performed at 40°C to obtain a light yellow viscous liquid, namely, compound I-6 product 0.826 g, with a yield of 44%. 1 HNMR(400MHz,Chloroform-d)δ4.41(t,J=5.5Hz,0H),3.69–3.51(m,1H),2.89(td,J=7.0,4.4Hz,1H),2.67–2.53(m ,1H),1.50(dd,J=5.6,1.2Hz,1H),1.31(d,J=6.8Hz,1H),1.32–1.24(m,5H),1.28–1.20(m,2H),0.93–0.81(m,8H).
[0068] By performing molecular formula, relative molecular mass, molecular size and elemental analysis on the obtained compounds (see Table 1), it can be seen that the organic tin dendrimer compound has a definite molecular structure and a small molecular size, which can meet the requirements of high-resolution lithography applications, and contains a large amount of tin elements that are sensitive to absorption by high-energy radiation sources such as electron beams, deep ultraviolet rays, and extreme ultraviolet rays, which will help to improve the sensitivity of this type of photoresist under corresponding high-energy radiation source lithography.
[0069] Table 1
[0070]
[0071] In some embodiments, the photoresist composition is a negative photoresist composition, comprising the organic tin dendron compound, a radical quencher, and a photoresist solvent.
[0072] Further preferably, in some embodiments, the mass of the organic tin dendrite compound accounts for 1 wt%-10 wt% of the total mass of the negative photoresist composition, the free radical quencher accounts for 0.01 wt%-1 wt%, and the rest is photoresist solvent.
[0073] Further preferably, in some embodiments, the free radical quencher can be selected from one or more of 2,2,6,6-tetramethylpiperidinyl oxide, 4-hydroxy-2,2,6,6-tetramethylpiperidinyl oxide, 1,1-diphenyl-2-trinitrophenylhydrazine (DPPH), benzoquinone or hydroquinone.
[0074] Further preferably, in some embodiments, the photoresist solvent is selected from one or more of ethyl acetate, tetrahydrofuran (THF), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, ethyl lactate, methyl ethyl ketone, 4-methyl-2-pentanone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or acetonitrile.
[0075] Further preferably, in some embodiments, the photoresist composition may use one or more of the following developers: ethyl acetate, tetrahydrofuran (THF), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, ethyl lactate, methyl ethyl ketone, 4-methyl-2-pentanone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or acetonitrile.
[0076] Furthermore, the present invention also provides a method for using the organotin dendrite photoresist composition, the specific steps of which are as follows:
[0077] The substrate (silicon wafer or silicon dioxide wafer) to be loaded with photoresist is subjected to hydrophilic treatment: the substrate is placed in a mixed solution of 20wt% hydrogen peroxide solution and 20wt% ammonia water at 80°C for 15 minutes, then washed with distilled water and isopropanol and blown dry with nitrogen for later use;
[0078] The photoresist composition is preferably filtered through a filter having a pore size of 0.22 μm;
[0079] The photoresist composition is dripped onto the substrate and spin-coated to form a film. Specifically, the spin-coating rate may be 500-5000 r / s and the spin-coating time may be 10-60 s.
[0080] The substrate coated with the photoresist composition film is further heated to remove the contained solvent, the heating temperature may be 40-100° C., and the heating time may be 10-180 seconds;
[0081] The obtained substrate loaded with the photoresist composition film is subjected to exposure photolithography under a high-energy radiation source such as an electron beam;
[0082] Finally, the exposed substrate is soaked in a developer, developed and taken out, and the developer remaining on the surface of the substrate is blown dry with nitrogen. The development time may be 5-60s, and the developer may use at least one of the aforementioned developers.
[0083] Embodiment 10:
[0084] A negative photoresist composition comprising 0.04 g of the compound I-1 prepared in Example 1 and 1 ml of propylene glycol monomethyl ether acetate. 2 Under the exposure conditions, uniform photolithography stripes can be obtained (see Figure 1), the resolution of the photolithography stripes is about 120nm.
[0085] Embodiment 11:
[0086] A negative photoresist composition comprising 0.04 g of compound I-1 prepared in Example 1, 0.1 mg of hydroquinone and 1 ml of propylene glycol monomethyl ether acetate. 2 Under the exposure conditions, uniform photolithography stripes can be obtained (see Figure 2 ), the resolution of the photolithography stripes is about 100nm.
[0087] The composition of the photoresist composition and the corresponding photolithography sensitivity and resolution of the specific embodiment are shown in Table 2 below
[0088] Table 2
[0089]
[0090] The smaller the exposure dose value, the higher the sensitivity of the photoresist composition. At present, the exposure dose of polymer photoresist (PMMA) is generally 1000μC / cm 2 above.
[0091] The smaller the resolution value, the higher the resolution of the photoresist composition. Currently, photoresists with a resolution less than or equal to 100 nm are classified as high-resolution photoresists.
[0092] Sensitivity and resolution are the main evaluation indicators of photoresist performance.
[0093] By comparing Example 10 with Example 11 and Examples 11-22, it can be seen that: adding a free radical quencher to the photoresist composition can effectively improve the resolution of the photoresist and improve the quality of the line pattern, but the sensitivity of the photoresist decreases with the increase in the amount added; the type of free radical quencher has an impact on the sensitivity and resolution of the photoresist; the type of photoresist solvent has a greater impact on the sensitivity of the photoresist composition, but has little impact on the resolution. In addition, all examples show a sensitivity higher than PMMA (a commonly used polymer photoresist) (300-500μC / cm 2 ) and mostly maintain a high lithographic resolution (~100nm).
[0094] It should be further explained that, in the implementation manner of the present invention, not every embodiment includes only one independent technical solution, and each embodiment is only used to understand the technical solution of the present invention, and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made to the technical solution of the present invention that belongs to the technical concept of the present invention shall be included in the protection scope of the present invention.
Claims
1. An organic tin dendrite compound having a structure as shown in the following formula (I): in: In the structural formula, R a1 -R a4 are the same and are selected from hydrogen, methyl, isopropyl or ethoxy; R b1 -R b4 The same is selected from a hydrogen atom, a methyl group or an ethoxy group; n-Bu represents a n-butyl group.
2. An organotin dendrimer compound according to claim 1, characterized in that: The organotin dendrimer compound is selected from the following compounds: Here, n-Bu represents a normal butyl group.
3. An organotin dendrimer compound according to claim 1, characterized in that: The compound represented by formula (I) is prepared by the following method: Synthesis route: wherein Ra1-Ra4 and Rb1-Rb4 are as defined in claim 1, Ra' represents a hydrogen atom, a methyl group, an isopropyl group or an ethoxy group, Rb' represents a hydrogen atom, a methyl group or an ethoxy group, and n-Bu represents a n-butyl group; The preparation process is to obtain the organic tin dendrite compound by a thiol-ene click reaction of the compound represented by formula (II) and the compound represented by formula (III).
4. A photoresist composition, characterized in that The photoresist composition is a negative photoresist composition, comprising the organic tin dendrite compound represented by formula (I) as described in any one of claims 1 to 3, a free radical quencher, and a photoresist solvent.
5. The photoresist composition according to claim 4, characterized in that The mass of the organic tin dendrite compound accounts for 1wt%-10wt% of the total mass of the negative photoresist composition, the free radical quencher accounts for 0.01wt%-1wt%, and the rest is photoresist solvent.
6. The photoresist composition according to claim 4, characterized in that The free radical quencher is selected from one or more of 2,2,6,6-tetramethylpiperidinyloxy, 4-hydroxy-2,2,6,6-tetramethylpiperidinyloxy, 1,1-diphenyl-2-trinitrophenylhydrazine (DPPH), benzoquinone or hydroquinone.
7. The photoresist composition according to claim 4, characterized in that The photoresist solvent is selected from one or more of ethyl acetate, tetrahydrofuran (THF), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, ethyl lactate, methyl ethyl ketone, 4-methyl-2-pentanone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or acetonitrile.
8. The photoresist composition according to claim 4, characterized in that The developer used in the photoresist composition is one or more of ethyl acetate, tetrahydrofuran (THF), propylene glycol methyl ether acetate (PGMEA), cyclohexanone, ethyl lactate, methyl ethyl ketone, 4-methyl-2-pentanone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or acetonitrile.
Citation Information
Patent Citations
Silicon-containing polyphenyl monomolecular resin and photoresist composition thereof
CN112142769A
Metal oxygen cluster composition and photoetching patterning application
CN117008416A
Tin dendrimers, their use as x-ray contrast agents and processes for their preparation
WO1998007730A1