Green repair construction method for urban ceramic tile facade
Through a green repair construction method, polymer cement mortar and waterproof decorative integrated coating are used, combined with expansion waterstop strips and alkali-resistant fiberglass mesh cloth, to solve the problems caused to the building during the repair process of ceramic tile facades in the existing technology. Problems of damage and high costs have been eliminated, and efficient, safe, and environmentally friendly repairs have been achieved.
Patent Information
- Application Number
- CN202411171959.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-10-18
AI Technical Summary
Repair methods for existing building tile facades usually require the removal of the original tile surface layer, causing damage to the base of the building's exterior wall, increasing costs and construction periods, and traditional methods involve the risk of large-scale demolition and environmental impact.
Adopt a green repair construction method, including cleaning the hollow and cracked areas of the tiles, using polymer cement mortar to level, adding a quick-drying agent to the putty layer to accelerate drying, and then applying a base-reinforced sealing primer and waterproof decoration integration Paint and varnish to avoid large-area demolition, and add intumescent waterstop strips and alkali-resistant fiberglass mesh to enhance the integrity of the repair base surface.
Shorten the construction period, reduce the generation of construction waste, reduce construction costs, improve the quality and safety of repairs, achieve green and environmentally friendly construction, extend the service life of the building and ensure safety.
Smart Images

Figure CN118793299A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building construction, and in particular to a green restoration construction method for urban ceramic tile facades. Background Art
[0002] At present, in the field of construction engineering, the exterior facades of existing buildings with tile bases have been exposed to wind and sun for many years, and the exterior tile decorative surfaces have been damaged to varying degrees. Conventional exterior facade renovation methods are mainly to remove the original tile surface layer and then re-apply the exterior facade paint. In the process of removing the exterior tile surface, it is inevitable that some damage will be caused to the exterior wall base of the building. This process will inevitably increase costs and increase construction time. Summary of the invention
[0003] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a green restoration construction method for urban ceramic tile facades. The present invention can shorten the construction period, avoid major construction modifications to the exterior wall structure of existing buildings, achieve cost reduction and efficiency improvement of the project, increase the service life of the building and ensure safe use.
[0004] A green restoration construction method for urban tile facades is carried out in the following steps:
[0005] S1: Clean the existing building facade, repair the hollow and cracked areas of tiles and then level them;
[0006] S2: After step S2, the outer surface of the wall is fully leveled with polymer cement mortar;
[0007] S3: Apply two coats of cement-based exterior wall putty, add quick-drying agent to the putty to accelerate the drying and forming of the putty, and then grind the putty to make it smooth;
[0008] S4: Then, a base reinforcement sealing primer is applied by roller coating on the outer surface of the putty after step S3;
[0009] S5: Roller-coat the waterproof decorative integrated paint twice on the outer surface of the sealing primer;
[0010] S6: Continue to roll on the topcoat over the waterproof decorative integrated paint to complete the wall repair.
[0011] Further, in step S1, the existing building facade includes the original building exterior wall base wall, the original building exterior wall brick mortar bonding layer and the original building exterior wall bricks arranged in sequence from the inside to the outside. The specific steps of step S1 are:
[0012] Step S1.1: Find the hollow and cracked areas of the wall, then use a hand drill to remove them locally, remove the corresponding original building exterior wall tiles, and clean the original building exterior wall tile mortar bonding layer behind the original building exterior wall tiles;
[0013] Step S1.2: Then brush cement mortar, remove the tiles formed at the repaired area, add an expansion water stop strip at the junction of the repaired area and the original building exterior wall tiles, press a layer of alkali-resistant glass fiber mesh cloth in the middle, and fix it with a fixing plate.
[0014] Furthermore, the expansion water stop strip is a water-expandable expansion water stop strip with a width of 200 mm and a thickness of 10 mm; the bulk density of the alkali-resistant glass fiber mesh cloth should be 160 g / m 2 , and the glass component ZrO in the alkali-resistant glass fiber mesh cloth 2 In the range of 14.5% ± 0.8%, TiO 2 Within the range of 6%±0.5%.
[0015] Furthermore, the fixing plate is composed of a 2.5×28mm galvanized cement nail and a 20mm diameter galvanized gasket. The fixing plate is anchored into the wall 15-20mm and arranged in a matrix, with a horizontal and vertical spacing of 600mm.
[0016] Furthermore, in step S2, the full batch of polymer cement mortar needs to be mixed with 5% cement-based modifier and enhancer, and the construction thickness of the polymer cement mortar is 15 mm.
[0017] Furthermore, in step S3, the model of the full batch of cement-based exterior wall putty should be R type; the fineness of the quick-drying agent is between 7.3-8.5, the alkali content is between 8.2-8.8, the 28d compressive strength ratio (%) is between 72-78, and the first exterior wall putty layer and the second exterior wall putty layer are formed after two coats of full batch of cement-based exterior wall putty.
[0018] Furthermore, in step S3, the putty should be polished with 240-mesh sandpaper after the putty is completely dry. The time for the putty to dry is 3-4 days in winter and 1-2 days in summer.
[0019] Furthermore, in step S4, the model of the base reinforcement sealing primer is WDQ-C-1; the performance requirements are: water permeability ≤ 0.3mL, low temperature stability without deterioration, alkali resistance for 48h without abnormality; resistance to salt and alkali for 120h without abnormality.
[0020] Furthermore, in step S5, the waterproof decorative integrated coating adopts a ZGLM type waterproof decorative integrated coating made by mixing acrylic emulsion and special cement, and the waterproof decorative integrated coating is rolled on the outer surface of the sealing primer twice to form a first waterproof decorative integrated coating layer and a second waterproof decorative integrated coating layer.
[0021] Furthermore, in step S6, the finishing paint is applied by roller coating.
[0022] In summary: The green repair construction method for urban ceramic tile facades provided by the present invention has the following advantages: it avoids the practice of removing all the original ceramic tile surface layers in the conventional ceramic tile facade renovation, reduces the amount of facade renovation and demolition engineering, and shortens the construction period; it also reduces the construction waste generated during the construction process, and plays a certain positive role in the green and environmentally friendly construction of the building facade renovation project, the implementation of sustainable development, and the promotion of minimization of environmental impact. The waterproof decorative integrated coating has both waterproof and decorative functions. In the process of renovation of the existing building ceramic tile facades, compared with the construction methods of traditional waterproof coatings and real stone paints, it reduces the construction process and can collaboratively solve the renewal needs of waterproofing and decoration. The construction method of the present invention only removes hollow and cracked wall tiles at the beginning of construction, and does not carry out large-scale demolition, reducing the risk of demolition and falling objects, thereby enhancing construction safety. The construction method of the present invention presses alkali-resistant glass fiber mesh cloth when the polymer cement mortar is leveled, and is fixed with a fixing plate, which effectively increases the integrity of the repair base surface, thereby ensuring the construction quality of the repair of the ceramic tile facade of the existing building. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the cross-sectional structure of the wall after repair according to the present invention;
[0024] Figure 2 It is a schematic diagram of the vertical cross-sectional structure of the repaired wall of the present invention.
[0025] Among them: the base wall of the original building's exterior wall 1; the original building's exterior wall brick mortar bonding layer 2; the original building's exterior wall bricks 3; the brick removal and repair area 4; the alkali-resistant glass fiber mesh cloth 5; the fixing plate 6; the polymer cement mortar 7; the expansion water stop strip 8; the first exterior wall putty layer 9; the second exterior wall putty layer 10; the sealing primer 11; the first waterproof decorative integrated coating layer 12; the second waterproof decorative integrated coating layer 13; the topcoat 14. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0027] like Figure 1 and Figure 2 As shown, a green restoration construction method for urban tile facades is carried out in the following steps:
[0028] S1: Clean the existing building facade, repair the hollow and cracked areas of tiles and then level them;
[0029] S2: After step S2, the outer surface of the wall is fully coated with polymer cement mortar 7 for leveling;
[0030] S3: Apply two coats of cement-based exterior wall putty, add quick-drying agent to the putty to accelerate the drying and forming of the putty, and then grind the putty to make it smooth;
[0031] S4: Then, a base reinforcement sealing primer 11 is applied by roller coating on the outer surface of the putty after step S3;
[0032] S5: Roller-coat the waterproof decorative integrated coating twice on the outer surface of the sealing primer 11;
[0033] S6: Continue to roll-coat the topcoat 14 on the waterproof decorative integrated coating to complete the wall repair.
[0034] As a preferred embodiment, in step S1, the existing building facade includes an original building exterior wall base wall 1, an original building exterior wall brick mortar bonding layer 2 and an original building exterior wall brick 3 arranged in sequence from the inside to the outside. The specific steps of step S1 are:
[0035] Step S1.1: Find the hollow and cracked areas of the wall, then use a hand drill to remove them locally, remove the corresponding original building exterior wall tiles 3, and clean the original building exterior wall tile mortar bonding layer 2 behind the original building exterior wall tiles 3;
[0036] Step S1.2: Then brush cement mortar, remove the tiles formed at the repair site, add an expansion water stop strip 8 at the junction of the repair area 4 and the original building exterior wall tiles 3, press a layer of alkali-resistant glass fiber mesh cloth 5 in the middle, and fix it with a fixing plate 6; the integrity of the repair base surface is effectively increased, thereby ensuring the construction quality of the repair of the existing building tile facade, and overcoming the defects of large safety risks, high costs and long periods caused by large-scale demolition.
[0037] As a preferred embodiment, the expansion water stop strip 8 is a water-expandable expansion water stop strip with a width of 200 mm and a thickness of 10 mm; the bulk density of the alkali-resistant glass fiber mesh cloth 5 should be 160 g / m 2 , and the performance of alkali-resistant glass fiber mesh cloth 5 should meet the following characteristics: ① The nominal value of unit performance quality should be ≥160g / m 2 ; ② Its tensile breaking strength shall satisfy the requirements of warp breaking strength ≥1200N / 50mm, and weft breaking strength ≥1200N / 50mm; ③ The retention rate of alkali-resistant tensile breaking strength shall satisfy the requirements of warp alkali-resistant breaking strength retention rate ≥75%, and weft alkali-resistant breaking strength retention rate ≥75%; ④ The elongation at break shall satisfy the requirements of warp breaking elongation ≤4%, and weft breaking elongation ≤4%; ⑤ The combustible content shall be ≥12%; ⑥ The glass component ZrO2 shall be within the range of 14.5%±0.8%, and TiO2 shall be within the range of 6%±0.5%, which improves the tensile resistance and has a good water-stopping and leak-proof effect.
[0038] As a preferred embodiment, the fixing plate 6 is composed of a 2.5×28mm galvanized cement nail and a 20mm diameter galvanized gasket. The fixing plate is anchored into the wall 15-20mm and arranged in a matrix, with a horizontal and vertical spacing of 600mm.
[0039] As a preferred embodiment, in step S2, the full batch of polymer cement mortar 7 needs to be mixed with 5% cement-based modifier and enhancer, and the construction thickness of polymer cement mortar 7 is 15mm. Polymer cement mortar 7 should meet the following characteristics: ① The state in the container should be free of lumps and uniform; ② The construction should be smooth; ③ Drying time ≤ 5h; ④ The standard state of bonding strength ≥ 0.6Mpa; ⑤ The bonding strength freeze-thaw cycle (5 times) ≥ 0.4Mpa; ⑥ It should be manually polishable; ⑦ Alkali resistance (48h) is normal; ⑧ Water resistance (96h) is normal; ⑨ Flexibility should be 50mm in diameter without cracks.
[0040] As a preferred embodiment, in step S3, the model of the full batch of cement-based exterior wall putty should be R type; the fineness of the quick-drying agent is between 7.3-8.5, the alkali content is between 8.2-8.8, and the 28d compressive strength ratio (%) is between 72-78, which improves the construction effect and reduces the construction period. After two coats of the full batch of cement-based exterior wall putty, the first exterior wall putty layer 9 and the second exterior wall putty layer 10 are formed. The performance of the cement-based exterior wall putty should meet the following characteristics: ① The state in the container should be free of lumps and uniform; ② The construction should be smooth and barrier-free; ③ Drying time ≤5h; ④ Initial drying crack resistance (6h) without cracks; ⑤ It should be manually polishable.
[0041] As a preferred embodiment, in step S3, the putty should be polished with 240-mesh sandpaper after the putty is completely dry. The time for the putty to dry is 3-4 days in winter and 1-2 days in summer.
[0042] As a preferred embodiment, in step S4, the model of the base reinforcement sealing primer 11 is WDQ-C-1; the performance requirements are: ① There should be no lumps in the container and it should be in a uniform state after stirring; ② The construction should be smooth after two strokes; ③ The low temperature stability should not deteriorate; ④ The appearance of the coating is normal; ⑤ Drying time (surface dry) ≤2h; ⑥ Water resistance (96h) is normal; ⑦ Alkali resistance (48h) is normal; ⑧ Water permeability ≤0.3mL; ⑨ Anti-salt and alkali (120h) is normal.
[0043] As a preferred embodiment, in step S5, the waterproof decorative integrated coating adopts a ZGLM waterproof decorative integrated coating mixed with acrylic emulsion and special cement. The ZGLM waterproof decorative integrated coating has good flexibility and can resist slight cracking of the base layer, thereby improving the waterproof and leak-proof performance of the building. After drying, it can be directly plastered on the waterproof layer, leveled and various decorative tiles can be pasted with suitable tile adhesive; it has good anti-ultraviolet and anti-aging properties, and has long-term moisture-proof and waterproof effects; after rolling the waterproof decorative integrated coating twice on the outer surface of the sealing primer 11, a first waterproof decorative integrated coating layer 12 and a second waterproof decorative integrated coating layer 13 are formed; the performance of the waterproof decorative integrated coating should meet the following requirements: ① There should be no lumps in the container and it should be in a uniform state after stirring; ② The construction performance should be smooth after two scrapings; ③ Low temperature stability is not deteriorated; ④ The appearance of the coating is normal; ⑤ Drying time (surface dry) ≤ 2h; ⑥ Water resistance (96h) is normal; ⑦ Alkali resistance (48h) is normal; ⑧ Washability (2000 times) The paint film is not damaged.
[0044] As a preferred embodiment, in step S6, the finishing paint 14 is applied by roller coating. This construction method has the characteristics of high efficiency, low cost, fine surface treatment, good durability, controllable uniform thickness, and no paint mist. The performance of the finishing paint 14 should meet the following requirements: ① There should be no lumps after stirring in the container and it should be in a uniform state; ② The construction should be barrier-free; ③ Low temperature stability (3 cycles) without deterioration; ④ The appearance of the coating is normal; ⑤ Water resistance (96h) is normal; ⑥ Alkali resistance (48h) is normal; ⑦ Washability (2000 times) the paint film is not damaged; ⑧ Stain resistance ≤15%.
[0045] The green repair construction method for tile facades provided by the present invention avoids the practice of removing all the original tile surface layers in the conventional tile facade renovation, reduces the amount of facade renovation and demolition engineering, and shortens the construction period; it also reduces the construction waste generated during the construction process, and plays a certain positive role in the green environmental protection of the building facade renovation project. The waterproof decorative integrated coating has both waterproof and decorative functions. In the process of renovating the tile facades of existing buildings, compared with traditional practices, it can not only reduce the construction process, but also coordinately solve the renewal needs of waterproofing and decoration. In the early stage of construction, only hollow and cracked wall tiles are removed, and large-scale demolition is not carried out, which reduces the risk of falling objects during demolition, thereby enhancing construction safety. When the polymer cement mortar 7 is leveled, the alkali-resistant glass fiber mesh cloth 5 is pressed in and fixed with a fixing plate 6, which effectively increases the integrity of the repair base surface, thereby ensuring the construction quality of the repair of the tile facades of existing buildings, improving the service life of the building and ensuring safety in use.
[0046] Although the specific embodiments of the present invention are described and illustrated in detail above, it should be pointed out that: we can make various equivalent changes and modifications to the above embodiments based on the concept of the present invention, and the functional effects produced by them still do not exceed the spirit covered by the specification, and they should all be within the scope of protection of the present invention.
Claims
1. A green restoration construction method for urban tile facades, Features: Follow these steps: S1: Clean the existing building facade, repair the hollow and cracked areas of tiles and then level them; S2: After step S2, the outer surface of the wall is fully leveled with polymer cement mortar; S3: Apply two coats of cement-based exterior wall putty, add quick-drying agent to the putty to accelerate the drying and forming of the putty, and then grind the putty to make it smooth; S4: Then, a base reinforcement sealing primer is applied by roller coating on the outer surface of the putty after step S3; S5: Roller-coat the waterproof decorative integrated paint twice on the outer surface of the sealing primer; S6: Continue to roll on the topcoat over the waterproof decorative integrated paint to complete the wall repair.
2. A green restoration construction method for urban tile facades according to claim 1, Features: In step S1, the existing building facade includes the original building exterior wall base wall, the original building exterior wall brick mortar bonding layer and the original building exterior wall bricks arranged in sequence from the inside to the outside. The specific steps of step S1 are: Step S1.1: Find the hollow and cracked areas of the wall, then use a hand drill to remove them locally, remove the corresponding original building exterior wall tiles, and clean the original building exterior wall tile mortar bonding layer behind the original building exterior wall tiles; Step S1.2: Then brush cement mortar, remove the tiles formed at the repaired area, add an expansion water stop strip at the junction of the repaired area and the original building exterior wall tiles, press a layer of alkali-resistant glass fiber mesh cloth in the middle, and fix it with a fixing plate.
3. A green restoration construction method for urban tile facades according to claim 2, Features: The expansion water stop strip is a water-expandable water stop strip with a width of 200 mm and a thickness of 10 mm. The bulk density of the alkali-resistant glass fiber mesh cloth should be 160 g / m 2 , and the glass component ZrO in the alkali-resistant glass fiber mesh cloth 2 In the range of 14.5% ± 0.8%, TiO 2 Within the range of 6%±0.5%.
4. A green restoration construction method for urban tile facades according to claim 2, Features: The fixing plates are composed of 2.5×28mm galvanized cement nails and 20mm diameter galvanized washers. The fixing plates are anchored into the wall 15-20mm and arranged in a matrix, with horizontal and vertical spacing of 600mm.
5. A green restoration construction method for urban tile facades according to claim 1, It is characterized in that In step S2, the full batch of polymer cement mortar needs to be mixed with 5% cement-based modifier and enhancer, and the construction thickness of the polymer cement mortar is 15 mm.
6. A green restoration construction method for urban tile facades according to claim 1, Features: In step S3, the model of the full batch of cement-based exterior wall putty should be R type; the fineness of the quick-drying agent is between 7.3-8.5, the alkali content is between 8.2-8.8, and the 28d compressive strength ratio is between 72-78. After two coats of full batch of cement-based exterior wall putty, the first exterior wall putty layer and the second exterior wall putty layer are formed.
7. A green restoration construction method for urban tile facades according to claim 1, Features: In step S3, the putty should be polished with 240-mesh sandpaper after the putty is completely dry. The time for the putty to dry is 3-4 days in winter and 1-2 days in summer.
8. A green restoration construction method for urban tile facades according to claim 1, Features: In step S4, the model of the base reinforcement sealing primer is WDQ-C-1; the performance requirements are: water permeability ≤ 0.3mL, low temperature stability without deterioration, alkali resistance for 48h without abnormality; anti-salt and alkali resistance for 120h without abnormality.
9. A green restoration construction method for urban tile facades according to claim 1, Features: In step S5, the waterproof decorative integrated coating is a ZGLM waterproof decorative integrated coating made of a mixture of acrylic emulsion and special cement. The waterproof decorative integrated coating is rolled twice on the outer surface of the sealing primer to form a first waterproof decorative integrated coating layer and a second waterproof decorative integrated coating layer.
10. A green restoration construction method for urban tile facades according to claim 1, Features: In step S6, the finishing paint is applied by roller coating.
Citation Information
Patent Citations
Method for retreading old porcelain brick wall by paint
CN101586401A
Basement wall repairing structure
CN203066128U
Building exterior wall coating facing waterproof decoration layer structure
CN221119000U