Preparation method of aluminum alloy plate for outer plate of automobile covering part
By improving the hot rolling process and process flow and canceling the intermediate annealing process, the paint line problem of 6xxx series aluminum alloy sheets in the preparation of outer panels of automobile panels has been solved, the production efficiency and sheet performance have been improved, and low energy consumption and high efficiency have been achieved Preparation of aluminum alloy plates.
Patent Information
- Application Number
- CN202410911834.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Existing 6xxx series aluminum alloy sheets have paint line problems in the preparation of exterior panels for automobile panels, which affects the surface quality. In addition, the intermediate annealing process in the traditional process is complex and energy-consuming, which limits production efficiency and carbon emissions.
A short-process preparation method without intermediate annealing is adopted. By improving the hot rolling process, including homogenization treatment, hot rough rolling, hot finish rolling, cold rolling, solution treatment and pre-aging treatment, the grain size and texture distribution are controlled to ensure The uniformity and high quality of the boards.
It achieves the production of high-quality aluminum alloy plates without intermediate annealing processes, shortens the production cycle, reduces energy consumption and carbon emissions, improves the yield strength and flanging performance of the plates, and meets the industrial production needs of automobile panels.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to an aluminum alloy and a preparation method thereof, and in particular to a preparation method of a 6xxx series aluminum alloy sheet material for an outer panel of an automobile covering part. Background Art
[0002] Exhaust emissions from gasoline vehicles are one of the important sources of global air pollution. Lightweighting of automobiles is an important means of saving energy, reducing emissions and reducing pollution. Aluminum alloy sheets are considered to be ideal materials for lightweighting of automobiles due to their light weight, high specific strength and excellent comprehensive performance. At present, 5xxx and 6xxx aluminum alloys are mainly used to prepare automobile sheets. 5xxx aluminum alloy has defects such as Luders bands, which limits its scope of use. 6xxx alloy has excellent surface quality and is more widely used in automobile cover outer panels. Although the surface quality of 6xxx aluminum alloy is better than that of 5xxx, there are still problems such as paint brush lines that affect the surface quality.
[0003] Paint brush lines are mainly caused by improper processing technology, which leads to the distribution of Cube, Goss and other textures in stripes along the rolling direction of the plate. During deformation such as stretching and stamping, the plate deforms unevenly, thus forming stripes along the rolling direction, affecting the appearance. In recent years, some domestic universities and research institutes have carried out a series of research on improving 6xxx aluminum alloy automotive plates: Patent CN 104532077A proposes a short-process preparation method for 6XXX series aluminum alloy body panels without a paint brush line. The method adopts a short-process preparation method without intermediate annealing, but it lacks attention to the hot rough rolling process and the uniformity of the coil.
[0004] Patent CN 107109547A proposes a highly formable automotive aluminum sheet with reduced or no surface streaks and a preparation method. In terms of process, the hot rolling temperature needs to be lower than 300°C to inhibit the formation of coarse Mg 2 Si precipitation; the intermediate annealing temperature is 350-450℃ box annealing, which can be carried out after hot rolling or one cold rolling to improve the texture and eliminate the paint brush line. In addition, this process precipitates a large amount of fine soluble Mg 2 Si is beneficial to obtain excellent comprehensive performance after solid solution. This method adopts an intermediate annealing process, which is quite different from the non-intermediate annealing process adopted by the present invention.
[0005] Patent CN 101918602A proposes an aluminum alloy plate, particularly an aluminum alloy plate with excellent ridging mark resistance, but the focus is mainly on analyzing the paint brush line of the plate through tissue analysis.
[0006] The present invention provides a method for preparing 6xxx series aluminum alloy sheets for automobile cover outer panels based on the preparation process of traditional 6xxx series aluminum alloy sheets by improving the hot rolling process. The method omits the intermediate annealing process, has a short process flow, low cost, and low carbon emissions. The prepared sheets have excellent paint brushing line performance and are more conducive to industrial production. Summary of the invention
[0007] The object of the present invention is to provide a method for preparing a 6xxx series aluminum alloy sheet for an outer panel of an automobile covering part.
[0008] To achieve the above object, the present invention adopts the following technical solution: A method for preparing an aluminum alloy sheet for an automobile cover outer panel comprises the following steps: (1) Preparing aluminum alloy ingots; (2) homogenizing the aluminum alloy ingot; (3) hot rough rolling the homogenized ingot; (4) hot finishing rolling the rough hot rolled billet to produce a hot rolled coil; (5) cold rolling the hot rolled coil to produce a cold rolled coil; (6) Solution treatment of the cold rolled coil; (7) Pre-aging treatment of the coil after solution treatment; (8) The pre-aging coil is uncoiled, straightened and sliced to obtain the finished product.
[0009] Furthermore, based on the sum of the mass percentages being 100%, the mass percentages of the components in the aluminum alloy ingot obtained in step (1) are: Si 0.50%~1.50%, Fe≤0.40%, Cu≤0.30%, Mn≤0.2%, Mg 0.3%~1.1%, Cr≤0.1%, Ti 0.01-0.10%, and the balance being Al.
[0010] Furthermore, the homogenization treatment in step (2) is carried out at 540-580°C for 4-20 h, followed by cooling to 490-540°C and keeping the temperature for 1-10 h.
[0011] Furthermore, the total deformation rate of the hot rough rolling in step (3) is not less than 90%, the total number of passes is 8-18 passes, the average pass reduction is not less than 30 mm, the final rolling thickness is 20-40 mm, the final rolling temperature is not less than 400°C; along the width direction of the plate, the temperature difference between the middle and the edge is not higher than 15°C.
[0012] Furthermore, the final rolling thickness of the hot finish rolling in step (4) is 2.5-6.0 mm, the rolling speed of the final pass is 2-8 m / s, the final rolling temperature is 300-380°C, and after 10 minutes of coiling, the temperature difference at all locations of the entire coil is not higher than 10°C; the cooling rate of the hot rolled coil to room temperature is not higher than 15°C / h.
[0013] Furthermore, the thickness of the cold-rolled sheet obtained in step (5) is 0.5-2.0 mm, and the cold rolling rate is 60-80%.
[0014] Furthermore, the solution treatment in step (6) is carried out in an air cushion continuous annealing furnace, with the temperature being raised to 520-580°C at a rate of 5-50°C / s and maintained at that temperature for 0.5-5 min.
[0015] Furthermore, the pre-aging treatment in step (7) is carried out at 70-100° C. for 4-12 hours.
[0016] Furthermore, the finished product obtained in step (8) is a T4P state plate, whose 7-day yield strength is less than 110 MPa and the flanging factor r / t min ≤0.5, the paint lines on the edges and the middle are better than level 2.
[0017] Furthermore, after the finished product is further pre-stretched by 2% and baked at 185°C for 20 minutes, a T8X state plate can be obtained, and its yield strength is greater than 200MPa.
[0018] Compared with the prior art, the technical progress of the present invention is mainly reflected in: (1) The present invention improves the hot rolling process and innovatively eliminates the intermediate annealing process that is essential in the production of the original aluminum alloy sheet for the outer cover, shortens the production cycle of the 6xxx aluminum alloy for the outer plate of the cover, greatly improves the production efficiency, reduces energy consumption, and further reduces carbon emissions.
[0019] (2) The present invention refines the grain size and changes the trend of continuous distribution of the texture along the rolling direction to make it uniformly distributed through process control such as the total reduction of hot rough rolling and the reduction of each pass. At the same time, by controlling the hot finishing rolling temperature, rolling speed, cooling speed and thickness, partial recrystallization of the hot finishing rolling structure of the plate is achieved, further breaking the trend of continuous distribution of the texture, thereby realizing the preparation of high-quality aluminum alloy plates that meet the performance requirements of the paint brushing line for outer cover plates without an intermediate annealing process.
[0020] (3) The present invention strictly controls the temperature uniformity of hot rough rolling and hot finish rolling to ensure uniformity throughout the coil, especially improving the problem of differences in paint brushing lines at the edges and middle along the width of the plate.
[0021] (4) The present invention does not add any additional processes or production equipment and can be applied to the existing production equipment of 6xxx plates without any additional conditional elements. It has strong applicability and can meet the requirements of industrial production.
[0022] (5) The aluminum alloy sheet prepared by the method of the present invention has the characteristics of low yield strength, high room temperature parking stability, good flanging performance and surface quality in the T4P state, which can meet the stamping, connection, painting and other requirements of automobile companies. After further baking, it can reach the T8X state, and its yield strength increases rapidly, meeting the strength requirements during service. DETAILED DESCRIPTION
[0023] Terminology explanation: Weight percentage: The percentage of a certain alloy component's mass (weight) to the total mass.
[0024] Reduction per pass: The thickness before each pass is H, the thickness after rolling is h, and the reduction per pass Δh=Hh.
[0025] Yield strength: The yield limit of aluminum alloy when yielding occurs. The stress value that produces 0.2% residual deformation is defined as its yield limit. The stress-strain curve is obtained through uniaxial tensile test, and the yield strength data is obtained through the curve.
[0026] Yield strength in T4P state: The finished plate is obtained after melting, homogenization, hot rolling, cold rolling, solution treatment, pre-aging and slicing. After the finished plate is stored at room temperature for 7 days, the yield strength is obtained by testing the mechanical properties through a uniaxial tensile test.
[0027] Yield strength in T8X state: After the finished plates have been stored at room temperature for 7 days, they are pre-stretched by 2% using a unidirectional stretching machine, and then kept in an oil bath furnace at 185°C for 20 minutes (simulating the baking process in the actual production process of the OEM), and the yield strength in the baking state is tested using a unidirectional tensile test.
[0028] Flanging performance: Cut a long strip sample with a length of 250mm and a width of 30mm from the finished plate, pre-stretch the sample by 10% along the length direction, and then cut a 50mm long rectangular sample. Use the indenter to perform a 180° bending test to test the flanging factor r / t, where r is the radius of the indenter and t is the plate thickness (during the test, the spacing between the support rollers must be 2r+2t+0.1mm). Take metallographic photos and grade evaluation of the outer surface after bending, Grade 1: smooth surface, no microcracks and continuous necking; Grade 2: slightly rough surface, no microcracks and continuous necking; Grade 3: microcracks or continuous necking on the surface; Grade 4: obvious cracks on the surface, of which Grades 1 and 2 are acceptable, and Grades 3 and 4 are unacceptable. The final flanging factor is the minimum flanging factor that satisfies the surface quality of Grade 2 or better after flanging.
[0029] Paint brush line performance: a strip sample with a length of 250mm and a width of 35mm is cut from the finished plate. The length direction of the sample is perpendicular to the rolling direction, and the width direction is parallel to the rolling direction. After the sample is pre-stretched by 10% along the length direction, it is polished with a 320-mesh oilstone. The surface morphology of the polished sample is graded and evaluated. Grade 1: no obvious paint brush line along the width direction; Grade 2: intermittent paint brush lines along the width direction, and no penetrating paint brush lines; Grade 3: sparse penetrating paint brush lines along the width direction; Grade 4: dense penetrating paint brush lines along the width direction. Grades 1 and 2 are acceptable, and grades 3 and 4 are unacceptable.
[0030] The present invention is further supplemented and illustrated below in conjunction with specific implementation schemes. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of them.
[0031] First, pure aluminum and various master alloys are melted according to the ratio in Table 1. After the melt is refined, an ingot is cast using a semi-continuous casting device. After the ingot is cut and milled, it is placed in a heat treatment furnace and homogenized according to the parameters in Table 2. After the homogenized ingot is taken out of the furnace, it is directly hot-rolled; after the hot rolling is completed, the hot-rolled plate is cold-rolled; the cold-rolled plate is subjected to solution and pre-aging treatment and then trimmed and blanked, that is, the finished plate. The obtained plate was parked at room temperature for 7 days, and the mechanical properties, flanging properties, and paint brush line properties were tested respectively. After that, the finished plate was pre-stretched by 2%, and then kept in an oil bath furnace at 185°C for 20 minutes, and the mechanical properties were tested after water quenching to room temperature. The test results are shown in Table 3.
[0032] Table 1 Composition ratio of aluminum alloy sheet
[0033] Table 2 Process parameters of aluminum alloy for outer panels (I)
[0034] Table 2 Process parameters of aluminum alloy for outer panel of cover parts (II) ,
[0035] Table 3 Performance test results of aluminum alloy for outer panels
[0036] As can be seen from Tables 2 and 3, the mechanical properties of the finished plates obtained in Examples 1 to 6 are qualified. However, due to the insufficient total deformation rate of hot rough rolling, the grain size and texture of Comparative Example 1 cannot meet the requirements, so the flanging performance and paint brush line performance are not good; in Comparative Example 2, the inner ring temperature of hot finishing rolling is low, and the temperature of the inner and outer rings is uneven, resulting in poor paint brush line performance at the edge; in Comparative Example 3, the final rolling temperature of hot rough rolling is too low, and the paint brush line cannot meet the requirements; in Comparative Example 4, the starting rolling temperature is too low, and the Mg 2 A large amount of Si precipitates, resulting in insufficient strength of the final finished plate; the final hot-rolling speed of Comparative Example 5 is too low, and the plate has poor paint-brushing performance; the cooling speed of Comparative Example 6 is too high, and the self-annealing of the hot-rolled coil is not effectively utilized, so the flanging performance and paint-brushing performance are poor; the single-pass reduction of Comparative Example 7 is insufficient, and the grain size and texture cannot meet the requirements, so the flanging performance and paint-brushing performance are not good; Comparative Example 8 has too small cold rolling rate and too large grain size, so the flanging performance and paint-brushing performance are poor; the cold rolling rate of Comparative Example 9 is too large, and the paint-brushing performance still cannot meet the requirements; the edge temperature of Comparative Example 10 is low in hot rough rolling, and the temperature difference in the edge is large, resulting in poor paint-brushing performance of the edge; Comparative Example 11 only has a low edge temperature in hot rough rolling, and the edge paint-brushing performance is also poor; the temperature of the hot-finished inner ring of Comparative Example 12 is low, and the temperature of the inner and outer rings is uneven, resulting in poor paint-brushing performance; Comparative Example 13 only has a low temperature in the hot-finished inner ring, resulting in poor paint-brushing performance.
[0037] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A method for preparing an aluminum alloy sheet for an automobile cover outer panel, It is characterized in that The steps include: (1) Preparing aluminum alloy ingots; (2) homogenizing the aluminum alloy ingot; (3) hot rough rolling the homogenized ingot; (4) hot finishing rolling the rough hot rolled billet to produce a hot rolled coil; (5) cold rolling the hot rolled coil to produce a cold rolled coil; (6) Solution treatment of the cold rolled coil; (7) Pre-aging treatment of the coil after solution treatment; (8) The pre-aging coil is uncoiled, straightened and sliced to obtain the finished product.
2. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that Taking the sum of the mass percentages as 100%, the mass percentages of the components in the aluminum alloy ingot obtained in step (1) are as follows: Si 0.50%-1.50%, Fe≤0.40%, Cu≤0.30%, Mn≤0.2%, Mg 0.3%-1.1%, Cr≤0.1%, Ti 0.01-0.10%, and the balance being Al.
3. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The homogenization treatment in step (2) is carried out by keeping the temperature at 540-580°C for 4-20 hours, then cooling to 490-540°C and keeping the temperature for 1-10 hours.
4. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The total deformation rate of the hot rough rolling in step (3) is not less than 90%, the total number of passes is 8-18 passes, the average pass reduction is not less than 30 mm, the final rolling thickness is 20-40 mm, and the final rolling temperature is not less than 400°C; along the width direction of the plate, the temperature difference between the middle and the edge is not higher than 15°C.
5. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The final rolling thickness of the hot finish rolling in step (4) is 2.5-6.0 mm, the rolling speed of the final pass is 2-8 m / s, the final rolling temperature is 300-380°C, and after 10 minutes of coiling, the temperature difference at all locations of the entire coil is not higher than 10°C; the speed at which the hot rolled coil is cooled to room temperature is not higher than 15°C / h.
6. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The thickness of the cold-rolled sheet obtained in step (5) is 0.5-2.0 mm, and the cold rolling rate is 60-80%.
7. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The solution treatment in step (6) is carried out in an air cushion continuous annealing furnace, with the temperature being raised to 520-580°C at a rate of 5-50°C / s and kept at that temperature for 0.5-5min.
8. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The pre-aging treatment in step (7) is carried out at 70-100°C for 4-12 hours.
9. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The finished product obtained in step (8) is a T4P state plate, whose 7-day yield strength is less than 110MPa and the flanging factor r / t min ≤0.5, the paint lines on the edges and the middle are better than level 2.
10. The method for preparing the aluminum alloy sheet for automobile outer panel according to claim 1, It is characterized in that The finished product is further pre-stretched by 2% and baked at 185°C for 20 minutes to obtain a T8X state plate with a yield strength greater than 200MPa.
Citation Information
Patent Citations
Aluminum-base alloy sheet
CN101918602A
Short-flow preparation method for 6XXX-series aluminum alloy automotive body sheet without paint brushed lines
CN104532077A
Highly formable automotive aluminum sheet with reduced or no surface roping and a method of preparation
CN107109547A
Autobody 6XXX series aluminium alloy plate with high edge-curling property and manufacturing method thereof
CN105441740A
Method of making 6xxx aluminium sheets with high surface quality
CN113166858A
Cited By
Short-process 6XXX series automobile inner and outer covering part general aluminum alloy preparation method