A refining slag changing process for regulating inclusions in grade 80 cord steel

By controlling the refining and slag transformation process of 80-level cord steel, the inclusions are controlled in the plastic zone, the wire breaking problem caused by inclusions in the steel cord is solved, the cleanliness and production quality of the steel is improved, and the production cost is reduced.

CN118792471BActive Publication Date: 2024-12-03LIANFENG STEEL (ZHANGJIAGANG) CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411276659.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-03
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

During the steel cord production process, there are wire breaking problems caused by inclusions in the 80-level cord steel, and the prior art is difficult to effectively control the size and type of inclusions, which affects the quality and production cost of steel cords.

Method used

A slag-changing process that regulates the inclusions of 80-level cord steel is adopted. By controlling the starting temperature of LF refining, adding deoxidant to diffusion and deoxygenation, adjusting the composition of the molten steel, extending the holding time of the white slag, and combining with the appropriate bottom blowing process, ensuring that Inclusions are in the plastic zone, reducing the formation of large-sized inclusions.

Benefits of technology

Effectively remove large-sized inclusions, reduce the wire breaking problems caused by inclusions, improve the cleanliness of steel, control the inclusion stages, and reduce the wire breaking rate during wire drawing and merging, which meets the needs of green and high-quality development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of cord steel production, and in particular to a refining and slag-changing process for regulating inclusions of grade 80 cord steel, comprising the following steps: controlling the LF refining starting temperature to 1470-1480°C, performing the first power transmission and slag-making, and adding a deoxidizer for diffusion deoxidation to make the slag basicity reach 1.8-2.2; after the first power transmission, adjusting the molten steel composition to a set range, and making the white slag holding time not less than 25min from the end of the molten steel composition adjustment to the slag-changing; after the composition and the white slag holding time reach the standard, slag-changing and power-transmitting slag, the final slag basicity after slag-changing is controlled at 0.8-1.2, and the soft blowing time is not less than 40min. The process of the present invention is used to improve the cleanliness of molten steel, reduce the size of molten steel inclusions, control the inclusions to be in the plastic zone, and reduce the problem of broken wire caused by inclusions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cord steel production, and in particular to a refining and slag-changing process for regulating inclusions in grade 80 cord steel. Background Art

[0002] Steel cord is known as the "crown jewel of wire". Φ5.5mm wire rod is drawn into Φ0.15-Φ0.38mm filaments through multiple drawing processes, and then made into steel cord products after being plied. The wire breakage rate of steel cord is an important indicator for evaluating the quality of cord steel wire rod. With many years of production and research and development in China, the production technology of 80-grade cord steel has become relatively mature, and the wire breakage rate is controlled at <4 times / ton. Although it can meet the market demand, there are still many quality fluctuations in the production process of steel cord factories.

[0003] At present, many studies believe that inclusions are not the main factor causing steel cord breakage, but from the various types and quantities of broken wires collected from downstream steel cord factories, there are still a certain amount of broken wire problems caused by inclusions. For the appearance of Class B alumina and Class C silicate inclusions, it is not fully explained by the fluctuation of production process control alone. Controlling the type and level of inclusions in the cord steel to ensure that the wire rod does not break during deep drawing and plying will help reduce the production cost of the steel cord factory and meet the needs of green and high-quality development.

[0004] The process flow of cord steel smelting is: KR desulfurization-converter-LF refining-continuous casting. In order to improve the cleanliness of molten steel, the introduction of Al element is avoided as much as possible in the whole process of cord steel smelting. Si-Mn deoxidation is adopted. In the most important refining link of inclusion control, the inclusions in the cord steel are modified to obtain plastic inclusions and avoid the formation of high melting point and high hardness inclusions. According to the plastic zone phase diagram of inclusions, under thermodynamic equilibrium conditions, when the slag basicity is about 1.0, the inclusions are in the plastic zone. Considering the actual production conditions and the influence of the slag slag formation route, a new refining and double slag making process is urgently needed to effectively obtain plastic inclusions, remove large-sized inclusions, and reduce the problem of broken wires caused by inclusions. Summary of the invention

[0005] In view of this, the purpose of the present invention is to propose a refining and slag-changing process for regulating inclusions in grade 80 cord steel, improve the cleanliness of molten steel, reduce the size of molten steel inclusions, control the inclusions in the plastic zone, and reduce the wire breakage problem caused by inclusions.

[0006] Based on the above purpose, the present invention provides a refining slag-changing process for regulating inclusions in grade 80 cord steel, comprising the following steps:

[0007] The starting temperature of LF refining is controlled at 1470-1480℃, and the first power supply is carried out to make slag, and deoxidizer is added for diffusion deoxidation to make the slag basicity reach 1.8-2.2; after the first power supply is completed, the molten steel composition is adjusted to be close to the internal control range of smelting, and the white slag retention time is not less than 25min from the completion of the molten steel composition adjustment to the slag change; after the composition and white slag retention time reach the standard, slag change is carried out and power is supplied to slag, and the final slag basicity after slag change is controlled at 0.8-1.2, and the soft blowing time is not less than 40min; among which, the parameters of the internal control range of smelting are: C: 0.81%~0.83%, Si: 0.18%~0.25%, Mn: 0.50%~0.55%, P: ≤0.012%, S: ≤0.08%, Al: ≤0.002%.

[0008] Among them, the white slag retention time is required to be ≥25min to ensure sufficient refining and deoxidation. The electrochemical slag is sent until the slag is completely dissolved, and stirred for 3-5min to promote the uniformity of the slag and the floating of inclusions. After the slag is changed, the soft blowing time is guaranteed to be ≥40min to further promote the floating adsorption of inclusions.

[0009] Preferably, before LF refining, the converter uses a 160-ton ladle for tapping steel, deoxidation and alloying are performed during the tapping process, and ladle top slag is added to the ladle, the ladle top slag is 520-600kg lime, 700-750kg pre-melted wollastonite, 200-250kg fluorite for cord steel.

[0010] Preferably, the power supply time of the first power supply slag making is 10-15 minutes, and fluorite specially used for cord steel is also added in the process of adding deoxidizer for diffusion deoxidation. The deoxidizer is calcium carbide and silicon 70 specially used for cord steel.

[0011] Preferably, 10-80 kg of fluorite specially used for cord steel, 0-60 kg of calcium carbide specially used for cord steel and 50-80 kg of silicon 70 are added to every 160 tons of steel ladle.

[0012] Preferably, white slag is formed after diffusion deoxidation, so that the slag FeO+MnO is less than 1.0%.

[0013] Preferably, the composition of the molten steel is adjusted by using high-purity ferrosilicon (Si≥75.0wt%, Al≤0.03wt%) and medium-carbon ferromanganese (Mn: 75.0wt%~82.0wt%).

[0014] Preferably, silicon is added after the molten steel composition is adjusted and before it becomes slag to maintain the white slag effect, and the amount of silicon added is 60-120 kg per 160 tons of ladle.

[0015] Preferably, for every 160 tons of ladle, 600-700 kg of quartz sand is added in 2-3 batches to change the slag, and the minimum single addition amount of quartz sand is not less than 120 kg.

[0016] Preferably, the bottom blowing Ar flow rate is 150-300NL / min when delivering electrochemical slag, the bottom blowing Ar flow rate is 50-150NL / min when changing slag, and the bottom blowing Ar flow rate is 20-100NL / min in the soft blowing stage.

[0017] The ladle heat preservation agent is added at the end of slag stirring and before soft blowing to ensure the stability of molten steel temperature and carbon content. The ladle heat preservation agent is carbonized rice husk.

[0018] Preferably, the superheat of the first furnace at the start-up of continuous casting is ensured to be between 30°C and 45°C, and the leaving-station temperature of LF refining is controlled at 1540°C to 1555°C.

[0019] The present invention also provides a high-strength 80-grade cord steel wire rod, which has the following chemical components, measured by mass percentage: C: 0.80-0.85%, Si: 0.15-0.30%, Mn: 0.30-0.45%, Cr: ≤0.20%, P: ≤0.012%, S: ≤0.008%, Ni≤0.05%, Cu≤0.05%, Al≤0.0030%, Mo≤0.030%, Ti≤0.0020%, O≤0.0020%, [N]≤0.0045%, and the remainder is Fe and unavoidable impurities.

[0020] Beneficial effects of the present invention: The refining and slag-changing operation of the present invention takes into account the influence of the slag-forming path on the plastic zone of non-metallic inclusions, and is combined with a suitable bottom blowing process to achieve complete removal of large-sized inclusions. The inclusion level control meets the standards of A≤1.5, Ae≤1.5, B≤1.5, Be≤1.0, C≤1.5, Ce≤1.5, D≤0.5, De≤0.5, and DS≤0.5. The cleanliness control effect of molten steel is good, plastic inclusions are obtained, and it is beneficial to reduce the wire breakage rate during wire drawing and stranding. DETAILED DESCRIPTION

[0021] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0022] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should have the common meanings understood by persons having ordinary skills in the field to which the present invention belongs.

[0023] The present invention provides a refining slag-changing process for regulating inclusions in grade 80 cord steel, which specifically comprises the following steps:

[0024] The converter uses a 160-ton ladle for steel tapping. During the steel tapping process, deoxidation and alloying are carried out, and 520-600kg of lime, 700-750kg of pre-melted wollastonite, and 200-250kg of fluorite for cord steel are added to the ladle to form the ladle top slag. The starting temperature of LF refining is 1470-1480℃, and the first power supply slag is carried out. The first power supply lasts for 10-15 minutes. At the same time, 10-80kg of fluorite for cord steel, 0-60kg of calcium carbide for cord steel, and 50-80kg of silicon 70 are added for diffusion deoxidation to ensure that the slag is fully melted and white slag is formed (slag FeO+MnO<1.0%), so that the slag basicity reaches 1.8-2.2. After the first power supply, the composition of the molten steel sample is analyzed, and high-purity ferrosilicon (Si≥75.0wt%, Al≤0.03wt%) and medium-carbon ferromanganese (Mn:75.0wt%~82.0wt%) are selected to adjust the composition. 60-120kg of silicon 70 is added before the slag is changed to maintain the white slag effect and ensure that the total white slag time is ≥25min. After the composition and white slag retention time reach the standard, 600-700kg of quartz sand is added in 2-3 batches to change the slag, and the slag is electrified until the slag is completely dissolved, stirred for 3-5min, to promote the uniformity of the slag and the floating of inclusions. After the slag is changed, the final slag basicity is maintained at 0.8-1.2. After the slag is changed, the soft blowing time is guaranteed to be ≥40min to further promote the floating adsorption of inclusions. The following is a detailed description through specific examples. Example 1

[0025] A high-strength 80-grade cord steel wire rod, the chemical composition of the wire rod comprising, by mass percentage, C: 0.83%, Si: 0.23%, Mn: 0.40%, Cr: 0.15%, P: 0.007%, S: 0.005%, Ni: 0.04%, Cu: 0.04%, Al: 0.0030%, Mo: 0.016%, Ti: 0.0009%, O: 0.0012%, N: 0.0029%, and the balance being Fe and unavoidable impurities.

[0026] A refining and slag-changing process for regulating inclusions in grade 80 cord steel comprises the following steps:

[0027] The converter uses a 160-ton ladle for steel tapping. During the tapping process, deoxidation and alloying are carried out, and 540kg of lime, 730kg of pre-melted wollastonite, and 220kg of fluorite for cord steel are added to the ladle to form the ladle top slag. The LF refining starts at 1475℃, and the first power supply is carried out for slag making. The first power supply lasts for 12 minutes. At the same time, 30kg of fluorite for cord steel, 40kg of calcium carbide for cord steel, and 60kg of silicon 70 are added for diffusion deoxidation to ensure that the slag is fully melted and white slag is formed (slag FeO+MnO<1.0%). At this time, the slag basicity is 2.1. After the first power supply, the steel sample was analyzed for composition, and high-purity ferrosilicon and medium-carbon ferromanganese were selected to adjust the composition to the internal control range of smelting (C: 0.81%~0.83%, Si: 0.18%~0.25%, Mn: 0.50%~0.55%, P: ≤0.012, S: ≤0.08, Al: ≤0.002%). After the composition adjustment was completed and before slag was changed, 80kg of silicon 70 was added to maintain the white slag effect. The total time of white slag was 28min. After the composition and white slag holding time reached the standard, 420kg was added first, and 260kg of quartz sand was added again after waiting for 2min to change the slag, and the slag was electrified until the slag was completely dissolved and stirred for 4min to promote the uniformity of the slag and the floating of inclusions. The final slag basicity after slag change was 1.1. The total soft blowing time after slag change was 43min, which further promoted the floating adsorption of inclusions. The bottom blowing Ar flow rate for electrified slag is 180NL / min, the bottom blowing Ar flow rate during slag change is 100NL / min, and the bottom blowing Ar flow rate during the soft blowing stage is 60NL / min. Example 2

[0028] A high-strength 80-grade cord steel wire rod, the chemical composition of the wire rod comprising, by mass percentage, C: 0.84%, Si: 0.18%, Mn: 0.38%, Cr: 0.11%, P: 0.008%, S: 0.004%, Ni: 0.023%, Cu: 0.036%, Al: 0.0026%, Mo: 0.012%, Ti: 0.0008%, O: 0.0012%, N: 0.0033%, and the balance being Fe and unavoidable impurities.

[0029] A refining and slag-changing process for regulating inclusions in grade 80 cord steel comprises the following steps:

[0030] The converter uses a 160-ton ladle for steel tapping. During the tapping process, deoxidation and alloying are carried out, and 580kg of lime, 710kg of pre-melted wollastonite, and 210kg of fluorite for cord steel are added to the ladle to form the ladle top slag. The LF refining starts at 1474℃, and the first power supply is carried out for slag making. The first power supply lasts for 12 minutes. At the same time, 30kg of fluorite for cord steel, 30kg of calcium carbide for cord steel, and 40kg of silicon 70 are added for diffusion deoxidation to ensure that the slag is fully melted and white slag is formed (slag FeO+MnO<1.0%), so that the slag basicity reaches 2.0. After the first power supply, the composition of the molten steel sample was analyzed, and high-purity ferrosilicon and medium-carbon ferromanganese were selected to adjust the composition to the internal control range of smelting (C: 0.81% ~ 0.83%, Si: 0.18% ~ 0.25%, Mn: 0.50% ~ 0.55%, P: ≤ 0.012%, S: ≤ 0.08%, Al: ≤ 0.002%). After the composition adjustment is completed and before slag change, 70kg of silicon 70 is added to maintain the white slag effect. The total time of white slag is 26min. After the composition and white slag retention time reach the standard, 410kg is added first, and 230kg is added again after waiting for 2min, and the slag is electrified until the slag is completely dissolved and stirred for 4min to promote the uniformity of the slag and the floating of inclusions. After the slag change, the final slag basicity is maintained at 0.9. After the slag change, the total soft blowing time is 55min, which further promotes the floating adsorption of inclusions. The Ar flow rate for bottom blowing during electrification slag delivery is 170NL / min, the Ar flow rate for bottom blowing during slag change is 110NL / min, and the Ar flow rate for bottom blowing during soft blowing stage is 70NL / min. Example 3

[0031] A high-strength 80-grade cord steel wire rod, the chemical composition of the wire rod comprising, by mass percentage, C: 0.81%, Si: 0.28%, Mn: 0.33%, Cr: 0.015%, P: 0.007%, S: 0.005%, Ni: 0.032%, Cu: 0.032%, Al: 0.0026%, Mo: 0.019%, Ti: 0.0007%, O: 0.0011%, [N]: 0.0032%, and the balance being Fe and unavoidable impurities.

[0032] A refining and slag-changing process for regulating inclusions in grade 80 cord steel comprises the following steps:

[0033] The converter uses a 160-ton ladle for steel tapping. During the tapping process, deoxidation and alloying are carried out, and 535kg of lime, 740kg of pre-melted wollastonite, and 230kg of fluorite for cord steel are added to the ladle to form the ladle top slag. The LF refining starts at 1477℃, and the first power supply is carried out for slag making. The first power supply lasts for 10 minutes. At the same time, 30kg of fluorite for cord steel, 20kg of calcium carbide for cord steel, and 30kg of silicon 70 are added for diffusion deoxidation to ensure that the slag is fully melted and white slag is formed (slag FeO+MnO<1.0%), so that the slag basicity reaches 2.1. After the first power supply, the composition of the molten steel sample was analyzed, and high-purity ferrosilicon and medium-carbon ferromanganese were selected to adjust the composition to the internal control range of smelting (C: 0.81%~0.83%, Si: 0.18%~0.25%, Mn: 0.50%~0.55%, P: ≤0.012%, S: ≤0.08%, Al: ≤0.002%). 75kg of silicon 70 was added before the slag change to maintain the white slag effect, and the total white slag time was 27min. After the composition and white slag holding time reached the standard, 420kg was added first, and 260kg of quartz sand was added again after waiting for 2min to change the slag, and the slag was electrified until the slag was completely dissolved and stirred for 5min to promote the uniformity of the slag and the floating of inclusions. After the slag change, the final slag basicity was maintained at 1.1. The total soft blowing time after the slag change was 53min, which further promoted the floating adsorption of inclusions. The Ar flow rate for bottom blowing during electrification slag delivery is 210NL / min, the Ar flow rate for bottom blowing during slag change is 130NL / min, and the Ar flow rate for bottom blowing during soft blowing stage is 70NL / min.

[0034] The final Φ5.5mm wire rods of furnace numbers of Examples 1, 2 and 3 were tested for inclusions, with 50 samples per furnace, and the results are shown in Tables 1, 2 and 3. It can be seen from the table that all inclusion ratings meet the standards, among which the maximum level of B, C and D inclusions is 0.5, and DS inclusions are all level 0. The slag changing operation combined with the appropriate soft blowing flow rate can obtain the type and size of inclusions that meet the standards. Table 4 is the verification results of 50 rolls of wire rods in Example 1, Example 2 and Example 3 fed back by the steel cord factory. It can be seen from the verification results that the broken wire rate caused by inclusions has been effectively controlled. The broken wire rate of inclusions in Examples 2 and 3 accounts for 0%, and a broken wire problem caused by inclusions was detected in Example 1.

[0035] Table 1 Wire rod inclusion rating of Example 1

[0036]

[0037] Table 2 Wire rod inclusion ratings of Example 2

[0038]

[0039] Table 3 Wire rod inclusion ratings of Example 3

[0040]

[0041] Table 4 Wire breakage rate of steel cord factory verification examples 1, 2 and 3

[0042]

[0043] Those skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A refining slag process for regulating inclusions in grade 80 cord steel, characterized in that: The steps include: The starting temperature of LF refining is controlled at 1470-1480℃, and the first power supply is carried out to make slag, and deoxidizer is added for diffusion deoxidation to make the slag basicity reach 1.8-2.2; after the first power supply, adjust the molten steel composition to the internal control range of smelting, and keep the white slag for no less than 25 minutes from the end of the adjustment of the molten steel composition to the slag change; after the composition and the white slag holding time reach the standard, slag change and power supply are carried out to make slag, and the final slag basicity after slag change is controlled at 0.8-1.2, and soft blowing The time is not less than 40min; among them, the internal control range parameters of smelting are: C: 0.81%~0.83%, Si: 0.18%~0.25%, Mn: 0.50%~0.55%, P: ≤0.012%, S: ≤0.08%; the bottom blowing Ar flow rate is 150-300NL / min when sending electrochemical slag, the bottom blowing Ar flow rate is 50-150NL / min when changing slag, and the bottom blowing Ar flow rate is 20-100NL / min in the soft blowing stage.

2. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 1, characterized in that: The power supply time of the first power supply slag making is 10-15 minutes. In the process of adding the deoxidizer for diffusion deoxidation, fluorite specially used for cord steel is also added. The deoxidizer is calcium carbide and silicon 70 specially used for cord steel.

3. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 2, characterized in that: For every 160-ton ladle, add 10-80kg of fluorite specially made for cord steel, 0-60kg of calcium carbide specially made for cord steel and 50-80kg of silicon 70.

4. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 1, characterized in that: After diffusion deoxidation, white slag is formed, making the slag FeO+MnO<1.0%.

5. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 1, characterized in that: The composition of the molten steel is adjusted by using high-purity ferrosilicon and medium-carbon ferromanganese.

6. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 1, characterized in that: Silicon is added after the molten steel composition is adjusted and before it becomes slag to maintain the white slag effect. The amount of silicon added is 60-120 kg per 160 tons of ladle.

7. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 1, characterized in that: For every 160-ton ladle, 600-700 kg of quartz sand is added in 2-3 batches during slag changing. The minimum single addition amount of quartz sand is not less than 120 kg.

8. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 1, characterized in that: The time to add the ladle insulation agent is when the slag stirring is completed and before the soft blowing begins.

9. The refining slag-changing process for controlling inclusions in grade 80 cord steel according to claim 1, characterized in that: The leaving station temperature of LF refining is controlled at 1540~1555℃.

Citation Information

Patent Citations

  • Control method for tire cord steel LX72A non-metallic inclusions

    CN106906330A

  • Method for controlling brittle inclusions of tire cord steel

    CN114438398A

  • Tire cord steel inclusion plasticization control method and tire cord steel

    CN114807727A

  • 45 # steel refining and slagging method

    CN115595402A

  • Molding control method for cord steel inclusions

    CN116814890A