Core-shell type polyester copolymerized acrylic acid water-based adhesive as well as preparation method and application thereof
By using core-shell polyester copolymer acrylic water-based adhesive in the negative electrode sheet of lithium ion battery, the problems of low adhesion, poor flexibility and poor swelling property of existing adhesives are solved, and high-performance bonding effect is achieved. .
Patent Information
- Application Number
- CN202310400119.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
AI Technical Summary
Existing adhesives for lithium-ion battery negative electrodes have low adhesion, poor flexibility, and poor swelling properties, and cannot meet high performance requirements.
A core-shell type polyester copolymerized acrylic water-based adhesive is used. By selecting basic monomers, functional monomers and cross-linking monomers, and introducing polyester segments, a core-shell type with high adhesion, flexibility and low swelling is prepared. Polyester copolymer acrylic water-based adhesive used in lithium-ion battery negative electrode plates.
It improves the adhesion and flexibility of the negative electrode sheet of lithium-ion batteries, reduces swelling, and meets the comprehensive demand for high-performance adhesives.
Smart Images

Figure BDA0004179150600000231
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water-based adhesives, and in particular relates to a core-shell polyester copolymer acrylic acid water-based adhesive and a preparation method and application thereof. Background Art
[0002] As a secondary battery, lithium-ion batteries are widely used in many fields due to their advantages such as high energy conversion rate, high energy density, high rate charge and discharge, no memory effect and environmental friendliness. Polymer adhesives have good bonding properties and can bond various particles together and tightly bond them to the current collector, making them an indispensable part of lithium-ion batteries. In addition to high adhesion, high-performance adhesives also need to have the following characteristics: good flexibility, electrolyte resistance, compactness, chemical and electrochemical stability, low cost and environmental protection.
[0003] At present, the adhesives used in lithium-ion batteries in the industry are mainly divided into three categories: polyvinylidene fluoride (PVDF), styrene-butadiene rubber latex and carboxymethyl cellulose (SBR / CMC), and polyacrylic acid (PAA). PVDF has the advantages of good adhesion to aluminum foil and strong resistance to electrochemical corrosion, but its adhesion to copper foil is poor, and PVDF has a large molecular weight and no hydrophilic groups. It is commonly dispersed and dissolved with N-methylpyrrolidone (NMP), but NMP solvent is sensitive to moisture, toxic, and volatilizes to pollute the environment; SBR / CMC adhesive has poor process performance and harsh conditions, and is greatly affected by factors such as stirring, pH, and electrode material ratio. At the same time, the prices of both PVDF and SBR / CMC are relatively high. PAA adhesive has the advantages of strong adhesion, good stability, low price, and environmental protection, and is now a hot research topic for negative electrode adhesives. However, ordinary PAA adhesives cannot meet the comprehensive requirements for negative electrode sheets.
[0004] Therefore, in the art, the PAA adhesive needs to be modified to simultaneously meet the requirements for adhesion, swelling rate and electrochemical performance. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a core-shell polyester copolymer acrylic acid aqueous adhesive and its preparation method and application. The core-shell polyester copolymer acrylic acid aqueous adhesive of the present invention has high bonding force, good flexibility and low swelling, and can be used in the negative electrode of lithium ion batteries.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] On the one hand, the present invention provides a core-shell polyester copolymer acrylic acid aqueous adhesive, wherein the core-shell polyester copolymer acrylic acid aqueous adhesive is a polymer having a core-shell structure obtained by polymerizing monomers, wherein the polymerizing monomers include a basic monomer, a first functional monomer, a second functional monomer and a cross-linking monomer;
[0008] The basic monomer is selected from the group consisting of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, isopropyl methacrylate, butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, n-octyl acrylate, isooctyl acrylate, lauric acrylate, 2-ethylhexyl acrylate, hexyl methacrylate or vinyl acetate, or a combination of at least two of them; the first functional monomer is selected from the group consisting of polyester monomers, hydroxy acrylate-polycaprolactone copolymers or hydroxy methacrylate-polycaprolactone copolymers, or a combination of at least two of them; the second functional monomer is selected from the group consisting of polyester monomers, hydroxy acrylate-polycaprolactone copolymers or hydroxy methacrylate-polycaprolactone copolymers, or a combination of at least two of them; The monomer is selected from any one of acrylic acid, methacrylic acid, acrylonitrile, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, hydroxypropyl methacrylate or 4-hydroxybutyl acrylate, or a combination of at least two thereof; the crosslinking monomer is selected from any one of acrylamide, allyl methacrylate, ethylene glycol acetoacetate methacrylate, diacetone acrylamide, N-hydroxymethyl acrylamide, divinylbenzene, aziridine, glycidyl methacrylate, ethoxylated trimethylolpropane triacrylate, polyethylene glycol diacrylate or a silane coupling agent, or a combination of at least two thereof;
[0009] The monomers for preparing the polyester monomer include polycarbonate diol, isophorone diisocyanate and hydroxy acrylic acid.
[0010] In the present invention, the self-made polyester monomer is prepared by the following preparation method:
[0011] (I) mixing polyester polyol and diisocyanate, heating, adding a catalyst, and reacting;
[0012] (II) adding a hydroxyl-containing acrylic acid ester monomer to the reaction solution of step (I) to react and obtain the polyester monomer;
[0013] Preferably, the mixing in step (I) is carried out under stirring;
[0014] Preferably, the stirring speed is 100-400r / min, for example 100r / min, 130r / min, 150r / min, 180r / min, 200r / min, 250r / min, 280r / min, 300r / min, 350r / min, 380r / min or 400r / min, preferably 200-350r / min.
[0015] Preferably, the polyester polyol in step (I) is a polycarbonate polyol, preferably any one of an aliphatic polycarbonate diol, an aromatic polycarbonate diol or a mixed aliphatic and aromatic polycarbonate diol, or a combination of at least two thereof.
[0016] Preferably, the diisocyanate in step (I) is any one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, methane diisocyanate, hexamethylene diisocyanate or lysine diisocyanate, or a combination of at least two thereof.
[0017] Preferably, the hydroxyl-containing acrylic ester monomer in step (I) is any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, β-hydroxypropyl acrylate, β-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate or 4-hydroxybutyl methacrylate, or a combination of at least two thereof.
[0018] Preferably, the molar ratio of hydroxyl group in the polyester polyol to isocyanate group in the diisocyanate in step (I) is 0.6-0.91:1, for example 0.6:1, 0.65:1, 0.7:1, 0.75:1, 0.8:1, 0.85:1 or 0.91:1.
[0019] Preferably, the heating in step (I) is to 45-90°C, such as 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, preferably 50-85°C.
[0020] Preferably, the catalyst in step (I) is an organotin catalyst, preferably dibutyltin dilaurate and / or stannous octoate.
[0021] Preferably, the reaction time in step (I) is 2-6 h, such as 2 h, 3 h, 4 h, 5 h or 6 h, preferably 2-4.5 h.
[0022] Preferably, the molar ratio of the hydroxy acrylic acid in step (II) to the isophorone diisocyanate in step (I) is 1:0.55-0.8, for example, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75 or 1:0.8.
[0023] Preferably, the reaction temperature in step (II) is 75-90°C, such as 75°C, 78°C, 80°C, 83°C, 85°C, 88°C or 90°C, preferably 78-85°C.
[0024] Preferably, the reaction time of step (II) is 2-6 h, such as 2 h, 3 h, 4 h, 5 h or 6 h, preferably 2-4.5 h.
[0025] In the present invention, by selecting basic monomers, first functional monomers, second functional monomers and cross-linking monomers, polyester segments are introduced during the monomer polymerization process to obtain a core-shell polyester copolymer acrylic acid aqueous adhesive with high adhesion, good flexibility and low swelling, which can be used in lithium-ion battery negative electrode plates.
[0026] Preferably, the polymerized monomers of the core include the following components in parts by weight: 12.25-80 parts (e.g., 12.25, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75 or 80 parts) of basic monomers, 0.25-30 parts (e.g., 0.25, 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of second functional monomers and 0.25-15 parts (e.g., 0.25, 0.3, 0.5, 1, 3, 5, 8, 10 or 15 parts) of cross-linking monomers.
[0027] Preferably, the polymerized monomers of the shell include the following components in percentage by weight: 10-80 parts (e.g., 10 parts, 13 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts or 80 parts) of the basic monomer, 0.2-25 parts (e.g., 0.25 parts, 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts) of the basic monomer, The invention also comprises the following steps: the first functional monomer comprises 0.2-30 parts (e.g., 0.25 parts, 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts, or 30 parts) of a first functional monomer, and 0.1-15 parts (e.g., 0.1 parts, 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, or 15 parts) of a cross-linking monomer.
[0028] In the present invention, by controlling the composition ratio of the core and shell polymer monomers, a core-shell type polyester copolymer acrylic acid aqueous adhesive that is hard inside and soft outside can be obtained. By introducing carboxylate and ester groups into the adhesive, a core-shell type polyester copolymer acrylic acid aqueous adhesive with flexibility, low swelling and good adhesion is obtained, so that the adhesive can be better applied to the negative electrode of lithium-ion batteries.
[0029] Preferably, the core-shell polyester copolymer acrylic acid aqueous adhesive is obtained by emulsion polymerization.
[0030] On the other hand, the present invention provides a method for preparing the core-shell polyester copolymer acrylic acid aqueous adhesive as described above, the preparation method comprising the following steps:
[0031] (1) preparing a core pre-emulsified liquid, a core pre-emulsified seed emulsion, a shell pre-emulsified liquid, a kettle bottom reaction liquid and an initiator solution;
[0032] (2) adding the pre-emulsified seed emulsion to the reaction liquid at the bottom of the kettle, heating it, adding the initiator solution, and reacting;
[0033] (3) adding the core pre-emulsion and the initiator solution to the reaction solution obtained in step (2) to react;
[0034] (4) adding the shell pre-emulsion and the initiator solution to the reaction solution obtained in step (3), reacting to obtain the core-shell polyester copolymer acrylic acid aqueous adhesive.
[0035] In the present invention, seed emulsion polymerization is used to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0036] Preferably, the seed emulsion polymerization of the present invention can increase the compatibility and adhesion of the obtained shell structure particles, and can also improve the mechanical properties; the latex particles obtained by the addition sequence and conditions of the present invention are stronger than ordinary emulsion polymerization in terms of rheology, minimum film forming temperature, glass transition temperature, adhesion, processability, etc. The seed emulsion polymerization can effectively control the diameter and distribution of the latex particles. Directly adding the core pre-emulsion liquid and the initiator to react will make the obtained latex particle size very small, which is not conducive to its adhesion, processing and mechanical properties.
[0037] Preferably, the core pre-emulsion comprises basic monomers, second functional monomers, cross-linking monomers, emulsifiers and deionized water.
[0038] Preferably, the core pre-emulsion comprises 12.25-65 parts (e.g., 12.25 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts or 65 parts) of basic monomers, 0.245-25 parts (e.g., 0.25 parts, 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts or 25 parts) of second functional monomers and 0.25-15 parts (e.g., 0.25 parts, 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts or 15 parts) of cross-linking monomers.
[0039] Preferably, the amount of emulsifier in the core pre-emulsion is 0.25%-4% of the total weight of the basic monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion, for example 0.25%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%.
[0040] Preferably, the amount of deionized water in the core pre-emulsion is 10% to 80% of the total weight of the basic monomers, second functional monomers and cross-linking monomers in the core pre-emulsion, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.
[0041] Preferably, the core pre-emulsified seed emulsion comprises a basic monomer, a second functional monomer, an emulsifier and deionized water.
[0042] Preferably, the core pre-emulsified seed emulsion contains 0.25-30 parts (e.g., 0.25, 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of basic monomer and 0.005-25 parts (e.g., 0.005, 0.01, 0.1, 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20 or 25 parts) of second functional monomer.
[0043] Preferably, the amount of emulsifier in the core pre-emulsified seed emulsion is 0.005%-4% of the total weight of the basic monomers and the second functional monomers in the seed emulsion of the core pre-emulsified liquid, for example 0.005%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%.
[0044] Preferably, the amount of deionized water in the core pre-emulsified seed emulsion is 10% to 80% of the total weight of the basic monomers and the second functional monomers in the seed emulsion of the core pre-emulsified solution, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.
[0045] Preferably, the shell pre-emulsion comprises basic monomers, first functional monomers, second functional monomers, cross-linking monomers, emulsifiers and deionized water.
[0046] Preferably, the shell pre-emulsion comprises 10-80 parts (e.g., 10 parts, 13 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts or 80 parts) of basic monomers, 0.2-25 parts (e.g., 0.25 parts, 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 1 part, 15 parts, 20 parts or 25 parts) of a first functional monomer, 0.2-30 parts (e.g., 0.25 parts, 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts, 20 parts, 25 parts or 30 parts) of a second functional monomer and 0.1-15 parts (e.g., 0.1 parts, 0.3 parts, 0.5 parts, 1 part, 3 parts, 5 parts, 8 parts, 10 parts or 15 parts) of a cross-linking monomer.
[0047] Preferably, the amount of emulsifier in the shell pre-emulsion is 0.2%-4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion, for example 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%.
[0048] Preferably, the amount of deionized water in the shell pre-emulsion is 10% to 80% of the total weight of the basic monomers, the first functional monomers, the second functional monomers and the cross-linking monomers in the core pre-emulsion, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.
[0049] Preferably, the reaction liquid at the bottom of the kettle comprises an emulsifier, deionized water and a buffer.
[0050] Preferably, the content of each component in the reaction liquid at the bottom of the kettle is 0.1-3 parts (for example, 0.3 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts or 3 parts) of emulsifier, 50-120 parts (for example, 50 parts, 60 parts, 70 parts, 75 parts, 80 parts, 90 parts, 100 parts, 110 parts or 120 parts) of deionized water, and 0.25-1 parts (for example, 0.25 parts, 0.3 parts, 0.5 parts, 0.7 parts or 1 parts) of buffer.
[0051] Preferably, the emulsifiers in the core pre-emulsified liquid, the core pre-emulsified seed emulsion, the shell pre-emulsified liquid and the bottom reaction liquid are independently selected from any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene octylphenol ether-10, allyloxy fatty alcohol oxyethylene ether ammonium sulfate or disodium succinic acid nonylphenol polyoxyethylene ether monoester sulfonate or a combination of at least two thereof.
[0052] Preferably, the buffer is any one of sodium bicarbonate, sodium dihydrogen phosphate, aqueous ammonia, ammonium bicarbonate or sodium hydroxide, or a combination of at least two thereof.
[0053] Preferably, the initiator solution comprises an initiator and deionized water.
[0054] Preferably, the amount of deionized water in the initiator solution is 1-20 parts, for example, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 13 parts, 15 parts, 18 parts or 20 parts, relative to 1 part by weight of the initiator.
[0055] Preferably, the initiator is selected from inorganic peroxide initiators.
[0056] Preferably, the initiator is selected from any one of potassium persulfate, ammonium persulfate or sodium persulfate, or a combination of at least two thereof.
[0057] Preferably, the reaction in steps (2) to (4) is carried out under stirring, and the stirring speed is 100-500 r / min (for example, 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min, 500 r / min).
[0058] Preferably, before adding the pre-emulsified seed emulsion in step (2), the reaction liquid at the bottom of the kettle is added to a reactor at 40-80°C (e.g., 40°C, 45°C, 48°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C).
[0059] Preferably, the heating in step (2) is to 75-85°C, for example, 75°C, 78°C, 80°C, 83°C or 85°C.
[0060] Preferably, the mass of the reaction liquid at the bottom of the kettle in step (2) is 1-100 times, for example, 3 times, 5 times, 8 times, 10 times, 20 times, 30 times, 40 times, 45 times, 50 times, 60 times, 70 times, 80 times, 90 times or 100 times, of the pre-emulsified seed emulsion.
[0061] Preferably, the amount of the initiator solution added in step (2) is 0.06%-25% by weight of the core pre-emulsified seed emulsion, for example 0.06%, 0.8%, 1%, 2%, 4%, 6%, 8%, 10%, 13%, 15%, 18%, 20%, 23% or 25%.
[0062] Preferably, the reaction time of step (2) is 10-30 min, for example, 10 min, 13 min, 15 min, 18 min, 20 min, 23 min, 25 min, 28 min or 30 min.
[0063] Preferably, the weight ratio of the core pre-emulsion in step (3) to the bottom reaction liquid in step (2) is 1:0.15-1, for example, 1:0.15, 1:0.3, 1:0.5, 1:0.7, 1:0.8 or 1:1.
[0064] Preferably, the amount of the initiator solution added in step (3) is 0.0045%-25% by weight of the core pre-emulsion, for example 0.0045%, 0.2%, 0.5%, 1%, 3%, 5%, 8%, 10%, 13%, 15%, 18%, 20%, 23% or 25%.
[0065] Preferably, the reaction temperature in step (3) is 75-85°C, such as 75°C, 78°C, 80°C, 83°C or 85°C.
[0066] Preferably, the reaction time of step (3) is 10-30 min, for example, 10 min, 13 min, 15 min, 18 min, 20 min, 23 min, 25 min, 28 min or 30 min.
[0067] Preferably, the weight ratio of the core pre-emulsion in step (3) to the shell pre-emulsion in step (4) is 1:0.25-3, for example, 1:0.25, 1:0.3, 1:0.5, 1:0.8, 1:1, 1:1.5, 1:1.8, 1:2, 1:2.5, 1:2.8 or 1:3.
[0068] Preferably, the amount of the initiator solution added in step (4) is 0.006%-15% by weight of the shell pre-emulsion, for example 0.006%, 0.1%, 0.5%, 1%, 3%, 5%, 8%, 10%, 13% or 15%.
[0069] Preferably, the reaction temperature in step (4) is 80-90°C, such as 80°C, 83°C, 85°C, 88°C or 90°C.
[0070] Preferably, the reaction time of step (4) is 0.5-2.5 h, for example 0.5 h, 0.8 h, 1 h, 1.5 h, 1.8 h, 2 h, 2.3 h or 2.5 h.
[0071] In the present invention, after the reaction in step (4) is completed, the temperature is lowered to 60-70°C (for example, 60°C, 63°C, 65°C, 68°C or 70°C), a residual monomer eliminator is added, and then the temperature is lowered to below 50°C (for example, 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, 20°C, 10°C, etc.), the pH is adjusted to 7-9 (for example, 7, 7.3, 7.5, 7.8, 8, 8.4, 8.8 or 9), and the material is filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0072] Preferably, the residual monomer eliminating agent is bleaching powder and tert-butyl peroxide.
[0073] Preferably, the reagent used to adjust the pH is any one of ammonia water, sodium hydroxide, lithium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two thereof.
[0074] In the present invention, by designing the monomer types and mass ratios in the core and shell pre-emulsions, a core-shell type polyester copolymer acrylic acid aqueous adhesive with a hard inner side and a soft outer side is prepared. By introducing carboxylate and ester groups into the adhesive, the prepared core-shell type polyester copolymer acrylic acid aqueous adhesive has flexibility, low swelling and good adhesion, so that the adhesive can be better applied to the negative electrode plates of lithium-ion batteries.
[0075] On the other hand, the present invention provides a negative electrode plate for a lithium ion battery, wherein the negative electrode plate for the lithium ion battery comprises the core-shell polyester copolymer acrylic acid aqueous adhesive as described above.
[0076] In another aspect, the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the lithium ion battery negative electrode sheet as described above.
[0077] Compared with the prior art, the present invention has the following beneficial effects:
[0078] The core-shell polyester copolymer acrylic acid aqueous adhesive provided by the present invention has high bonding force, good flexibility and low swelling, solves the problems of low bonding, poor flexibility and high swelling in the current adhesives used for negative electrodes of lithium ion batteries, and has good application prospects in negative electrode plates of lithium ion batteries. DETAILED DESCRIPTION
[0079] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0080] Preparation Example 1
[0081] (I) 120 g of polycarbonate diol (PH-50, Green Union (Jining) Chemical Technology Co., Ltd.) and 107 g of isophorone diisocyanate were mixed at a speed of 500 r / min, the temperature was raised to 70° C., 0.05 g of dibutylene dilaurate catalyst was added, and the reaction was carried out for 3.5 h;
[0082] (II) Add 56 g of hydroxyethyl acrylate to the reaction solution of step (I), and react at 80° C. for 2.5 h to obtain a polyester monomer.
[0083] Preparation Example 2
[0084] (I) 36 g of polycarbonate diol (Green Union (Jining) Chemical Technology Co., Ltd., PH-50) and 32.1 g of toluene diisocyanate were mixed at a speed of 400 r / min, heated to 85° C., 0.015 g of stannous octoate was added, and the reaction was carried out for 2 h;
[0085] (II) Add 16.8 g of hydroxypropyl methacrylate to the reaction solution of step (I), and react at 85° C. for 5 h to obtain a polyester monomer.
[0086] Preparation Example 3
[0087] (I) 180 g of polycarbonate diol (Green Union (Jining) Chemical Technology Co., Ltd., PH-50) and 160.5 g of diphenylmethane diisocyanate were mixed at a speed of 400 r / min, the temperature was raised to 50° C., 0.075 g of dibutylene dilaurate was added, and the reaction was carried out for 6 h;
[0088] (II) Add 84 g of 4-hydroxybutyl acrylate to the reaction solution of step (I), and react at 78° C. for 2 h to obtain a polyester monomer.
[0089] Example 1
[0090] In this embodiment, a method for preparing a core-shell polyester copolymer acrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0091] Core pre-emulsion: 0.98 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.82 parts of polyoxyethylene octylphenol ether-10 are dissolved in 27.6 parts of deionized water, and then 30.59 parts of methyl methacrylate, 24.84 parts of butyl acrylate, 3.91 parts of lauric acid acrylate, 0.92 parts of acrylonitrile, 0.92 parts of acrylamide, 0.69 parts of acrylic acid, 0.23 parts of methacrylic acid, and 0.92 parts of hydroxyethyl methacrylate are added in sequence for emulsification, and then 0.92 parts of ethoxylated trimethylolpropane triacrylate are added for uniform emulsification to obtain a core pre-emulsion;
[0092] Seed emulsion: dissolve 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.07 parts of polyoxyethylene octylphenol ether-10 in 2.4 parts of deionized water, and then sequentially add 2.66 parts of methyl methacrylate, 2.16 parts of butyl acrylate, 0.34 parts of lauric acid acrylate, 0.08 parts of acrylonitrile, 0.08 parts of acrylamide, 0.06 parts of acrylic acid, 0.02 parts of methacrylic acid, and 0.08 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0093] Shell pre-emulsion: 1.06 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 are dissolved in 50 parts of deionized water, and then 40.5 parts of methyl methacrylate, 20 parts of butyl acrylate, 15 parts of lauric acid acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 0.75 parts of acrylic acid, 0.25 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate and 2 parts of glycidyl methacrylate dissolved with 0.5 parts of polyester monomer are added in sequence for emulsification to obtain a shell pre-emulsion;
[0094] Still bottom reaction liquid: dissolve 0.54 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, and then add 0.5 parts of sodium bicarbonate to obtain a still bottom reaction liquid;
[0095] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.
[0096] 61.58 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 150rpm. 8.03 parts of the seed emulsion were added to the reactor, heated to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 93.34 parts of the core pre-emulsion and 1.9 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 15 minutes, 133.95 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, it was kept at 87°C for 1h, and after the insulation was completed, it was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and then it was cooled to 40°C, and the pH was adjusted to 7.33 with 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0097] Example 2
[0098] In this embodiment, a method for preparing a core-shell polyester copolymer acrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0099] Core pre-emulsion: 0.98 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.82 parts of polyoxyethylene octylphenol ether-10 are dissolved in 27.6 parts of deionized water, and then 30.59 parts of methyl methacrylate, 24.84 parts of butyl acrylate, 3.91 parts of lauric acid acrylate, 0.92 parts of acrylonitrile, 0.92 parts of acrylamide, 0.69 parts of acrylic acid, 0.23 parts of methacrylic acid, and 0.92 parts of hydroxyethyl methacrylate are added in sequence for emulsification, and then 0.92 parts of ethoxylated trimethylolpropane triacrylate are added for uniform emulsification to obtain a core pre-emulsion;
[0100] Seed emulsion: dissolve 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.07 parts of polyoxyethylene octylphenol ether-10 in 2.4 parts of deionized water, and then sequentially add 2.66 parts of methyl methacrylate, 2.16 parts of butyl acrylate, 0.34 parts of lauric acid acrylate, 0.08 parts of acrylonitrile, 0.08 parts of acrylamide, 0.06 parts of acrylic acid, 0.02 parts of methacrylic acid, and 0.08 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0101] Shell pre-emulsion: 1.06 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 are dissolved in 50 parts of deionized water, and then 40.5 parts of ethyl methacrylate dissolved with 1 part of polyester monomer, 20 parts of butyl acrylate, 15 parts of lauric acid acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 0.75 parts of acrylic acid, 0.25 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate are added in sequence for emulsification to obtain a shell pre-emulsion;
[0102] Still bottom reaction liquid: dissolve 0.54 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, and then add 0.5 parts of sodium bicarbonate to obtain a still bottom reaction liquid;
[0103] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.
[0104] 61.58 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 200rpm. 8.03 parts of the seed emulsion were added to the reactor, heated to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 93.34 parts of the core pre-emulsion and 1.9 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 15 minutes, 134.45 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, it was kept at 87°C for 1h, and after the insulation was completed, it was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and then it was cooled to 40°C, and the pH was adjusted to 7.33 with 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0105] Example 3
[0106] In this embodiment, a method for preparing a core-shell polyester copolymer acrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0107] Core pre-emulsion: 2 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 1 part of polyoxyethylene octylphenol ether-10 are dissolved in 30 parts of deionized water, and then 25 parts of styrene, 18 parts of isobutyl methacrylate, 10 parts of lauric acid acrylate, 8 parts of acrylonitrile, 2 parts of acrylamide, 4 parts of acrylic acid, 2 parts of methacrylic acid, and 4 parts of hydroxypropyl methacrylate are added in sequence for emulsification, and then 6 parts of divinylbenzene are added for uniform emulsification to obtain a core pre-emulsion;
[0108] Seed emulsion: dissolve 0.4 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 0.2 parts of polyoxyethylene octylphenol ether-10 in 6 parts of deionized water, and then add 5 parts of styrene, 3.6 parts of isobutyl methacrylate, 2 parts of lauric acid acrylate, 1.6 parts of acrylonitrile, 0.4 parts of acrylamide, 0.8 parts of acrylic acid, 0.4 parts of methacrylic acid, and 0.8 parts of hydroxypropyl methacrylate in sequence for emulsification to obtain a seed emulsion;
[0109] Shell pre-emulsion: 2 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 1 part of polyoxyethylene octylphenol ether-10 are dissolved in 40 parts of deionized water, and then 15 parts of styrene, 35 parts of isobutyl methacrylate, 15 parts of lauric acid acrylate, 5 parts of hydroxyethyl acrylate-polycaprolactone (Hunan Juren Chemical New Material Technology Co., Ltd., PCL-HA2), 8 parts of acrylonitrile, 2 parts of acrylamide, 7 parts of acrylic acid, 4 parts of methacrylic acid, 4 parts of hydroxypropyl methacrylate, 5 parts of diacetone acrylamide, and parts are added in sequence for emulsification to obtain a shell pre-emulsion;
[0110] Still bottom reaction liquid: dissolve 1 part of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 1 part of polyoxyethylene octylphenol ether-10 in 100 parts of deionized water, and then add 1 part of ammonia water to obtain a still bottom reaction liquid;
[0111] Initiator solution: Add 0.6 parts of ammonium persulfate into 13 parts of deionized water to obtain an initiator aqueous solution.
[0112] 103 parts of the bottom reaction liquid were added to a reactor at 65°C, with a rotation speed of 250rpm. 21.2 parts of the seed emulsion were added to the reactor, heated to 78°C, 1.23 parts of the initiator solution were added, and after reacting for 20 minutes, 112 parts of the core pre-emulsion and 6.15 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 18 minutes, 143 parts of the shell pre-emulsion and 8.21 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 85°C for 1.8 hours. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 35°C. The pH was adjusted to 7.68 with sodium hydroxide, and the material was filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0113] Example 4
[0114] In this embodiment, a method for preparing a core-shell polyester copolymer acrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0115] Nuclear pre-emulsion: 2 parts of sodium dodecylbenzene sulfonate and 2 parts of polyoxyethylene octylphenol ether-10 are dissolved in 30 parts of deionized water, and then 13 parts of styrene, 17 parts of methyl methacrylate, 15 parts of butyl acrylate, 13 parts of lauric acid methacrylate, 5 parts of acrylamide, 8 parts of acrylic acid, 4 parts of methacrylic acid, and 4 parts of hydroxypropyl methacrylate are added in sequence for emulsification, and then 6 parts of ethoxylated trimethylolpropane triacrylate are added for uniform emulsification to obtain a nuclear pre-emulsion;
[0116] Seed emulsion: 0.4 parts of sodium dodecylbenzene sulfonate and 0.4 parts of polyoxyethylene octylphenol ether-10 were dissolved in 7.5 parts of deionized water, and then 3.25 parts of styrene, 4.25 parts of methyl methacrylate, 3.75 parts of butyl acrylate, 3.25 parts of lauric acid methacrylate, 1.25 parts of acrylamide, 2 parts of acrylic acid, 1 part of methacrylic acid, and 1 part of hydroxypropyl methacrylate were added in sequence for emulsification to obtain a seed emulsion;
[0117] Shell pre-emulsion: 2 parts of sodium dodecylbenzene sulfonate and 2 parts of polyoxyethylene octylphenol ether-10 are dissolved in 40 parts of deionized water, and then 10 parts of styrene, 15 parts of methyl methacrylate, 30 parts of butyl acrylate, 20 parts of lauric acid methacrylate, 6.5 parts of hydroxyethyl methacrylate-polycaprolactone (Hunan Juren Chemical New Material Technology Co., Ltd., PCL-HAM2), 5 parts of acrylamide, 8 parts of acrylic acid, 4 parts of methacrylic acid, 4 parts of hydroxypropyl methacrylate, 1 part of silane coupling agent, and 5 parts of polyethylene glycol diacrylate are added in sequence for emulsification to obtain a shell pre-emulsion;
[0118] Still bottom reaction liquid: 1.5 parts of sodium dodecylbenzene sulfonate and 1.5 parts of polyoxyethylene octylphenol ether-10 are dissolved in 120 parts of deionized water, and then 0.25 parts of sodium hydroxide are added to obtain a still bottom reaction liquid;
[0119] Initiator solution: Add 0.6 parts of ammonium persulfate into 15 parts of deionized water to obtain an initiator aqueous solution.
[0120] 123.25 parts of the bottom reaction liquid were added to a reactor at 75°C, with a rotation speed of 250rpm. 28.05 parts of the seed emulsion were added to the reactor, heated to 83°C, 1.4 parts of the initiator solution were added, and after reacting for 25 minutes, 119 parts of the core pre-emulsion and 12 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 23 minutes, 152.5 parts of the shell pre-emulsion and 2.2 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 88°C for 0.5h. After the reaction was completed, the temperature was lowered to 60°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 10°C. The pH was adjusted to 7.68 using lithium hydroxide, and the material was filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0121] Example 5
[0122] In this embodiment, a method for preparing a core-shell polyester copolymer acrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0123] Core pre-emulsion: 3 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate were dissolved in 25 parts of deionized water, followed by the addition of 28 parts of styrene, 18 parts of butyl acrylate, 3 parts of isooctyl acrylate, 5 parts of acrylamide, 2 parts of methacrylic acid, and 10 parts of hydroxyethyl methacrylate in order for emulsification, and then 3 parts of N-hydroxymethyl acrylamide were added for uniform emulsification to obtain a core pre-emulsion;
[0124] Seed emulsion: dissolve 0.45 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 4 parts of deionized water, and then sequentially add 4.2 parts of styrene, 2.7 parts of butyl acrylate, 0.45 parts of isooctyl acrylate, 0.75 parts of acrylamide, 0.3 parts of methacrylic acid, and 1.5 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0125] Shell pre-emulsion: dissolve 2.5 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 25 parts of deionized water, and then add 25 parts of styrene, 35 parts of butyl acrylate, 17 parts of isooctyl acrylate, 3 parts of hydroxyethyl acrylate-polycaprolactone (Hunan Juren Chemical New Material Technology Co., Ltd., PCL-HA2), 3 parts of hydroxyethyl methacrylate-polycaprolactone (Hunan Juren Chemical New Material Technology Co., Ltd., PCL-HAM2), 4 parts of acrylamide, 8 parts of methacrylic acid, and 3 parts of glycidyl methacrylate in sequence for emulsification to obtain a shell pre-emulsion;
[0126] Still bottom reaction liquid: dissolve 1 part of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate in 90 parts of deionized water, and then add 0.5 parts of sodium bicarbonate to obtain a still bottom reaction liquid;
[0127] Initiator solution: Add 0.6 parts of ammonium persulfate into 10 parts of deionized water to obtain an initiator aqueous solution.
[0128] 91.5 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 300rpm. 14.35 parts of the seed emulsion were added to the reactor, heated to 80°C, 0.742 parts of the initiator solution were added, and after reacting for 15 minutes, 97 parts of the core pre-emulsion and 6 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 125.5 parts of the shell pre-emulsion and 3.858 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 87°C for 1h. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 35°C. The pH was adjusted to 7.54 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0129] Example 6
[0130] In this embodiment, a method for preparing a core-shell polyester copolymer acrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0131] Core pre-emulsion: 2.5 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate are dissolved in 20 parts of deionized water, followed by the addition of 25 parts of methyl methacrylate, 14 parts of isooctyl acrylate, 5 parts of acrylamide, 4 parts of acrylic acid, and 8 parts of hydroxyethyl methacrylate in sequence for emulsification, and then 4 parts of ethoxylated trimethylolpropane triacrylate are added for uniform emulsification to obtain a core pre-emulsion;
[0132] Seed emulsion: dissolve 0.45 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 2.5 parts of deionized water, and then add 5 parts of methyl methacrylate, 2.8 parts of isooctyl acrylate, 1 part of acrylamide, 0.8 parts of acrylic acid, and 1.6 parts of hydroxyethyl methacrylate in sequence for emulsification to obtain a seed emulsion;
[0133] Shell pre-emulsion: 2.5 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate were dissolved in 30 parts of deionized water, and then 10 parts of styrene, 30 parts of lauric acid methacrylate, 5 parts of hydroxyethyl acrylate-polycaprolactone (Hunan Juren Chemical New Material Technology Co., Ltd., PCL-HA2), 4 parts of acrylonitrile, 8 parts of methacrylic acid, 2 parts of diacetone acrylamide, and 3 parts of allyl methacrylate were added in sequence for emulsification to obtain a shell pre-emulsion;
[0134] Still bottom reaction liquid: dissolve 1 part of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 70 parts of deionized water, and then add 1 part of ammonia water to obtain a still bottom reaction liquid;
[0135] Initiator solution: Add 0.6 parts of ammonium persulfate into 8 parts of deionized water to obtain an initiator aqueous solution.
[0136] 72 parts of the bottom reaction liquid were added to a reactor at 55°C, with a rotation speed of 350rpm. 14.15 parts of the seed emulsion were added to the reactor, heated to 82°C, 0.43 parts of the initiator solution were added, and after reacting for 15 minutes, 82.5 parts of the core pre-emulsion and 3 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 94.5 parts of the shell pre-emulsion and 5.17 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 86°C for 1.5 hours. After the reaction was completed, the temperature was lowered to 67°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 40°C. The pH was adjusted to 7.71 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0137] Example 7
[0138] In this embodiment, a method for preparing a core-shell polyester copolymer acrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0139] Core pre-emulsion: 2 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate were dissolved in 30 parts of deionized water, followed by the addition of 10 parts of methyl methacrylate, 18 parts of butyl acrylate, 10 parts of acrylonitrile, 5 parts of acrylic acid, and 6 parts of hydroxyethyl methacrylate in sequence for emulsification, and then 3 parts of ethoxylated trimethylolpropane triacrylate were added for uniform emulsification to obtain a core pre-emulsion;
[0140] Seed emulsion: dissolve 0.5 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 3 parts of deionized water, and then sequentially add 1 part of methyl methacrylate, 1.8 parts of butyl acrylate, 1 part of acrylonitrile, 0.5 parts of acrylic acid, and 0.6 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0141] Shell pre-emulsion: dissolve 2 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 35 parts of deionized water, and then add 10 parts of styrene, 30 parts of isooctyl acrylate, 3 parts of homemade polyester monomer, 4 parts of acrylamide, 8 parts of methacrylic acid, 4 parts of 4-hydroxybutyl acrylate, and 2 parts of ethylene glycol acetoacetate methacrylate in order to obtain a shell pre-emulsion;
[0142] Still bottom reaction liquid: dissolve 0.5 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate in 60 parts of deionized water, and then add 1 part of ammonia water to obtain a still bottom reaction liquid;
[0143] Initiator solution: Add 0.6 parts of ammonium persulfate into 9 parts of deionized water to obtain an initiator aqueous solution.
[0144] 61.5 parts of the bottom reaction liquid were added to a 50°C reactor at a speed of 150 rpm. 8.4 parts of the seed emulsion were added to the reactor, heated to 81°C, 0.5 parts of the initiator solution were added, and after reacting for 15 minutes, 126 parts of the core pre-emulsion and 4.5 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 98 parts of the shell pre-emulsion and 4.6 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 85°C for 1.2 hours. After the reaction was completed, the temperature was lowered to 67°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 30°C. The pH was adjusted to 7.71 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive.
[0145] Comparative Example 1
[0146] In this comparative example, unlike Example 1, the shell pre-emulsion does not include polyester monomers, and the shell pre-emulsion is prepared as follows: 1.06 parts of disodium succinic nonylphenol polyoxyethylene ether monoester sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 are dissolved in 50 parts of deionized water, and then 40.5 parts of ethyl methacrylate, 20 parts of butyl acrylate, 15 parts of lauric acid acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 0.75 parts of acrylic acid, 0.25 parts of methacrylic acid, and 1 part of hydroxyethyl methacrylate are added in sequence for emulsification to obtain the shell pre-emulsion. The rest is the same as Example 1.
[0147] Comparative Example 2
[0148] In this comparative example, unlike Example 1, a core-shell structure is not prepared, and the specific preparation method is as follows:
[0149] Pre-emulsion: 2.04 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 1.71 parts of polyoxyethylene octylphenol ether-10 were dissolved in 77.6 parts of deionized water, and then 71.09 parts of methyl methacrylate, 44.84 parts of butyl acrylate, 18.91 parts of lauric acid acrylate, 1.92 parts of propylene, 1.92 parts of acrylamide, 1.44 parts of acrylic acid, 0.48 parts of methacrylic acid, 1.92 parts of hydroxyethyl methacrylate, and 2 parts of glycidyl methacrylate were added in sequence for emulsification, and 0.92 parts of ethoxylated trimethylolpropane triacrylate was added to the core pre-emulsion for uniform emulsification;
[0150] Seed emulsion: dissolve 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.07 parts of polyoxyethylene octylphenol ether-10 in 2.4 parts of deionized water, and then sequentially add 2.66 parts of methyl methacrylate, 2.16 parts of butyl acrylate, 0.34 parts of lauric acid acrylate, 0.08 parts of acrylonitrile, 0.08 parts of acrylamide, 0.06 parts of acrylic acid, 0.02 parts of methacrylic acid, and 0.08 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0151] A bottom reaction liquid: 0.54 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.54 parts of polyoxyethylene octylphenol ether-10 are dissolved in 60 parts of deionized water, and then 0.5 parts of sodium bicarbonate are added to obtain a bottom reaction liquid;
[0152] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.
[0153] 61.58 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 150rpm. 8.03 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 1.65 parts of the initiator solution were added, and after the reaction for 15 minutes, 226.79 parts of the pre-emulsion and 3.85 parts of the initiator solution were added dropwise, and after the addition was completed, the reaction was kept at 87°C for 1 hour, and after the insulation was completed, the temperature was lowered to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and then the temperature was lowered to 40°C, and the pH was adjusted to 7.24 with 25% mass percentage concentration of ammonia water, and the material was filtered to obtain a polyester copolymer acrylic acid water-based adhesive.
[0154] Comparative Example 3
[0155] In this comparative example, a core-shell structured polyester copolymer acrylic acid aqueous adhesive with a soft inner side and a hard outer side was prepared. The specific preparation method is as follows:
[0156] Core pre-emulsion: 0.98 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.82 parts of polyoxyethylene octylphenol ether-10 are dissolved in 46 parts of deionized water, and then 37.26 parts of ethyl methacrylate, 18.4 parts of butyl acrylate, 13.8 parts of lauric acid acrylate, 0.92 parts of acrylonitrile, 0.92 parts of acrylamide, 0.69 parts of acrylic acid, 0.23 parts of methacrylic acid, 0.92 parts of hydroxyethyl methacrylate and 2 parts of glycidyl methacrylate dissolved with 0.46 parts of polyester monomer are added in sequence for emulsification to obtain a core pre-emulsion;
[0157] Seed emulsion: 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.07 parts of polyoxyethylene octylphenol ether-10 are dissolved in 4 parts of deionized water, and then 3.24 parts of methyl methacrylate, 1.6 parts of butyl acrylate, 1.2 parts of lauric acid acrylate, 0.08 parts of acrylonitrile, 0.08 parts of acrylamide, 0.06 parts of acrylic acid, 0.02 parts of methacrylic acid, and 0.08 parts of hydroxyethyl methacrylate dissolved in 0.04 parts of polyester monomer are added in sequence for emulsification to obtain a seed emulsion;
[0158] Shell pre-emulsion: 1.06 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.89 parts of polyoxyethylene octylphenol ether-10 are dissolved in 30 parts of deionized water, and then 33.25 parts of methyl methacrylate, 27 parts of butyl acrylate, 4.25 parts of lauric acid acrylate, 1 part of acrylonitrile, 1 part of acrylamide, 0.75 parts of acrylic acid, 0.25 parts of methacrylic acid, 1 part of hydroxyethyl methacrylate, and 0.92 parts of ethoxylated trimethylolpropane triacrylate are dissolved in sequence for emulsification to obtain a shell pre-emulsion;
[0159] Still bottom reaction liquid: dissolve 0.54 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.54 parts of polyoxyethylene octylphenol ether-10 in 60 parts of deionized water, and then add 0.5 parts of sodium bicarbonate to obtain a still bottom reaction liquid;
[0160] Initiator solution: Add 0.5 parts of ammonium persulfate to 5 parts of deionized water to obtain an initiator aqueous solution.
[0161] 61.58 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 150rpm. 10.55 parts of the seed emulsion were added to the reactor, heated to 80°C, 1.65 parts of the initiator solution were added, and after reacting for 20 minutes, 123.4 parts of the core pre-emulsion and 1.9 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 15 minutes, 101.37 parts of the shell pre-emulsion and 1.95 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, it was kept at 87°C for 1h, and after the insulation was completed, it was cooled to 65°C, 0.1 parts of bleaching powder and 0.096 parts of tert-butyl peroxide were added, and then it was cooled to 40°C, and the pH was adjusted to 7.33 with 25% mass percentage concentration of ammonia water, and the material was filtered to obtain a core-shell polyester copolymer acrylic acid water-based adhesive.
[0162] The adhesives obtained in the embodiments and comparative examples were subjected to performance tests, and the test methods were as follows:
[0163] (1) Take graphite slurry without adding adhesive, and then add the adhesives of the above embodiments and comparative examples in an amount of 2% of the solid component of the graphite slurry to the solid component of the adhesive, stir evenly, and obtain a mixed slurry. Take 8g of the mixed slurry, apply it evenly on the copper foil with a 200μm thick applicator, and then bake it in a 75℃ oven for 20min to obtain an electrode. Cut the electrode into 30mm wide strips, use 3M tape to stick the strips to the plywood, use a 2kg standard rolling wheel to roll the strips back and forth 3 times to compact them, and then stretch the strips at a stretching speed of 50mm / min to obtain the peel strength;
[0164] (2) After drying the water-based adhesive prepared in the above examples and comparative examples at 65° C. to form a film, 1.5 g of the film sample was cut and immersed in an electrolyte at 65° C. for 3 days. The swelling ratio was calculated by weighing, where the swelling ratio = (weight after swelling - weight before swelling) / weight before swelling × 100%;
[0165] The test results are shown in Table 1.
[0166] Table 1
[0167]
[0168]
[0169] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the core-shell polyester copolymer acrylic acid water-based adhesive and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A core-shell polyester copolymer acrylic acid water-based adhesive, characterized in that: The core-shell polyester copolymer acrylic acid aqueous adhesive is a polymer with a core-shell structure obtained by polymerizing monomers, and the polymerizing monomers include basic monomers, first functional monomers, second functional monomers and cross-linking monomers; The basic monomer is selected from the group consisting of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, isopropyl methacrylate, butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, n-octyl acrylate, isooctyl acrylate, lauric acrylate, 2-ethylhexyl acrylate, hexyl methacrylate or vinyl acetate, or a combination of at least two of them; the first functional monomer is selected from the group consisting of polyester monomers, hydroxy acrylate-polycaprolactone copolymers or hydroxy methacrylate-polycaprolactone copolymers, or a combination of at least two of them; the second functional monomer is selected from the group consisting of polyester monomers, hydroxy acrylate-polycaprolactone copolymers or hydroxy methacrylate-polycaprolactone copolymers, or a combination of at least two of them; The monomer is selected from any one of acrylic acid, methacrylic acid, acrylonitrile, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, hydroxypropyl methacrylate or 4-hydroxybutyl acrylate, or a combination of at least two thereof; the crosslinking monomer is selected from any one of acrylamide, allyl methacrylate, ethylene glycol acetoacetate methacrylate, diacetone acrylamide, N-hydroxymethyl acrylamide, divinylbenzene, aziridine, glycidyl methacrylate, ethoxylated trimethylolpropane triacrylate, polyethylene glycol diacrylate or a silane coupling agent, or a combination of at least two thereof; The monomers for preparing the polyester monomer include polycarbonate diol, isophorone diisocyanate and hydroxy acrylic acid.
2. The core-shell polyester copolymer acrylic acid aqueous adhesive according to claim 1, characterized in that: The polyester monomer is prepared by the following preparation method: (I) mixing polyester polyol and diisocyanate, heating, adding a catalyst, and reacting; (II) adding a hydroxyl-containing acrylic acid ester monomer to the reaction solution of step (I) to react and obtain the polyester monomer; Preferably, the mixing in step (I) is carried out under stirring; Preferably, the stirring speed is 100-400r / min, preferably 200-350r / min; Preferably, the polyester polyol in step (I) is a polycarbonate polyol, preferably any one or a combination of at least two of an aliphatic polycarbonate diol, an aromatic polycarbonate diol, or a mixed aliphatic and aromatic polycarbonate diol; Preferably, the diisocyanate in step (I) is any one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, methane diisocyanate, hexamethylene diisocyanate or lysine diisocyanate, or a combination of at least two thereof; Preferably, the hydroxyl-containing acrylic ester monomer in step (I) is any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, β-hydroxypropyl acrylate, β-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate or 4-hydroxybutyl methacrylate, or a combination of at least two thereof; Preferably, the molar ratio of the hydroxyl group in the polyester polyol to the isocyanate group in the diisocyanate in step (I) is 0.6-0.91:1; Preferably, the temperature in step (I) is raised to 45-90°C, preferably 50-85°C; Preferably, the catalyst in step (I) is an organotin catalyst, preferably dibutyltin dilaurate and / or stannous octoate; Preferably, the reaction time in step (I) is 2-6 h, preferably 2-4.5 h; Preferably, the molar ratio of the hydroxy acrylic acid in step (II) to the isophorone diisocyanate in step (I) is 1:0.55-0.8; Preferably, the reaction temperature in step (II) is 75-90°C, preferably 78-85°C; Preferably, the reaction time of step (II) is 2-6 h, preferably 2-4.5 h.
3. The core-shell polyester copolymer acrylic acid aqueous adhesive according to claim 1 or 2, characterized in that: The polymerizable monomers of the core include the following components in parts by weight: 12.25-80 parts of basic monomers, 0.25-30 parts of second functional monomers, and 0.25-15 parts of crosslinking monomers; Preferably, the polymerized monomers of the shell include the following components in percentage by mass: 10-80 parts of basic monomers, 0.2-25 parts of first functional monomers, 0.2-30 parts of second functional monomers, and 0.1-15 parts of cross-linking monomers; Preferably, the core-shell polyester copolymer acrylic acid aqueous adhesive is obtained by emulsion polymerization.
4. The method for preparing the core-shell polyester copolymer acrylic acid aqueous adhesive according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) preparing a core pre-emulsified liquid, a core pre-emulsified seed emulsion, a shell pre-emulsified liquid, a kettle bottom reaction liquid and an initiator solution; (2) adding the pre-emulsified seed emulsion to the reaction liquid at the bottom of the kettle, heating it, adding the initiator solution, and reacting; (3) adding the core pre-emulsion and the initiator solution to the reaction solution obtained in step (2) to react; (4) adding the shell pre-emulsion and the initiator solution to the reaction solution obtained in step (3), reacting to obtain the core-shell polyester copolymer acrylic acid aqueous adhesive.
5. The preparation method according to claim 4, characterized in that: Preferably, the core pre-emulsion comprises a basic monomer, a second functional monomer, a cross-linking monomer, an emulsifier and deionized water; Preferably, the core pre-emulsion includes 12.25-65 parts of basic monomers, 0.245-25 parts of second functional monomers and 0.25-15 parts of cross-linking monomers; Preferably, the amount of the emulsifier in the core pre-emulsion is 0.25% to 4% of the total weight of the basic monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion; Preferably, the amount of deionized water in the core pre-emulsion is 10%-80% of the total weight of the basic monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion; Preferably, the core pre-emulsified seed emulsion comprises a basic monomer, a second functional monomer, an emulsifier and deionized water; Preferably, the core pre-emulsified seed emulsion contains 0.25-30 parts of the basic monomer and 0.005-25 parts of the second functional monomer; Preferably, the amount of emulsifier in the core pre-emulsified seed emulsion is 0.005%-4% of the total weight of the basic monomers and the second functional monomers in the core pre-emulsified seed emulsion; Preferably, the amount of deionized water in the core pre-emulsified seed emulsion is 10% to 80% of the total weight of the basic monomers and the second functional monomers in the core pre-emulsified seed emulsion; Preferably, the shell pre-emulsion comprises a basic monomer, a first functional monomer, a second functional monomer, a cross-linking monomer, an emulsifier and deionized water; Preferably, the shell pre-emulsion includes 10-80 parts of basic monomers, 0.2-25 parts of first functional monomers, 0.2-30 parts of second functional monomers and 0.1-15 parts of cross-linking monomers; Preferably, the amount of the emulsifier in the shell pre-emulsion is 0.2% to 4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion; Preferably, the amount of deionized water in the shell pre-emulsion is 10%-80% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion; Preferably, the reaction liquid at the bottom of the kettle comprises an emulsifier, deionized water and a buffer; Preferably, the contents of the components in the bottom reaction liquid are 0.1-3 parts of emulsifier, 50-120 parts of deionized water, and 0.25-1 parts of buffer; Preferably, the emulsifiers in the core pre-emulsified liquid, the core pre-emulsified seed emulsion, the shell pre-emulsified liquid and the bottom reaction liquid are independently selected from any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene octylphenol ether-10, allyloxy fatty alcohol oxyethylene ether ammonium sulfate or disodium succinic acid nonylphenol polyoxyethylene ether monoester sulfonate or a combination of at least two thereof; Preferably, the buffer is sodium bicarbonate, ammonia water, ammonium bicarbonate, or sodium hydroxide; Preferably, the initiator solution comprises an initiator and deionized water; Preferably, the amount of deionized water in the initiator solution is 1-20 parts relative to 1 part by weight of the initiator; Preferably, the initiator is selected from inorganic peroxide initiators; Preferably, the initiator is selected from any one or a combination of at least two of potassium persulfate, ammonium persulfate or sodium persulfate; Preferably, the reaction in step (2) to step (4) is carried out under stirring, and the stirring speed is 100-500r / min.
6. The preparation method according to any one of claims 4-5, characterized in that: Before adding the pre-emulsified seed emulsion in step (2), the bottom reaction liquid is first added into the reaction kettle at 40-80°C; Preferably, the temperature in step (2) is increased to 75-85°C; Preferably, the mass of the reaction liquid at the bottom of the kettle in step (2) is 1 to 100 times that of the seed emulsion pre-emulsified in the core; Preferably, the amount of the initiator solution added in step (2) is 0.06%-25% of the weight of the core pre-emulsified seed emulsion; Preferably, the reaction time in step (2) is 10-30 min; Preferably, the weight ratio of the nuclear pre-emulsion in step (3) to the bottom reaction liquid in step (2) is 1:0.15-1; Preferably, the amount of the initiator solution added in step (3) is 0.0045%-25% of the weight of the core pre-emulsion; Preferably, the reaction temperature in step (3) is 75-85°C; Preferably, the reaction time in step (3) is 10-30 min.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The weight ratio of the core pre-emulsion in step (3) to the shell pre-emulsion in step (4) is 1:0.25-3; Preferably, the amount of the initiator solution added in step (4) is 0.006%-15% of the weight of the shell pre-emulsion; Preferably, the reaction temperature in step (4) is 80-90°C; Preferably, the reaction time in step (4) is 0.5-2.5 h.
8. The preparation method according to any one of claims 4 to 7, characterized in that: After the reaction in step (4) is completed, the temperature is lowered to 60-70° C., a residual monomer eliminator is added, and then the temperature is lowered to below 50° C., the pH is adjusted to 7-9, and the material is filtered to obtain the core-shell polyester copolymer acrylic acid water-based adhesive; Preferably, the residual monomer eliminator is bleaching powder and tert-butyl peroxide; Preferably, the reagent used to adjust the pH is any one of ammonia water, sodium hydroxide, lithium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two thereof.
9. A negative electrode plate for a lithium ion battery, characterized in that: The negative electrode plate of the lithium-ion battery comprises the core-shell polyester copolymer acrylic acid aqueous adhesive as described in any one of claims 1 to 8.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-ion battery negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Water-based sealing compound adhesive emulsion and preparation method thereof
CN106366985A
Water-based binder, modified diaphragm, battery and preparation method of water-based binder
CN115260403A
Core-shell latex with non-yellowing properties
WO2020170272A1