A kind of anti-aging polyurethane material and preparation method thereof
By reacting modified polysiloxane with polyurethane materials, hypophosphoric acid, fluorine-containing groups and functional monomers are introduced to form a stable crosslinking structure and a six-membered ring of conjugated hydrogen bonds, solving the existing anti-aging polyurethane materials The problem of insufficient flame retardant properties, tensile strength and hydrophobic properties has achieved higher aging resistance and anti-aging properties.
Patent Information
- Application Number
- CN202411288805.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The existing anti-aging polyurethane materials have shortcomings in flame retardant properties, tensile strength and hydrophobic properties, and are difficult to meet the application needs in many fields.
Preparation by reacting modified polysiloxane with polyurethane materials, hypophosphoric acid, fluorine-containing groups and functional monomers are introduced to form a stable crosslinking structure and a six-membered ring of conjugated hydrogen bonds, improving flame retardant properties and tensile strength , and reduce the surface energy of the material to enhance hydrophobic properties.
The flame retardant properties, tensile strength and hydrophobic properties of anti-aging polyurethane materials are significantly improved, and their stability and aging resistance under high temperature, ultraviolet light and photothermal conditions are enhanced.
Smart Images

Figure SMS_5 
Figure SMS_6 
Figure SMS_7
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, in particular to an anti-aging polyurethane material and a preparation method thereof. Background Art
[0002] Polyurethane is a polymer material with excellent tensile strength formed by polyols and polyisocyanates through polycondensation reaction, and has strong plasticity. This material has a wide range of applications, involving products such as coatings, adhesives, fabric finishing agents, leather modifiers, polyurethane soft / rigid foams, elastomers, etc., and is used in the fields of textiles, construction, aviation, ships, transportation, medicine, electronics, etc. Polysiloxane is a type of polymer material whose main chain is composed of repeated alternating Si-O bonds and organic groups are connected to silicon atoms. In the polysiloxane molecular chain, it contains both inorganic structures and organic groups. Therefore, polysiloxane is a semi-inorganic and semi-organic polymer, which has the dual advantages of inorganic and organic materials, and has many excellent properties such as high and low temperature resistance, flexibility, aging resistance, hydrophobicity and physiological inertness, making polysiloxane materials widely used in aerospace, chemical and light industry, automobile industry, medical and health care and other fields.
[0003] The anti-aging polyurethane material prepared by the invention is prepared by reacting modified polysiloxane with polyurethane material, has good anti-aging performance, hydrophobicity, flame retardancy and tensile strength, and has good market prospects. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing an anti-aging polyurethane material to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] The invention discloses a preparation process of an anti-aging polyurethane material. The anti-aging polyurethane material is prepared by reacting octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane and hypophosphorous acid modified silane to obtain modified polysiloxane; reacting 4-hydroxybutyraldehyde with 2-chloro-4,6-diamino-1,3,5-triazine to obtain a functional monomer; reacting diphenylmethane diisocyanate, polyethylene glycol and a functional monomer to obtain a polyurethane material; and reacting the polyurethane material with the modified polysiloxane and resorcinol to obtain the anti-aging polyurethane material.
[0007] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0008] (1) 3-glycidyloxypropyltrimethoxysilane, 2-aminoethyl hypophosphorous acid and anhydrous ethanol were mixed in a mass ratio of 1: (1.2-1.4): (8-12), 0.3-0.5 times the mass of 3-glycidyloxypropyltrimethoxysilane was added dropwise with a 1 mol / L sodium hydroxide aqueous solution, stirred at 95-105°C and 600-800 r / min for 9-11 hours, filtered and the filtrate was collected to obtain hypophosphorous acid-modified silane;
[0009] (2) Octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide are mixed in a mass ratio of 1: (0.6-0.8): (0.5-0.7): (0.01-0.03), stirred at 80-90°C and 200-400 r / min for 2-3 h under a nitrogen atmosphere, heated to 95-105°C and continued to stir for 7-9 h, heated to 130-140°C at 10-20°C / min and continued to stir for 40-50 min, and distilled under a vacuum environment for 1-2 h to obtain modified polysiloxane;
[0010] (3) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene are mixed in a mass ratio of 1: (1.6-1.8): (8-12), stirred at 50-60°C at 100-200 r / min for 20-40 min, heated to 60-70°C and then vacuumed, stirred for 4-6 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 3-5 times, respectively, and vacuum dried at 45-55°C for 8-12 h to obtain a functional monomer;
[0011] (4) Mix diphenylmethane diisocyanate, polyethylene glycol and N,N-dimethylformamide in a mass ratio of 1: (2.3-2.7): (8-12), pass nitrogen gas for protection, stir at 80-90°C and 200-400 r / min for 20-40 min, monitor the -NCO content by toluene dibutylamine titration during stirring, and after the prepolymerization reaction is completed, lower the temperature to 70-80°C, add functional monomers in an amount of 0.3-0.5 times the mass of diphenylmethane diisocyanate, and continue stirring for 3-5 h to obtain a polyurethane material;
[0012] (5) The polyurethane material, anhydrous aluminum chloride and chlorobenzene are mixed uniformly in a mass ratio of 1: (0.3-0.4): (10-12), stirred at 200-300 r / min at 0-3°C for 20-30 min, then 0.6-0.8 times the mass of resorcinol of the polyurethane material is added, the temperature is raised to 75-85°C, stirred for 4-6 h, 0.4-0.6 times the mass of modified polysiloxane of the polyurethane material is added, the temperature is raised to 95-105°C, stirring is continued for 2-4 h, cooled to room temperature, centrifuged to separate the solid, washed with anhydrous ethanol for 3-5 times, and vacuum dried at 55-65°C for 8-12 h to obtain an anti-aging polyurethane material.
[0013] As an optimization, the reaction process of the hypophosphorous acid-modified silane in step (1) is as follows:
[0014] .
[0015] As an optimization, the reaction process of the modified polysiloxane in step (2) is as follows:
[0016] .
[0017] As an optimization, the functional monomer reaction process in step (3) is as follows:
[0018] .
[0019] As an optimization, the polyethylene glycol in step (4) has a molecular weight of 1000.
[0020] As an optimization, the reaction process of the polyurethane material in step (4) is as follows:
[0021] .
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] When preparing the anti-aging polyurethane material, the present invention comprises the following steps: 3-glycidyloxypropyltrimethoxysilane is reacted with 2-aminoethyl hypophosphorous acid to obtain hypophosphorous acid-modified silane; octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane and hypophosphorous acid-modified silane are reacted to obtain modified polysiloxane; 4-hydroxybutyraldehyde is reacted with 2-chloro-4,6-diamino-1,3,5-triazine to obtain a functional monomer; diphenylmethane diisocyanate, polyethylene glycol and a functional monomer are reacted to obtain a polyurethane material; and the polyurethane material is reacted with the modified polysiloxane and resorcinol to obtain the anti-aging polyurethane material.
[0024] Firstly, octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane and hypophosphorous acid-modified silane are reacted to obtain modified polysiloxane, and hypophosphorous acid is introduced into the linear polysiloxane to further improve the flame retardant properties of the polysiloxane itself, thereby further improving the flame retardant properties of the anti-aging polyurethane. In addition, the phosphorus and hydrogen on the hypophosphorous acid can be used as reaction sites, which can react with the imine bonds on the polyurethane material to form a stable cross-linking structure, thereby improving the tensile strength of the anti-aging polyurethane material. 3,3,3-trifluoropropylmethyldimethoxysilane introduces fluorine-containing groups on the linear polysiloxane, and the fluorine-containing groups can reduce the surface energy of the material and improve the hydrophobic properties of the anti-aging polyurethane material.
[0025] Secondly, 4-hydroxybutyraldehyde and 2-chloro-4,6-diamino-1,3,5-triazine are reacted through the dehydration condensation reaction of amino group and aldehyde group to obtain functional monomer. The triazine structure is rich in nitrogen, which will produce nitrogen when heated, and has the effect of gas phase flame retardancy. It also has a carbonizing effect, and can synergistically flame retardant with the phosphorus on the polysiloxane, thereby improving the flame retardant properties of the anti-aging polyurethane material. The chlorine on the triazine structure of the polyurethane material reacts with resorcinol to form a conjugated hydrogen bonded six-membered ring, which has a good ultraviolet light absorption effect and improves the anti-aging effect. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0029] (1) 3-glycidyloxypropyltrimethoxysilane, 2-aminoethyl hypophosphorous acid and anhydrous ethanol were mixed in a mass ratio of 1:1.2:8, 0.3 times the mass of 3-glycidyloxypropyltrimethoxysilane was added dropwise with a 1 mol / L sodium hydroxide aqueous solution, stirred at 95°C and 600 r / min for 9 h, filtered and the filtrate was collected to obtain hypophosphorous acid-modified silane;
[0030] (2) Octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:0.6:0.5:0.01, stirred at 80°C and 200 r / min for 2 h under a nitrogen atmosphere, heated to 95°C and continued to stir for 7 h, heated to 130°C at 10°C / min and continued to stir for 40 min, and distilled under a vacuum environment for 1 h to obtain modified polysiloxane;
[0031] (3) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene were mixed in a mass ratio of 1:1.6:8, stirred at 100 r / min for 20 min at 50°C, heated to 60°C and then vacuumed, stirred for 4 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 3 times, respectively, and vacuum dried at 45°C for 8 h to obtain a functional monomer;
[0032] (4) Diphenylmethane diisocyanate, polyethylene glycol, and N,N-dimethylformamide were mixed in a mass ratio of 1:2.3:8, and nitrogen was passed through the mixture. The mixture was stirred at 200 r / min for 20 min at 80°C. During the stirring process, the -NCO content was monitored by toluene dibutylamine titration method. After the prepolymerization reaction was completed, the temperature was lowered to 70°C, and a functional monomer with a mass of 0.3 times that of diphenylmethane diisocyanate was added and stirred for 3 h to obtain a polyurethane material.
[0033] (5) The polyurethane material, anhydrous aluminum chloride and chlorobenzene were mixed uniformly in a mass ratio of 1:0.3:10, stirred at 200 r / min at 0°C for 20 min, then 0.6 times the mass of resorcinol of the polyurethane material was added, the temperature was raised to 75°C, stirred for 4 h, and 0.4 times the mass of modified polysiloxane of the polyurethane material was added, the temperature was raised to 95°C, stirring was continued for 2 h, cooled to room temperature, the solid was separated by centrifugation, washed with anhydrous ethanol for 3 times, and vacuum dried at 55°C for 8 h to obtain an anti-aging polyurethane material.
[0034] Example 2
[0035] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0036] (1) 3-glycidyloxypropyltrimethoxysilane, 2-aminoethyl hypophosphorous acid and anhydrous ethanol were mixed in a mass ratio of 1:1.3:10, 0.4 times the mass of 3-glycidyloxypropyltrimethoxysilane was added dropwise with a 1 mol / L sodium hydroxide aqueous solution, stirred at 700 r / min at 100°C for 10 h, filtered and the filtrate was collected to obtain hypophosphorous acid-modified silane;
[0037] (2) Octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:0.7:0.6:0.02, stirred at 85°C and 300 r / min for 2.5 h under a nitrogen atmosphere, heated to 100°C and continued to stir for 8 h, heated to 135°C at 15°C / min and continued to stir for 45 min, and distilled under a vacuum environment for 1.5 h to obtain modified polysiloxane;
[0038] (3) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene were mixed in a mass ratio of 1:1.7:10, stirred at 150 r / min for 30 min at 55°C, heated to 65°C and then vacuumed, stirred for 5 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 4 times, respectively, and vacuum dried at 50°C for 10 h to obtain a functional monomer;
[0039] (4) Diphenylmethane diisocyanate, polyethylene glycol, and N,N-dimethylformamide were mixed at a mass ratio of 1:2.5:10, and nitrogen was passed through the mixture. The mixture was stirred at 85°C and 300 r / min for 30 min. During the stirring process, the -NCO content was monitored by toluene dibutylamine titration method. After the prepolymerization reaction was completed, the temperature was lowered to 75°C, and a functional monomer with a mass of 0.4 times that of diphenylmethane diisocyanate was added and stirred for 4 h to obtain a polyurethane material.
[0040] (5) The polyurethane material, anhydrous aluminum chloride and chlorobenzene were mixed in a mass ratio of 1:0.35:11, stirred at 250 r / min at 1.5°C for 25 min, then 0.7 times the mass of resorcinol of the polyurethane material was added, the temperature was raised to 80°C, stirred for 5 h, and 0.5 times the mass of modified polysiloxane of the polyurethane material was added, the temperature was raised to 100°C, and stirring was continued for 3 h. The mixture was cooled to room temperature, and the solid was separated by centrifugation. The solid was washed with anhydrous ethanol for 4 times and vacuum dried at 60°C for 10 h to obtain an anti-aging polyurethane material.
[0041] Example 3
[0042] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0043] (1) Octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:0.8:0.7:0.03, stirred at 90°C and 400 r / min for 3 h under a nitrogen atmosphere, heated to 105°C and continued to stir for 9 h, heated to 140°C at 20°C / min and continued to stir for 50 min, and distilled under a vacuum environment for 2 h to obtain modified polysiloxane;
[0044] (2) Octamethylcyclotetrasiloxane, tetramethyltri-3-trifluoropropylcyclotetrasiloxane, DOPO modified silane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:1.3:0.8:0.7:0.03, stirred at 90°C and 400 r / min for 3 h under a nitrogen atmosphere, heated to 105°C and continued to stir for 9 h, heated to 140°C at 20°C / min and continued to stir for 50 min, and distilled under a vacuum environment for 2 h to obtain modified polysiloxane;
[0045] (3) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene were mixed in a mass ratio of 1:1.8:12, stirred at 200 r / min at 60°C for 40 min, heated to 70°C and then vacuumed, stirred for 6 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 5 times, respectively, and vacuum dried at 55°C for 12 h to obtain a functional monomer;
[0046] (4) Diphenylmethane diisocyanate, polyethylene glycol, and N,N-dimethylformamide were mixed in a mass ratio of 1:2.7:12, and nitrogen was passed through the mixture. The mixture was stirred at 400 r / min for 40 min at 90°C. During the stirring process, the -NCO content was monitored by toluene dibutylamine titration method. After the prepolymerization reaction was completed, the temperature was lowered to 80°C, and a functional monomer with a mass of 0.5 times that of diphenylmethane diisocyanate was added and stirred for 5 h to obtain a polyurethane material.
[0047] (5) The polyurethane material, anhydrous aluminum chloride and chlorobenzene were mixed in a mass ratio of 1:0.4:12, stirred at 300 r / min at 3°C for 30 min, then 0.8 times the mass of resorcinol of the polyurethane material was added, the temperature was raised to 85°C, stirred for 6 h, and 0.6 times the mass of modified polysiloxane of the polyurethane material was added, the temperature was raised to 105°C, and stirring was continued for 4 h. The mixture was cooled to room temperature, and the solid was separated by centrifugation. The solid was washed with anhydrous ethanol for 5 times and vacuum dried at 65°C for 12 h to obtain an anti-aging polyurethane material.
[0048] Comparative Example 1
[0049] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0050] (1) 3-glycidyloxypropyltrimethoxysilane, 2-aminoethyl hypophosphorous acid and anhydrous ethanol were mixed in a mass ratio of 1:1.3:10, 0.4 times the mass of 3-glycidyloxypropyltrimethoxysilane was added dropwise with a 1 mol / L sodium hydroxide aqueous solution, stirred at 700 r / min at 100°C for 10 h, filtered and the filtrate was collected to obtain hypophosphorous acid-modified silane;
[0051] (2) Octamethylcyclotetrasiloxane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:0.6:0.02, stirred at 85°C and 300 r / min for 2.5 h under a nitrogen atmosphere, heated to 100°C and continued to stir for 8 h, heated to 135°C at 15°C / min and continued to stir for 45 min, and distilled under a vacuum environment for 1.5 h to obtain modified polysiloxane;
[0052] (3) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene were mixed in a mass ratio of 1:1.7:10, stirred at 150 r / min for 30 min at 55°C, heated to 65°C and then vacuumed, stirred for 5 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 4 times, respectively, and vacuum dried at 50°C for 10 h to obtain a functional monomer;
[0053] (4) Diphenylmethane diisocyanate, polyethylene glycol, and N,N-dimethylformamide were mixed at a mass ratio of 1:2.5:10, and nitrogen was passed through the mixture. The mixture was stirred at 85°C and 300 r / min for 30 min. During the stirring process, the -NCO content was monitored by toluene dibutylamine titration method. After the prepolymerization reaction was completed, the temperature was lowered to 75°C, and a functional monomer with a mass of 0.4 times that of diphenylmethane diisocyanate was added and stirred for 4 h to obtain a polyurethane material.
[0054] (5) The polyurethane material, anhydrous aluminum chloride and chlorobenzene were mixed in a mass ratio of 1:0.35:11, stirred at 250 r / min at 1.5°C for 25 min, then 0.7 times the mass of resorcinol of the polyurethane material was added, the temperature was raised to 80°C, stirred for 5 h, and 0.5 times the mass of modified polysiloxane of the polyurethane material was added, the temperature was raised to 100°C, and stirring was continued for 3 h. The mixture was cooled to room temperature, and the solid was separated by centrifugation. The solid was washed with anhydrous ethanol for 4 times and vacuum dried at 60°C for 10 h to obtain an anti-aging polyurethane material.
[0055] Comparative Example 2
[0056] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0057] (1) 3-glycidyloxypropyltrimethoxysilane, 2-aminoethyl hypophosphorous acid and anhydrous ethanol were mixed in a mass ratio of 1:1.3:10, 0.4 times the mass of 3-glycidyloxypropyltrimethoxysilane was added dropwise with a 1 mol / L sodium hydroxide aqueous solution, stirred at 700 r / min at 100°C for 10 h, filtered and the filtrate was collected to obtain hypophosphorous acid-modified silane;
[0058] (2) Octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:0.7:0.02, stirred at 85°C and 300 r / min for 2.5 h under a nitrogen atmosphere, heated to 100°C and continued to stir for 8 h, heated to 135°C at 15°C / min and continued to stir for 45 min, and distilled under a vacuum environment for 1.5 h to obtain a modified polysiloxane;
[0059] (3) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene were mixed in a mass ratio of 1:1.7:10, stirred at 150 r / min for 30 min at 55°C, heated to 65°C and then vacuumed, stirred for 5 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 4 times, respectively, and vacuum dried at 50°C for 10 h to obtain a functional monomer;
[0060] (4) Diphenylmethane diisocyanate, polyethylene glycol, and N,N-dimethylformamide were mixed at a mass ratio of 1:2.5:10, and nitrogen was passed through the mixture. The mixture was stirred at 85°C and 300 r / min for 30 min. During the stirring process, the -NCO content was monitored by toluene dibutylamine titration method. After the prepolymerization reaction was completed, the temperature was lowered to 75°C, and a functional monomer with a mass of 0.4 times that of diphenylmethane diisocyanate was added and stirred for 4 h to obtain a polyurethane material.
[0061] (5) The polyurethane material, anhydrous aluminum chloride and chlorobenzene were mixed in a mass ratio of 1:0.35:11, stirred at 250 r / min at 1.5°C for 25 min, then 0.7 times the mass of resorcinol of the polyurethane material was added, the temperature was raised to 80°C, stirred for 5 h, and 0.5 times the mass of modified polysiloxane of the polyurethane material was added, the temperature was raised to 100°C, and stirring was continued for 3 h. The mixture was cooled to room temperature, and the solid was separated by centrifugation. The solid was washed with anhydrous ethanol for 4 times and vacuum dried at 60°C for 10 h to obtain an anti-aging polyurethane material.
[0062] Comparative Example 3
[0063] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0064] (1) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene were mixed in a mass ratio of 1:1.7:10, stirred at 150 r / min for 30 min at 55°C, heated to 65°C and then vacuumed, stirred for 5 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 4 times, respectively, and vacuum dried at 50°C for 10 h to obtain a functional monomer;
[0065] (2) Diphenylmethane diisocyanate, polyethylene glycol, and N,N-dimethylformamide were mixed at a mass ratio of 1:2.5:10, and nitrogen was passed through the mixture. The mixture was stirred at 85°C and 300 r / min for 30 min. During the stirring process, the -NCO content was monitored by toluene dibutylamine titration method. After the prepolymerization reaction was completed, the temperature was lowered to 75°C, and a functional monomer with a mass of 0.4 times that of diphenylmethane diisocyanate was added and stirred for 4 h to obtain a polyurethane material.
[0066] (3) The polyurethane material, anhydrous aluminum chloride and chlorobenzene were mixed uniformly in a mass ratio of 1:0.35:11, stirred at 250 r / min at 1.5°C for 25 min, and then 0.7 times the mass of resorcinol of the polyurethane material was added. The temperature was raised to 80°C, stirred for 5 h, cooled to room temperature, and the solid was separated by centrifugation. The solid was washed with anhydrous ethanol for 4 times and vacuum dried at 60°C for 10 h to obtain an anti-aging polyurethane material.
[0067] Comparative Example 4
[0068] A method for preparing an anti-aging polyurethane material comprises the following preparation steps:
[0069] (1) 3-glycidyloxypropyltrimethoxysilane, 2-aminoethyl hypophosphorous acid and anhydrous ethanol were mixed in a mass ratio of 1:1.3:10, 0.4 times the mass of 3-glycidyloxypropyltrimethoxysilane was added dropwise with a 1 mol / L sodium hydroxide aqueous solution, stirred at 700 r / min at 100°C for 10 h, filtered and the filtrate was collected to obtain hypophosphorous acid-modified silane;
[0070] (2) Octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide were mixed in a mass ratio of 1:0.7:0.6:0.02, stirred at 85°C and 300 r / min for 2.5 h under a nitrogen atmosphere, heated to 100°C and continued to stir for 8 h, heated to 135°C at 15°C / min and continued to stir for 45 min, and distilled under a vacuum environment for 1.5 h to obtain modified polysiloxane;
[0071] (3) Diphenylmethane diisocyanate, polyethylene glycol, and N,N-dimethylformamide were mixed at a mass ratio of 1:2.5:10, and nitrogen was passed through the mixture. The mixture was stirred at 85°C and 300 r / min for 30 min. During the stirring process, the -NCO content was monitored by toluene dibutylamine titration. After the prepolymerization reaction was completed, the temperature was lowered to 75°C, 1,4-butanediol (0.4 times the mass of diphenylmethane diisocyanate) was added, and the mixture was stirred for 4 h to obtain a polyurethane material.
[0072] (4) The polyurethane material, modified polysiloxane and chlorobenzene were mixed in a mass ratio of 1:0.5:10, stirred at 100°C and 400 r / min for 3 h, cooled to room temperature, centrifuged to separate the solid, washed with anhydrous ethanol for 4 times, and vacuum dried at 60°C for 10 h to obtain an anti-aging polyurethane material.
[0073] Test Example 1
[0074] Test method: The anti-aging polyurethane materials of each embodiment and comparative example were used to prepare standard specimens with a specification of 100 mm×6.5 mm×3.2 mm, and the limiting oxygen index of the standard specimens was tested. The results are shown in Table 1.
[0075] Table 1
[0076]
[0077] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the anti-aging polyurethane material prepared by the present invention has good flame retardant properties.
[0078] By comparison, the limiting oxygen index of Examples 1 to 3 is significantly greater than that of Comparative Example 2, indicating that hypophosphorous acid modified silane introduces hypophosphorous acid into linear polysiloxane, and the introduction of phosphorus-containing groups improves the flame retardant properties of the anti-aging polyurethane material; the limiting oxygen index of Examples 1 to 3 is significantly greater than that of Comparative Example 4, indicating that 4-hydroxybutyraldehyde and 2-chloro-4,6-diamino-1,3,5-triazine are reacted through the dehydration condensation reaction of amino and aldehyde groups to prepare functional monomers, and the triazine structure contains rich nitrogen, which will produce nitrogen when heated, and has a gas-phase flame retardant effect, and also has a carbonizing effect, which can synergistically flame retard with the phosphorus on the polysiloxane, thereby improving the flame retardant properties of the anti-aging polyurethane material.
[0079] Test Example 2
[0080] Tensile strength test method: CMT4204 tensile testing machine of Mester Industrial (China) Co., Ltd. was used to test the tensile strength and elongation at break of the dumbbell-shaped specimens, and the tensile rate was set to 200 mm / min.
[0081] Aging resistance: Use a xenon lamp to simulate sunlight, put the sample into a xenon lamp accelerated aging test chamber, the aging time is 360h, the experimental atmosphere is air, the temperature is 65℃, the light source is 25cm away from the sample, and the radiation intensity is 550W / m 2 , the tensile strength was tested again, and the performance decline rate was calculated as 1-tensile strength after aging / initial tensile strength. The results are shown in Table 2.
[0082] Table 2
[0083]
[0084] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 2, it can be found that the anti-aging polyurethane material prepared by the present invention has good tensile strength and anti-aging performance.
[0085] By comparison, the tensile strength of Examples 1 to 3 is significantly greater than that of Comparative Examples 2 and 4, indicating that the phosphorus hydrogen on the modified polysiloxane hypophosphorous acid reacts with the imine bond on the polyurethane material to form a stable cross-linked structure, thereby improving the tensile strength of the anti-aging polyurethane material.
[0086] By comparison, the performance degradation rates of Examples 1 to 3 are significantly lower than that of Comparative Example 3, indicating that the Si-O-Si structure on the polysiloxane is difficult to break under thermal motion, has good thermal stability, can maintain good tensile strength under photothermal conditions, and improves the anti-aging performance of the anti-aging polyurethane material; the performance degradation rates of Examples 1 to 3 are significantly lower than that of Comparative Example 4, indicating that the conjugated hydrogen-bonded six-membered ring structure formed by the reaction of Cl on the functionalized monomer with hydroquinone can convert light energy into heat energy through ring opening and ring closing, and has good ultraviolet light absorption effect, thereby improving the anti-aging performance of the anti-aging polyurethane material.
[0087] Test Example 3
[0088] Hydrophobic performance test:
[0089] Test method: The contact angle test was conducted using a Y-82 contact angle tester from Kruss DSA, Germany. The test contact medium was deionized water, the droplet size was 5 μL, and the contact time was 60 seconds. The results are shown in Table 3.
[0090] Table 3
[0091]
[0092] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 3, it can be found that the anti-aging polyurethane material prepared by the present invention has good hydrophobic properties.
[0093] By comparison, the contact angles of Examples 1 to 3 are significantly greater than the contact angles of Comparative Examples 1 and 3, indicating that 3,3,3-trifluoropropylmethyldimethoxysilane introduces fluorine-containing groups on the linear polysiloxane, and the fluorine-containing groups can reduce the surface energy of the material and improve the hydrophobic properties of the anti-aging polyurethane material.
[0094] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An anti-aging polyurethane material, characterized in that: The anti-aging polyurethane material is prepared by reacting modified polysiloxane, polyurethane material and resorcinol; The modified polysiloxane is prepared by reacting octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane and hypophosphorous acid modified silane; The reaction equation of hypophosphorous acid modified silane is: ; The reaction equation of modified polysiloxane is: ; The polyurethane material is prepared by reacting 4,4-diisocyanate dicyclohexylmethane, polyethylene glycol and functional monomers; The reaction equation of the functional monomer is: ; The reaction equation of polyurethane material is: 。 2. A method for preparing an anti-aging polyurethane material, characterized in that: The method comprises the following preparation steps: (1) Mix 3-glycidylpropyl(dimethoxy)methylsilane, 2-aminoethylphosphorous acid and anhydrous ethanol in a mass ratio of 1:(1.2-1.4):(8-12), add dropwise 1 mol / L sodium hydroxide aqueous solution with a mass of 0.3-0.5 times that of 3-glycidylpropyl(dimethoxy)methylsilane, stir at 95-105°C and 600-800 r / min for 9-11 hours, filter and collect the filtrate to obtain hypophosphorous acid-modified silane; (2) Octamethylcyclotetrasiloxane, 3,3,3-trifluoropropylmethyldimethoxysilane, hypophosphorous acid modified silane and tetramethylammonium hydroxide silicon alkoxide are mixed in a mass ratio of 1: (0.6-0.8): (0.5-0.7): (0.01-0.03), stirred at 80-90°C and 200-400 r / min for 2-3 h under a nitrogen atmosphere, heated to 95-105°C and continued to stir for 7-9 h, heated to 130-140°C at 10-20°C / min and continued to stir for 40-50 min, and distilled under a vacuum environment for 1-2 h to obtain modified polysiloxane; (3) 4-hydroxybutyraldehyde, 2-chloro-4,6-diamino-1,3,5-triazine and xylene are mixed in a mass ratio of 1: (1.6-1.8): (8-12), stirred at 50-60°C at 100-200 r / min for 20-40 min, heated to 60-70°C and then vacuumed, stirred for 4-6 h, filtered, and the residue was washed with xylene and anhydrous ethanol for 3-5 times, respectively, and vacuum dried at 45-55°C for 8-12 h to obtain a functional monomer; (4) Mix 4,4-diisocyanate dicyclohexylmethane, polyethylene glycol, and N,N-dimethylformamide in a mass ratio of 1: (2.3-2.7): (8-12), and stir at 200-400 r / min for 20-40 min at 80-90°C under nitrogen protection. During the stirring process, monitor the -NCO content by toluene dibutylamine titration method. After the prepolymerization reaction is completed, lower the temperature to 70-80°C, add a functional monomer in an amount of 0.3-0.5 times the mass of 4,4-diisocyanate dicyclohexylmethane, and continue stirring for 3-5 h to obtain a polyurethane material; (5) The polyurethane material, anhydrous aluminum chloride and chlorobenzene are mixed uniformly in a mass ratio of 1: (0.3-0.4): (10-12), stirred at 200-300 r / min at 0-3°C for 20-30 min, then 0.6-0.8 times the mass of resorcinol of the polyurethane material is added, the temperature is raised to 75-85°C, stirred for 4-6 h, 0.4-0.6 times the mass of modified polysiloxane of the polyurethane material is added, the temperature is raised to 95-105°C, stirring is continued for 2-4 h, cooled to room temperature, centrifuged to separate the solid, washed with anhydrous ethanol for 3-5 times, and vacuum dried at 55-65°C for 8-12 h to obtain an anti-aging polyurethane material.
3. The method for preparing an anti-aging polyurethane material according to claim 2, characterized in that: The polyethylene glycol in step (4) has a molecular weight of 1000.