A non-silicon release film and preparation method thereof

A method using nano starch crystals and cross-linked microspheres addresses the issues of high viscosity and cracking in non-silicone release films, achieving a film with moderate release force, high transparency, and good durability using water as a solvent, thus improving environmental friendliness and performance.

CN118791767BActive Publication Date: 2024-12-03WEIFANG FUWEI PLASTIC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411244254.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-03
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Existing non-silicone release films prepared with water as a solvent face issues of high viscosity, low durability, poor transparency, and surface cracking due to the use of acrylate resin, and acrylate resin's poor durability and adhesion.

Method used

A method involving the preparation of nano starch crystals and cross-linked microspheres is used to create a coating material solution, which includes mixing nano starch crystals, tannic acid, formaldehyde, L-lysine, ethylenediamine, and cross-linked microspheres, along with specific ratios and conditions, to form a coating material solution that is then applied to a polyester substrate through melt extrusion and shaping.

Benefits of technology

The method results in a non-silicone release film with moderate release force, high transparency, good durability, and no surface cracks, while using environmentally friendly water as a solvent and reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a non-silicon release film and a preparation method thereof, belonging to the technical field of non-silicon release films. The preparation method comprises the following steps: preparing a coating material solution, pre-treating, melt extruding, and shaping; the preparation of the coating material solution comprises the following steps: preparing a viscosity reducer, preparing cross-linked microspheres, and mixing; the shaping comprises preheating at 110-120°C, longitudinally stretching a cast sheet at 120-130°C to obtain a base film; coating the coating material solution on one surface of the base film, controlling the coating thickness to be 4-5μm, and obtaining the coated base film; preheating at 110-120°C, transversely stretching the coated base film at 120-130°C, and then heat-setting; the preparation method of the invention uses water as a solvent for the coating material, and the prepared non-silicon release film has moderate release force, good durability, high transparency, and no cracks on the surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of non-silicon release films, and in particular to a non-silicon release film and a preparation method thereof. Background Art

[0002] Release film is a film material with a special non-sticky surface, which is composed of a substrate and a coating. The commonly used substrate materials are plastic films such as polyethylene and polyester. The coating gives the film non-stick or low-stick properties. The commonly used coating material is silicone oil. However, release films prepared with silicone oil as the coating material have the disadvantages of poor environmental protection and high temperature stability.

[0003] Non-silicone release film is a thin film material with special functions. Unlike traditional silicon-based release films, the coating material of non-silicone release film does not contain silicon, which is environmentally friendly. In addition, non-silicone release film has excellent transparency, chemical stability, and high-temperature stability. It can also play an excellent release effect under high temperature and strong acid and alkali environment. Non-silicone release film is mainly used in the preparation of tiny structures and devices in the fields of semiconductors, optoelectronics, microelectronics, etc. In semiconductor preparation, non-silicone release film is mainly used to prepare photolithography masks, photoresists, electron beam exposure masks, etc. Therefore, non-silicone release film has important application value.

[0004] The methods for preparing non-silicon release films mainly include solution impregnation method, vapor deposition method, and self-assembly method. Among them, the solution impregnation method is to deposit the precursor substance in the solution on the surface of the substrate to form a film layer; the vapor deposition method is to use the precursor molecules in the gas to deposit on the surface of the substrate to form a thin film; the self-assembly method is to use the interaction between molecules to spontaneously form a film layer on the surface of the substrate. Among them, the solution impregnation method is the simplest and most commonly used method.

[0005] The solution impregnation method is to dissolve the coating material in a solvent to form a coating material solution, and then evenly apply the coating material solution to the surface of the substrate by spin coating, spray coating or dipping. The commonly used solvents are water or organic solvents such as alcohols, esters, ketones, and ethers. Considering that organic solvents are highly toxic and volatile, causing environmental pollution, as people's awareness of environmental protection and sustainable development increases, more and more people choose to use water as a solvent for coating materials.

[0006] However, when water is used as a solvent for coating materials, the following problems are found: compared with organic solvents, the coating material solution prepared with water as a solvent has a large viscosity. In order to reduce the viscosity, the solid content of the coating material is generally reduced, which will cause the prepared non-silicone release film to have too small a release force and poor durability; compared with organic solvents, the coating material solution prepared with water as a solvent has a slow drying speed and is prone to uneven drying, which will cause the prepared non-silicone release film to have a decreased transparency.

[0007] In order to solve the above problems, the most commonly used method is to add acrylate resin to the coating material. Acrylate resin can increase the solid content of the coating material solution, increase the drying temperature and increase the drying air volume. However, the durability and adhesion of acrylate resin are poor. Therefore, although it can improve the problems of non-silicone release film to a certain extent, the improvement effect is not obvious. Increasing the drying temperature and increasing the drying air volume will cause cracks on the surface of the release film during the drying process. Summary of the invention

[0008] In view of the shortcomings of the prior art, the present invention provides a non-silicone release film and a preparation method thereof. Water is used as the solvent of the coating material. The prepared non-silicone release film has moderate release force, good durability, high transparency, and no cracks on the surface.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing a non-silicon release film, comprising the following steps: preparing a coating material solution, pre-treating, melt extruding, and shaping;

[0011] The method for preparing the coating material solution comprises the following steps: preparing a viscosity reducing agent, preparing cross-linked microspheres, and mixing;

[0012] The method for preparing the viscosity reducing agent comprises the following steps: preparing nano starch crystals and coating them;

[0013] The nano starch crystals are prepared by mixing corn starch and deionized water, heating to boiling, maintaining for 20-25 minutes, then cooling to 10-12° C., adding anhydrous ethanol dropwise thereto, stirring at a stirring speed of 100-200 rpm for 20-30 minutes after the addition is completed, standing for 40-50 minutes, centrifuging at a speed of 9000-10000 rpm for 9-10 minutes, taking a precipitate, washing the precipitate with deionized water for 3-5 times, and vacuum drying at 60-70° C. to obtain nano starch crystals;

[0014] In the preparation of the nano starch crystals, the mass volume ratio of corn starch, deionized water and anhydrous ethanol is 2000-2400 g: 20-24 L: 20-26 L;

[0015] The dropping speed of the anhydrous ethanol is 90-100 mL / min;

[0016] The coating comprises mixing the nano starch crystals, tannic acid and the first portion of deionized water, stirring at a speed of 400-500 rpm for 40-50 minutes at room temperature, dropping formaldehyde aqueous solution, continuing stirring for 40-50 minutes after the dropping is completed, centrifuging at a speed of 9000-10000 rpm for 9-10 minutes, taking a precipitate, adding L-lysine, ethylenediamine and the second portion of deionized water to the precipitate, stirring at a speed of 200-300 rpm for 4-5 hours at 70-75° C., centrifuging at a speed of 9000-10000 rpm for 9-10 minutes, taking a precipitate, washing the precipitate with deionized water for 3-5 times, and freeze-drying at -40° C. to -35° C. for 25-30 hours to obtain a viscosity reducer;

[0017] In the coating, the mass volume ratio of the nano starch crystal, tannic acid, the first portion of deionized water, the formaldehyde aqueous solution, L-lysine, ethylenediamine, and the second portion of deionized water is 400-460 g: 600-700 g: 70-80 L: 100-120 mL: 50-60 g: 40-50 g: 60-70 L;

[0018] The concentration of the formaldehyde aqueous solution is 37wt%;

[0019] The drop rate of the formaldehyde aqueous solution is 20-30 mL / min;

[0020] The cross-linked microspheres are prepared by mixing ethyl methacrylate, lauryl methacrylate, N-vinyl pyrrolidone, dipentaerythritol hexaacrylate, polyvinyl pyrrolidone, deionized water, and ethylene glycol monomethyl ether, stirring at 200-300 rpm for 30-40 min at room temperature under the protection of nitrogen, adding azobisisobutyronitrile, stirring at 200-300 rpm for 16-18 h at 70-75° C., centrifuging at 4000-5000 rpm for 4-5 min, taking a precipitate, washing the precipitate with deionized water for 3-5 times, and freeze-drying at -40° C. to -35° C. for 30-35 h to obtain cross-linked microspheres;

[0021] In the preparation of the cross-linked microspheres, the mass volume ratio of ethyl methacrylate, dodecyl methacrylate, N-vinyl pyrrolidone, dipentaerythritol hexaacrylate, polyvinyl pyrrolidone, deionized water, ethylene glycol monomethyl ether, and azobisisobutyronitrile is 1000-1200g:360-400g:600-800g:120-140g:120-140g:26-28L:4-6L:24-26g;

[0022] The mixing comprises mixing sodium methacrylic acid sulfonate and the first portion of deionized water, and then high shearing them at a speed of 5000-6000 rpm for 4-5 minutes at room temperature under the protection of nitrogen; adding methyl methacrylate, methacrylic acid, butyl acrylate, and hydroxyethyl methacrylate, and then high shearing them at a speed of 5000-6000 rpm for 10-15 minutes at 70-75° C. under the protection of nitrogen; adding trimethylolpropane trimethacrylate, and continuing to high shear them at a speed of 5000-6000 rpm for 10-15 minutes at 70-75° C.; adding potassium persulfate, and continuing to high shear them at a speed of 5000-6000 rpm for 3-3.5 hours at 70-75° C.; adding the second portion of deionized water, a viscosity reducer, cross-linked microspheres, and a water-soluble antistatic agent, and continuing to high shear them at a speed of 5000-6000 rpm for 15 minutes at 70-75° C. to obtain a coating material solution;

[0023] In the mixture, the mass volume ratio of sodium methacrylate sulfonate, the first portion of deionized water, methyl methacrylate, methacrylic acid, butyl acrylate, hydroxyethyl methacrylate, trimethylolpropane trimethacrylate, potassium persulfate, the second portion of deionized water, viscosity reducer, crosslinked microspheres, and water-soluble antistatic agent is 520-560g:36-38L:6000-6800g:3200-4000g:1120-1280g:680-800g:400-440g:200-240g:20-20.8L:960-1080g:1400-1600g:600-640g;

[0024] The water-soluble antistatic agent is MI00-10T water-soluble antistatic agent produced by Mooney Chemical Technology (Shanghai) Co., Ltd.

[0025] The pretreatment uses hot air at 130-135° C. to pre-crystallize the polyester chips for 20-25 minutes, then dries them at 155-160° C. for 20-25 minutes, and dries them at 145-150° C. for 5.5-6.5 hours to obtain pretreated polyester chips;

[0026] The melt extrusion is to divide the pretreated polyester chips into three parts as A layer raw material, B layer raw material and C layer raw material, respectively put them into the corresponding extruders, control the heating zone temperature of the main extruder and the auxiliary extruder to be 275-285° C. After melt extrusion, cool and solidify them on the surface of the casting roller to form casting sheets;

[0027] In the melt extrusion, the mass ratio of the raw material of layer A, the raw material of layer B, and the raw material of layer C is 12-15:65-70:12-15;

[0028] The shaping process comprises preheating at 110-120° C., longitudinally stretching the cast sheet at 120-130° C., controlling the longitudinal stretching ratio to be 3.5-4, and obtaining a base film; coating a coating material solution on one surface of the base film, controlling the coating thickness to be 4-5 μm, and obtaining a coated base film; preheating at 110-120° C., transversely stretching the coated base film at 120-130° C., controlling the transverse stretching ratio to be 4-4.2, and then heat-setting at 230-240° C. for 3-5 seconds to obtain a non-silicone release film.

[0029] A non-silicon release film prepared by the above-mentioned preparation method.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The method for preparing the non-silicone release film of the present invention uses water as the solvent of the coating material, which is highly environmentally friendly and causes little pollution to the environment;

[0032] (2) The non-silicone release film of the present invention has a moderate release force of 27-30 g / in and a residual bonding rate of 94-95%;

[0033] (3) The non-silicone release film of the present invention has good durability, with a release force of 29-31 g / in after aging at 70°C for 20 hours and a residual bonding rate of 90-92% after aging at 70°C for 20 hours;

[0034] (4) The non-silicone release film of the present invention has high transparency, a light transmittance of 89.0-89.4%, and a haze of 2.7-3.0%;

[0035] (5) The non-silicone release film of the present invention has no surface cracks. DETAILED DESCRIPTION

[0036] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0037] Example 1

[0038] A method for preparing a non-silicon release film, specifically comprising:

[0039] 1. Prepare coating material solution:

[0040] (1) Preparation of viscosity reducer: 2000 g corn starch and 20 L deionized water were mixed, heated to boiling, maintained at boiling temperature for 20 min, then cooled to 10°C, 20 L anhydrous ethanol was added dropwise at a rate of 90 mL / min, stirred at a rate of 100 rpm for 20 min after the addition was completed, allowed to stand for 40 min, centrifuged at a rate of 9000 rpm for 9 min, the precipitate was taken, the precipitate was washed with deionized water for 3 times, and vacuum dried at 60°C to obtain nano starch crystals; then 400 g nano starch crystals, 600 g tannic acid, and 70 L deionized water were mixed, stirred at a rate of 400 rpm for 40 min at room temperature, 100 mL 37 wt % formaldehyde aqueous solution was added dropwise at a rate of 20 mL / min, stirring was continued for 40 min after the addition was completed, the precipitate was centrifuged at a rate of 9000 rpm for 9 min, 50 g L-lysine, 40 g ethylenediamine, and 60 L deionized water were stirred at 200 rpm for 4 h at 70 ° C, centrifuged at 9000 rpm for 9 min, and the precipitate was taken, washed with deionized water for 3 times, and freeze-dried at -40 ° C for 25 h to obtain a viscosity reducer;

[0041] (2) Preparation of cross-linked microspheres: 1000 g of ethyl methacrylate, 360 g of dodecyl methacrylate, 600 g of N-vinyl pyrrolidone, 120 g of dipentaerythritol hexaacrylate, 120 g of polyvinyl pyrrolidone, 26 L of deionized water, and 4 L of ethylene glycol monomethyl ether were mixed, and stirred at 200 rpm for 30 min at room temperature under the protection of nitrogen. 24 g of azobisisobutyronitrile was added, and the mixture was stirred at 200 rpm for 16 h at 70 ° C. The mixture was centrifuged at 4000 rpm for 4 min, and the precipitate was taken. The precipitate was washed three times with deionized water and freeze-dried at -40 ° C for 30 h to obtain cross-linked microspheres.

[0042] (3) Mixing: 520 g of sodium methacrylic acid sulfonate and 36 L of deionized water were mixed, and then high sheared at 5000 rpm for 4 min at room temperature under the protection of nitrogen. 6000 g of methyl methacrylate, 3200 g of methacrylic acid, 1120 g of butyl acrylate and 680 g of hydroxyethyl methacrylate were added and mixed, and then high sheared at 5000 rpm for 10 min at 70° C. under the protection of nitrogen. 400 g of trimethylolpropane trimethacrylate was added, and high shearing was continued at 5000 rpm for 10 min at 70° C. 200 g of potassium persulfate was added, and high shearing was continued at 5000 rpm for 3 h at 70° C. 20 L of deionized water, 960 g of viscosity reducer, 1400 g of cross-linked microspheres and 600 g of water-soluble antistatic agent were added, and high shearing was continued at 5000 rpm for 15 min at 70° C. to obtain a coating material solution.

[0043] The water-soluble antistatic agent is MI00-10T water-soluble antistatic agent produced by Mooney Chemical Technology (Shanghai) Co., Ltd.

[0044] 2. Pretreatment: Use hot air at 130°C to pre-crystallize the polyester chips for 20 minutes, then dry them at 155°C for 20 minutes and at 145°C for 5.5 hours to obtain pretreated polyester chips;

[0045] 3. Melt extrusion: the pretreated polyester chips are divided into three parts as A layer raw material, B layer raw material and C layer raw material, respectively put into the corresponding extruders, wherein the mass ratio of A layer raw material, B layer raw material and C layer raw material is 12:65:12, and the heating zone temperature of the main extruder and the auxiliary extruder is controlled to be 275°C. After melt extrusion, the chips are cooled and solidified on the surface of the casting roller to form casting sheets;

[0046] 4. Setting: After preheating at 110°C, the cast sheet is longitudinally stretched at 120°C, and the longitudinal stretching ratio is controlled to be 3.5 to obtain a base film; the coating material solution is coated on one surface of the base film, and the coating thickness is controlled to be 4 μm to obtain a coated base film; after preheating at 110°C, the coated base film is transversely stretched at 120°C, and the transverse stretching ratio is controlled to be 4, and then heat-set at 230°C for 3s to obtain a non-silicone release film.

[0047] This embodiment also provides a non-silicon release film prepared by the aforementioned preparation method.

[0048] Example 2

[0049] A method for preparing a non-silicon release film, specifically comprising:

[0050] 1. Prepare coating material solution:

[0051] (1) Preparation of viscosity reducer: 2200 g corn starch and 22 L deionized water were mixed, heated to boiling, maintained at boiling temperature for 22 min, then cooled to 11°C, 24 L anhydrous ethanol was added dropwise at a rate of 95 mL / min, stirred at a rate of 150 rpm for 25 min after the addition was completed, allowed to stand for 45 min, centrifuged at 9500 rpm for 9 min, the precipitate was taken, the precipitate was washed with deionized water for 4 times, and vacuum dried at 65°C to obtain nano starch crystals; then 440 g nano starch crystals, 660 g tannic acid, and 76 L deionized water were mixed, stirred at 450 rpm for 45 min at room temperature, 110 mL 37 wt % formaldehyde solution was added dropwise at a rate of 24 mL / min, the addition was continued for 45 min, centrifuged at 9500 rpm for 9 min, the precipitate was taken, and 56 g L-lysine, 44 g ethylenediamine, and 64 L deionized water were stirred at 250 rpm for 4.5 h at 70 ° C, centrifuged at 9500 rpm for 9 min, and the precipitate was taken, washed with deionized water for 4 times, and freeze-dried at -40 ° C for 28 h to obtain a viscosity reducer;

[0052] (2) Preparation of cross-linked microspheres: 1100 g of ethyl methacrylate, 380 g of dodecyl methacrylate, 700 g of N-vinyl pyrrolidone, 130 g of dipentaerythritol hexaacrylate, 140 g of polyvinyl pyrrolidone, 27 L of deionized water, and 5 L of ethylene glycol monomethyl ether were mixed, and stirred at 250 rpm for 35 min at room temperature under the protection of nitrogen. 25 g of azobisisobutyronitrile was added, and the mixture was stirred at 250 rpm for 17 h at 70 °C, and centrifuged at 4500 rpm for 5 min. The precipitate was taken, and the precipitate was washed 4 times with deionized water, and freeze-dried at -40 °C for 32 h to obtain cross-linked microspheres.

[0053] (3) Mixing: 540 g of sodium methacrylic acid sulfonate and 36.8 L of deionized water were mixed, and then high sheared at 5500 rpm for 5 min at room temperature under the protection of nitrogen. 6400 g of methyl methacrylate, 3600 g of methacrylic acid, 1200 g of butyl acrylate and 720 g of hydroxyethyl methacrylate were added and mixed, and then high sheared at 5500 rpm for 12 min at 70° C. under the protection of nitrogen. 420 g of trimethylolpropane trimethacrylate was added, and high shearing was continued at 5500 rpm for 12 min at 70° C., 220 g of potassium persulfate was added, and high shearing was continued at 5500 rpm for 3 h at 70° C., 20.4 L of deionized water, 1000 g of viscosity reducer, 1520 g of cross-linked microspheres and 620 g of water-soluble antistatic agent were added, and high shearing was continued at 5500 rpm for 15 min at 70° C. to obtain a coating material solution.

[0054] The water-soluble antistatic agent is MI00-10T water-soluble antistatic agent produced by Mooney Chemical Technology (Shanghai) Co., Ltd.

[0055] 2. Pretreatment: Use hot air at 130°C to pre-crystallize the polyester chips for 22 minutes, then dry them at 155°C for 22 minutes and at 145°C for 6 hours to obtain pretreated polyester chips;

[0056] 3. Melt extrusion: the pretreated polyester chips are divided into three parts as A layer raw material, B layer raw material and C layer raw material, respectively put into the corresponding extruders, wherein the mass ratio of A layer raw material, B layer raw material and C layer raw material is 14:68:13, the heating zone temperature of the main extruder and the auxiliary extruder is controlled to be 280°C, and after melt extrusion, they are cooled and solidified on the surface of the casting roller to form casting sheets;

[0057] 4. Setting: After preheating at 115°C, the cast sheet is longitudinally stretched at 125°C, and the longitudinal stretching ratio is controlled to be 3.5 to obtain a base film; the coating material solution is coated on one surface of the base film, and the coating thickness is controlled to be 4.5 μm to obtain a coated base film; after preheating at 115°C, the coated base film is transversely stretched at 125°C, and the transverse stretching ratio is controlled to be 4, and then heat-set at 235°C for 4s to obtain a non-silicone release film.

[0058] This embodiment also provides a non-silicon release film prepared by the aforementioned preparation method.

[0059] Example 3

[0060] A method for preparing a non-silicon release film, specifically comprising:

[0061] 1. Prepare coating material solution:

[0062] (1) Preparation of viscosity reducer: 2400 g corn starch and 24 L deionized water were mixed, heated to boiling, maintained for 25 min, then cooled to 12°C, 26 L anhydrous ethanol was added dropwise at a rate of 100 mL / min, stirred at 200 rpm for 30 min after the addition was completed, allowed to stand for 50 min, centrifuged at 10,000 rpm for 10 min, the precipitate was taken, the precipitate was washed with deionized water for 5 times, and vacuum dried at 70°C to obtain nano starch crystals; then 460 g nano starch crystals, 700 g tannic acid, and 80 L deionized water were mixed, stirred at 500 rpm for 50 min at room temperature, 120 mL 37 wt % formaldehyde aqueous solution was added dropwise at a rate of 30 mL / min, stirring was continued for 50 min after the addition was completed, centrifuged at 10,000 rpm for 10 min, the precipitate was taken, and 60 g L-lysine, 50 g ethylenediamine, and 70 L deionized water were stirred at 300 rpm for 5 h at 75 ° C, centrifuged at 10000 rpm for 10 min, and the precipitate was taken, washed with deionized water for 5 times, and freeze-dried at -35 ° C for 30 h to obtain a viscosity reducer;

[0063] (2) Preparation of cross-linked microspheres: 1200 g of ethyl methacrylate, 400 g of dodecyl methacrylate, 800 g of N-vinyl pyrrolidone, 140 g of dipentaerythritol hexaacrylate, 140 g of polyvinyl pyrrolidone, 28 L of deionized water, and 6 L of ethylene glycol monomethyl ether were mixed, and stirred at 300 rpm for 40 min at room temperature under the protection of nitrogen. 26 g of azobisisobutyronitrile was added, and the mixture was stirred at 300 rpm for 18 h at 75 °C, and centrifuged at 5000 rpm for 5 min. The precipitate was taken, and the precipitate was washed 5 times with deionized water, and freeze-dried at -35 °C for 35 h to obtain cross-linked microspheres.

[0064] (3) Mixing: 560 g of sodium methacrylic acid sulfonate and 38 L of deionized water were mixed, and then high sheared at 6000 rpm for 5 min at room temperature under the protection of nitrogen. 6800 g of methyl methacrylate, 4000 g of methacrylic acid, 1280 g of butyl acrylate and 800 g of hydroxyethyl methacrylate were added and mixed, and then high sheared at 6000 rpm for 15 min at 75° C. under the protection of nitrogen. 440 g of trimethylolpropane trimethacrylate was added, and high shearing was continued at 6000 rpm for 15 min at 75° C. 240 g of potassium persulfate was added, and high shearing was continued at 6000 rpm for 3.5 h at 75° C. 20.8 L of deionized water, 1080 g of viscosity reducer, 1600 g of cross-linked microspheres and 640 g of water-soluble antistatic agent were added, and high shearing was continued at 6000 rpm for 15 min at 75° C. to obtain a coating material solution.

[0065] The water-soluble antistatic agent is MI00-10T water-soluble antistatic agent produced by Mooney Chemical Technology (Shanghai) Co., Ltd.

[0066] 2. Pretreatment: Use hot air at 135°C to pre-crystallize the polyester chips for 25 minutes, then dry them at 160°C for 25 minutes and at 150°C for 6.5 hours to obtain pretreated polyester chips;

[0067] 3. Melt extrusion: the pretreated polyester chips are divided into three parts as A layer raw material, B layer raw material and C layer raw material, respectively put into the corresponding extruders, wherein the mass ratio of A layer raw material, B layer raw material and C layer raw material is 15:70:15, the heating zone temperature of the main extruder and the auxiliary extruder is controlled to be 285°C, and after melt extrusion, they are cooled and solidified on the surface of the casting roller to form casting sheets;

[0068] 4. Shaping: After preheating at 120°C, the cast sheet is longitudinally stretched at 130°C, and the longitudinal stretching ratio is controlled to be 4 to obtain a base film; the coating material solution is coated on one surface of the base film, and the coating thickness is controlled to be 5 μm to obtain a coated base film; after preheating at 120°C, the coated base film is transversely stretched at 130°C, and the transverse stretching ratio is controlled to be 4.2, and then heat-set at 240°C for 5s to obtain a non-silicone release film.

[0069] This embodiment also provides a non-silicon release film prepared by the aforementioned preparation method.

[0070] Comparative Example 1

[0071] The method for preparing the non-silicone release film described in Example 1 is adopted, except that: in the step of preparing the coating material solution in step 1, the step of preparing the viscosity reducing agent in step (1) is omitted, and the addition of the viscosity reducing agent in the mixing step in step (3) is omitted.

[0072] This comparative example also provides a non-silicon release film prepared by the aforementioned preparation method.

[0073] Comparative Example 2

[0074] The method for preparing the non-silicone release film described in Example 1 is adopted, except that: in the step of preparing the coating material solution in step 1, the step of preparing the cross-linked microspheres in step (2) is omitted, and the addition of the cross-linked microspheres in the mixing step (3) is omitted.

[0075] This comparative example also provides a non-silicon release film prepared by the aforementioned preparation method.

[0076] Test Example 1

[0077] The release force, residual adhesion rate, 70°C × 20h aging release force, 70°C × 20h aging residual adhesion rate, light transmittance, and haze of the non-silicone release films prepared in Examples 1-3 and Comparative Examples 1-2 were tested, and the surface was observed to see if cracks appeared. The observation results are as follows:

[0078]

[0079] When testing the release force, the Nitto 31B test tape is used for bonding and the tensile force is measured when peeling at an angle of 180° and a peeling speed of 300mm / min.

[0080] When testing the residual bonding rate, use the Nitto 31B test tape to stick to the release surface of the release film, then peel it off, and test the adhesion value of the Nitto 31B test tape after peeling off, which is taken as B; test the adhesion value of the Nitto 31B test tape after not sticking to the release surface of the release film, which is taken as A; calculate the residual bonding rate, residual bonding rate = B / A×100%;

[0081] 70℃×20h aging release force: When testing the release force, Nitto 31B test tape is laminated to the release surface of the release film, aged at 70℃ for 20h, and the tensile force is measured when peeling at an angle of 180° and a peeling speed of 300mm / min.

[0082] When testing the residual adhesion rate after aging at 70℃×20h, the Nitto 31B test tape is laminated to the release surface of the release film, aged at 70℃ for 20h, peeled off, and the adhesion value of the Nitto 31B test tape after peeling is tested as D; the adhesion value of the Nitto 31B test tape not laminated to the release surface of the release film is tested as C; the residual adhesion rate after aging at 70℃×20h is calculated, and the residual adhesion rate after aging at 70℃×20h=D / C×100%.

[0083] It can be seen from the above results that adding viscosity reducers and cross-linked microspheres to the coating material solution can improve the release force, residual adhesion rate, durability and transparency of the prepared non-silicone release film to a certain extent, and avoid cracking on the surface of the non-silicone release film.

[0084] The preparation method of the viscosity reducer is as follows: after preparing nano starch crystals, using the hydroxyl groups and high specific surface area on the surface of the nano starch crystals, the nano starch crystals are added to tannic acid for adsorption, and then formaldehyde is added for further adsorption to obtain the nano starch crystals after adsorbing the tannic acid and formaldehyde; then the nano starch crystals after adsorbing the tannic acid and formaldehyde are mixed with lysine and ethylenediamine, and the tannic acid, formaldehyde, lysine and ethylenediamine undergo a Mannich reaction to obtain a Mannich base, so that the obtained viscosity reducer is the nano starch crystals with the Mannich base coated on the surface. The presence of the Mannich base can improve the fluidity of the coating material solution and reduce the viscosity of the coating material solution; it can also improve the internal bonding force of the coating material, avoid a significant increase in the release force or a significant decrease in the residual bonding rate after high-temperature aging, thereby improving the durability of the non-silicon release film; in addition, it can also reduce the release force between the coating material and the substrate, promote heat dispersion during drying, increase the drying speed of the coating material solution, and avoid cracking of the non-silicon release film during drying.

[0085] The cross-linked microspheres are cross-linked microspheres formed by copolymerization of methacrylates, N-vinyl pyrrolidone, and dipentaerythritol hexaacrylate with different molecular weights. Methacrylates with different molecular weights can improve the compatibility and bonding strength between the cross-linked microspheres and the coating material, N-vinyl pyrrolidone can improve the dispersibility of the cross-linked microspheres, and dipentaerythritol hexaacrylate can improve the cross-linking density of the cross-linked microspheres, thereby improving the fixation and stability of the cross-linked microspheres, avoiding a significant increase in the release force or a significant decrease in the residual bonding rate after high-temperature aging, thereby improving the durability and transparency of the prepared non-silicon release film. In addition, the presence of N-vinyl pyrrolidone can also improve the bonding strength between the coating material and the substrate, thereby improving the release force of the non-silicon release film. In addition, the presence of the cross-linked microspheres can also play a role in heat dispersion, thereby increasing the drying speed of the coating material solution and avoiding cracking of the non-silicon release film during drying.

[0086] Unless otherwise specified, all percentages used in the present invention are by mass.

[0087] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a non-silicon release film, characterized in that: The method comprises the following steps: preparing a coating material solution, pre-treating, melt extruding, and shaping; The method for preparing the coating material solution comprises the following steps: preparing a viscosity reducing agent, preparing cross-linked microspheres, and mixing; The method for preparing the viscosity reducing agent comprises the following steps: preparing nano starch crystals and coating them; The method for preparing nano starch crystals comprises mixing corn starch and deionized water, heating to boiling, maintaining boiling, and then cooling to 10-12° C., adding anhydrous ethanol dropwise thereto, stirring after the addition is completed, standing, centrifuging, taking a precipitate, washing, and vacuum drying the precipitate to obtain nano starch crystals; The coating comprises mixing nano starch crystals, tannic acid and the first portion of deionized water, stirring at room temperature, dropping formaldehyde aqueous solution, continuing stirring after the dropping is completed, centrifuging, taking a precipitate, adding L-lysine, ethylenediamine and the second portion of deionized water to the precipitate, stirring at 70-75° C., centrifuging, taking a precipitate, washing and freeze-drying the precipitate to obtain a viscosity reducer; The preparation of cross-linked microspheres comprises mixing ethyl methacrylate, lauryl methacrylate, N-vinyl pyrrolidone, dipentaerythritol hexaacrylate, polyvinyl pyrrolidone, deionized water and ethylene glycol monomethyl ether, stirring at room temperature under the protection of nitrogen, adding azobisisobutyronitrile, stirring at 70-75° C., centrifuging, taking a precipitate, washing and freeze-drying the precipitate to obtain cross-linked microspheres; The mixing comprises mixing sodium methacrylic acid sulfonate and the first portion of deionized water, and then subjecting the mixture to high shear at room temperature under the protection of nitrogen; adding methyl methacrylate, methacrylic acid, butyl acrylate, and hydroxyethyl methacrylate, and then subjecting the mixture to high shear at 70-75° C. under the protection of nitrogen; adding trimethylolpropane trimethacrylate, and then subjecting the mixture to high shear at 70-75° C.; adding potassium persulfate, and then subjecting the mixture to high shear at 70-75° C.; adding the second portion of deionized water, a viscosity reducer, cross-linked microspheres, and a water-soluble antistatic agent, and then subjecting the mixture to high shear at 70-75° C. to obtain a coating material solution; The melt extrusion is to divide the pretreated polyester chips into three parts as A layer raw material, B layer raw material and C layer raw material, respectively put them into the corresponding extruders, control the heating zone temperature of the main extruder and the auxiliary extruder to be 275-285° C. After melt extrusion, cool and solidify them on the surface of the casting roller to form casting sheets; The shaping process comprises preheating at 110-120° C., longitudinally stretching the cast sheet at 120-130° C. to obtain a base film; coating a coating material solution on one surface of the base film, controlling the coating thickness to be 4-5 μm, to obtain a coated base film; preheating at 110-120° C., transversely stretching the coated base film at 120-130° C., and then heat-setting to obtain a non-silicon release film.

2. The method for preparing a non-silicone release film according to claim 1, characterized in that: In the preparation of the nano starch crystals, the mass volume ratio of corn starch, deionized water and anhydrous ethanol is 2000-2400 g: 20-24 L: 20-26 L; The dropping speed of the anhydrous ethanol is 90-100 mL / min.

3. The method for preparing a non-silicone release film according to claim 1, characterized in that: In the coating, the mass volume ratio of the nano starch crystal, tannic acid, the first portion of deionized water, the formaldehyde aqueous solution, L-lysine, ethylenediamine, and the second portion of deionized water is 400-460 g: 600-700 g: 70-80 L: 100-120 mL: 50-60 g: 40-50 g: 60-70 L; The concentration of the formaldehyde aqueous solution is 37wt%; The dropping speed of the formaldehyde aqueous solution is 20-30 mL / min.

4. The method for preparing a non-silicone release film according to claim 1, characterized in that: In the preparation of the cross-linked microspheres, the mass volume ratio of ethyl methacrylate, dodecyl methacrylate, N-vinyl pyrrolidone, dipentaerythritol hexaacrylate, polyvinyl pyrrolidone, deionized water, ethylene glycol monomethyl ether, and azobisisobutyronitrile is 1000-1200g:360-400g:600-800g:120-140g:120-140g:26-28L:4-6L:24-26g.

5. The method for preparing a non-silicone release film according to claim 1, characterized in that: In the mixture, the mass volume ratio of sodium methacrylate sulfonate, the first portion of deionized water, methyl methacrylate, methacrylic acid, butyl acrylate, hydroxyethyl methacrylate, trimethylolpropane trimethacrylate, potassium persulfate, the second portion of deionized water, viscosity reducer, crosslinked microspheres, and water-soluble antistatic agent is 520-560g:36-38L:6000-6800g:3200-4000g:1120-1280g:680-800g:400-440g:200-240g:20-20.8L:960-1080g:1400-1600g:600-640g.

6. The method for preparing a non-silicone release film according to claim 1, characterized in that: The pretreatment uses hot air at 130-135° C. to pre-crystallize the polyester chips, and then dries them at 155-160° C. and 145-150° C. to obtain the pretreated polyester chips.

7. The method for preparing a non-silicone release film according to claim 1, characterized in that: In the melt extrusion, the mass ratio of the A layer raw material, the B layer raw material, and the C layer raw material is 12-15:65-70:12-15.

8. The method for preparing a non-silicone release film according to claim 1, characterized in that: In the shaping, the ratio of longitudinal stretching is 3.5-4; the ratio of transverse stretching is 4-4.2; The temperature of the heat setting is 230-240° C., and the time is 3-5 seconds.

9. A non-silicon release film prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Nanometer starch microsphere hydrocarbon reservoir protective agent and preparation method thereof

    CN113122211A

  • High-temperature-resistant non-silicon release material, non-silicon release film and preparation method and application thereof