Operation method of RCO device filled with integral VOCs oxidation catalyst
Through pre-operation in the RCO device, the gas to be treated is used to reduce the VOCs oxidation catalyst, which solves the problems of poor stability of the catalyst at high temperatures and limited precious metal resources, improves the catalyst activity and conversion rate, and achieves safe and efficient VOCs control. .
Patent Information
- Application Number
- CN202310382892.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-18
AI Technical Summary
Existing VOCs oxidation catalysts have poor stability at high temperatures, limited precious metal resources, and require high concentrations of hydrogen for activation, making it difficult to achieve in-situ activation, affecting catalyst activity and operational safety.
During the pre-operation of the RCO device, the gas to be treated is introduced under oxygen-poor and heated conditions to reduce the integral VOCs oxidation catalyst, improve the catalyst activity, and directly perform catalytic oxidation treatment, avoiding the use of high-concentration reducing gas and air Oxidation.
It improves the activity and conversion rate of the catalyst, reduces equipment investment and operational risks, extends the service life of the catalyst, and meets the demand for industrial VOCs degradation efficiency.
Smart Images

Figure CN118794028A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysts, and in particular relates to an operation method of an RCO device equipped with an integral VOCs oxidation catalyst. Background Art
[0002] As of 2020, more than 50% of cities in China still have excessive ambient air quality, of which PM2.5 and O3 are the primary pollutants accounting for more than 80%. Volatile organic compounds (hereinafter referred to as VOCs) are important precursors to the formation of PM2.5 and O3. We need to focus on winning the battle against ozone pollution. Focusing on industries such as petrochemicals, chemicals, coatings, pharmaceuticals, packaging and printing, and oil storage, transportation and marketing, we will safely and efficiently promote the comprehensive management of volatile organic compounds and implement source replacement projects for raw and auxiliary materials and products. By 2025, the total emissions of volatile organic compounds and other substances will drop by more than 10% compared to 2020. In order to further improve air quality, comprehensive management of key VOCs emission industries should be strengthened.
[0003] Catalytic combustion technology is an effective means of controlling low-concentration VOCs with large air volumes, and is the last resort for air pollution control. VOCs oxidation catalysts are generally composed of two parts: a carrier and an active component (precious metal). γ-Al2O3 has a high specific surface area and can maintain a stable crystal phase at 700-800°C. Therefore, γ-Al2O3 is generally used as a carrier for VOCs oxidation catalysts in industry. Precious metal catalysts have unsurpassed advantages over other catalysts. They have excellent catalytic oxidation performance and long service life. Under certain conditions, they can achieve a lower ignition temperature. However, precious metal resources are limited, expensive, and have poor stability at high temperatures. They are easy to volatilize and sinter during the preparation of supported catalysts. Therefore, improving the activity of VOCs catalysts by certain means is of great significance to reducing the amount of precious metals used and ensuring that VOCs emissions meet standards.
[0004] The document High Durable Metal Ensemble Catalysts with Full Dispersion for Automotive Applications Beyond Single-atom Catalysis, Nature Catalysis 20203(4)368-375 discloses that the prepared Pt / CeO2 catalyst and Pd / CeO2 catalyst are reduced by passing hydrogen (10% H2:N2) at 500°C to prepare an activated catalyst in which the precious metal is reduced. At the same time, the oxygen defect sites on the catalyst carrier are increased, which is beneficial to the adsorption and activation of oxygen. This method requires the use of hydrogen to activate the catalyst first, and then test the catalyst performance. It is impossible to achieve in-situ activation to achieve the purpose of improving activity. This method is difficult to implement, and the use of high hydrogen concentration is not conducive to operational safety. Summary of the invention
[0005] The object of the present invention is to provide an operating method of an RCO device equipped with an integral VOCs oxidation catalyst, which can conveniently and effectively improve the activity of the installed integral VOCs oxidation catalyst.
[0006] To achieve the purpose of the present invention, the following technical solutions are adopted:
[0007] A method for operating an RCO device equipped with an integral VOCs oxidation catalyst is to pre-operate the RCO device before formally starting the RCO device; the pre-operation is to introduce a gas to be treated into the RCO device under oxygen-deficient and heating conditions for pre-operation;
[0008] Wherein, the monolithic VOCs oxidation catalyst is a noble metal supported catalyst;
[0009] The gas to be treated is volatile organic gas.
[0010] Those skilled in the art understand that the gas to be treated is a volatile organic gas in the working condition of the integrated VOCs oxidation catalyst, such as the gas to be treated in the polyethylene project, which is the ethylene silo waste gas containing ethylene, and the exhaust gas containing methane in coal mining. In one embodiment, the total hydrocarbon content in the gas to be treated is 100-3500 mg / m 3 , for example 200 mg / m 3 , 500mg / m 3 , 1000mg / m 3 , 1500mg / m 3 , 2000mg / m 3 , 2500mg / m 3 and 3000mg / m3 .
[0011] Those skilled in the art understand that the monolithic VOCs oxidation catalyst can be prepared by conventional catalyst formulations and conventional methods, such as using Pt / Pd as active components and γ-Al2O3 as a carrier to prepare a honeycomb monolithic VOCs oxidation catalyst by an impregnation method. For example, the preparation process includes:
[0012] (1) Slurry preparation
[0013] Water, surfactant (polyethylene glycol / P123), binder (pseudo-boehmite / aluminum sol), salt solution of precious metal and powder (γ-Al2O3) raw materials are added to the reactor in sequence. Then the pH value is tested. If the test value is within the range of 2.8-4.0, the addition is stopped; if the pH value is too high, nitric acid is used to adjust the pH until the pH test value is within the above range; if the pH value is too low, urea is used to adjust the pH until the pH test value is within the above range; after completing the above steps, the slurry is stirred for 2.5 hours; wherein,
[0014] The mass ratio of water / surfactant / binder / alumina powder / precious metal is 69.9 / 0.1 / 6 / 25 / 0.15 (wherein the ratio of precious metal is calculated based on the mass of precious metal), and the precious metal accounts for 0.5% of the total solid content.
[0015] (2) Slurry ball milling
[0016] ①Continuous stirring: After the slurry raw materials are added, stirring is continued for 45 minutes at a stirring speed of 300r / min.
[0017] ② Ball milling: Use a ball mill to ball mill the slurry at a speed of 350r / min and a ball milling time of 1 hour.
[0018] (3) Coating
[0019] Target coating amount: 100 g / L (coating weight / carrier volume), of which the amount of precious metal used is 0.5 g / L.
[0020] Follow these steps to apply:
[0021] ① Place the empty carrier on a high-precision platform scale; ② Take the carrier and transfer it to the coating chamber; ③ Feed the slurry pump and return the material after reaching the set amount; ④ Take the carrier and transfer it to the purge chamber; ⑤ High-pressure purge the excess slurry; ⑥ Take the carrier and transfer it to the platform scale; ⑦ Until the solid coating amount reaches 100g / L;
[0022] (4) Calcination
[0023] The specific calcination curve is: the room temperature is increased to 200°C at a heating rate of 10°C / min and kept for 20 minutes, then the temperature is further increased to 400°C at a heating rate of 10°C / min and kept for 20 minutes, and finally the temperature is increased to 500°C and kept for 5-6 hours, and then the temperature is naturally cooled to room temperature to obtain an integral VOCs oxidation catalyst.
[0024] Those skilled in the art understand that, on the one hand, since the catalyst is placed in the air at room temperature during the interval between the completion of production and the installation and use, the highly dispersed precious metal Pt / Pd nanoparticles on the surface of the integral VOCs oxidation catalyst have high surface energy and easily adsorb oxygen in the air to form metal oxides, thereby reducing its catalytic activity; on the other hand, when the air humidity is high, moisture in the air will enter the catalyst pores, or be adsorbed on the catalyst interface to form bound water, which is not easy to remove and competes with VOCs molecules for adsorption, reducing the ability of VOCs molecules to adsorb on the catalyst interface to undergo oxidation reactions.
[0025] The operating method of the RCO device equipped with the integral VOCs oxidation catalyst of the present invention can directly reduce the installed integral VOCs oxidation catalyst by using the gas to be treated after installing the integral VOCs oxidation catalyst, thereby conveniently and effectively improving the activity of the installed integral VOCs oxidation catalyst, and the RCO device can be directly started after the activity is improved to catalytically oxidize the VOCs in the gas to be treated, improve the conversion rate of VOCs, and improve its conversion rate at the same temperature, thereby saving time and improving efficiency. Compared with the method of first improving the activity of the catalyst and then installing and operating it, the present invention does not need to provide corresponding processing equipment or activation procedures for improving the activity of the integral VOCs oxidation catalyst, but directly uses the RCO device for catalytic oxidation treatment of the gas to be treated, and directly uses the gas to be treated as the reducing gas to improve the activity of the integral VOCs oxidation catalyst, which is convenient, easy to operate, and saves equipment investment; on the other hand, the integral VOCs oxidation catalyst after the activity is improved is directly used, without a time interval in between, and there is no situation where it is partially deactivated by oxidation of oxygen in the air and adsorption of water vapor, which can ensure that the catalyst is used in the highest activity state after the activity is improved. In addition, in the present invention, the gas to be treated is used to activate the integral VOCs oxidation catalyst, which not only reduces the process of first activating and then loading, but also does not use high-concentration reducing gas, thereby improving operation safety.
[0026] In one embodiment, the operating temperature T of the pre-operation satisfies T 10 ≤T≤T 90 , such as T 15 、T 20 、T 25 、T 30 、T 35 、T40 、T 45 、T 50 、T 55 、T 60 、T 65 、T 70 、T 75 、T 80 and T 85 ; T is preferred 10 ≤T≤T 50 , such as T 15 、T 20 、T 25 、T 30 、T 35 、T 40 and T 45 .
[0027] Those skilled in the art understand that T 10 and T 50 They respectively represent the temperatures at which the main pollutants in the reaction atmosphere (gas to be treated) are catalytically converted by 10% and 50% on the fresh integral VOCs oxidation catalyst.
[0028] In one embodiment, the running time of the pre-run is 3-9 hours, such as 4 hours, 5 hours, 6 hours, 7 hours and 8 hours.
[0029] In one embodiment, during the pre-operation, the volume space velocity of the integrated VOCs oxidation catalyst is 1000-10000h -1 , for example 2000h -1 、3000h -1 , 4000h -1 , 5000h -1 、6000h -1 、7000h -1 、8000h -1 and 9000h -1 .
[0030] In one embodiment, the oxygen concentration in the pre-run is 0-5%, such as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% and 4.5%.
[0031] In one embodiment, the pre-operation includes a first stage and a second stage;
[0032] The operating temperature T1 of the first stage satisfies T 10 ≤T1≤T 20 , such as T 11 、T 12 、T 13 、T 14 、T15 、T 16 、T 17 、T 18 and T 19 ; and / or
[0033] The operating temperature T2 of the second stage satisfies T 20 ≤T2≤T 50 , such as T 25 、T 30 、T 35 、T 40 and T 45 .
[0034] In one embodiment, the running time of the first stage is 2-6 hours, such as 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours and 5.5 hours; and / or
[0035] The running time of the second stage is 1-3 hours, such as 1.5 hours, 2 hours and 2.5 hours.
[0036] In one embodiment, the oxygen concentration in the first stage is 0-2%, such as 0.5%, 1% and 1.5%; and / or
[0037] The oxygen concentration in the second stage is 0-5%, such as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% and 4.5%; and / or
[0038] In the first stage, the volume space velocity of the integral VOCs oxidation catalyst is 1000-10000h -1 , for example 2000h -1 、3000h -1 , 4000h -1 , 5000h -1 、6000h -1 、7000h -1 、8000h -1 , and 9000h -1 ; and / or
[0039] In the second stage, the volume space velocity of the integral VOCs oxidation catalyst is 1000-10000h -1 , for example 2000h -1 、3000h -1 , 4000h -1 , 5000h -1 、6000h -1 、7000h -1 、8000h -1 , and 9000h -1 .
[0040] In one embodiment, the precious metal in the integrated VOCs oxidation catalyst includes any one or more combinations of platinum, palladium, rhodium, gold, and ruthenium.
[0041] In one embodiment, the installed integral VOCs oxidation catalyst is a fresh catalyst, that is, a catalyst that has not been used after preparation.
[0042] The present invention performs a pre-operation before officially starting the RCO device to heat the installed integral VOCs oxidation catalyst for activation, which can avoid the situation where the activated integral VOCs oxidation catalyst loses part of its activity after being placed in air at room temperature for a long time, resulting in reduced activity. This is convenient and efficient, and can maximize the development and utilization of the active sites of the catalyst.
[0043] The beneficial effects of the present invention are:
[0044] The operating method of the RCO device equipped with the monolithic VOCs oxidation catalyst of the present invention can maximize the utilization of the precious metal atoms of the monolithic VOCs oxidation catalyst and meet the industrial VOCs degradation efficiency requirements;
[0045] The catalyst is activated by the gas to be treated, which reduces the process of activation before loading, does not use high-concentration reducing gas, and improves operation safety.
[0046] Through the heating activation during the first run, more catalytic active sites are exposed, which stimulates and enhances the low-temperature activity potential of the fresh catalyst, ensuring that VOCs treatment meets the standards without increasing the precious metal content of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 is a comparison chart of the catalytic oxidation performance of the monolithic platinum-based VOCs oxidation catalyst before and after activation described in Example 1;
[0048] Figure 2 This is a comparison chart of the catalytic oxidation performance of the integral palladium-based VOCs oxidation catalyst described in Example 2 before and after activation. DETAILED DESCRIPTION
[0049] The technical scheme and its effects of the present invention are further described below in conjunction with specific implementation methods / examples. The following implementation methods / examples are only used to illustrate the content of the present invention, and the invention is not limited to the following implementation methods or examples. Simple changes made to the present invention using the concept of the present invention are all within the scope of protection claimed by the present invention.
[0050] The main raw materials and instruments used in the following examples and comparative examples are from the following sources:
[0051] Polyethylene glycol 400, industrial grade, Shanghai Aladdin;
[0052] Pseudoboehmite, Sasol, P 2, in which the Al2O3 content is 72%;
[0053] Platinum nitrate, containing 15wt% platinum, Shanghai Jiuling Chemical Co., Ltd.;
[0054] Palladium nitrate, containing 15wt% palladium, Shanghai Jiuling Chemical Co., Ltd.;
[0055] γ-Al2O3 powder, Aluminum Corporation of China
[0056] pH tester, Mettler Toledo specification is SevenDirect SD20 HA Kit.
[0057] Example 1 (S1)
[0058] (I) Preparation of monolithic platinum-based VOCs oxidation catalyst 1; the specific process is as follows:
[0059] (1) Slurry preparation
[0060] Water, surfactant (polyethylene glycol 400), binder (pseudo-boehmite), precious metal solution (platinum nitrate solution with a concentration of 15wt% Pt, that is, the concentration of platinum nitrate solution is 15wt% based on platinum element) and powder (γ-Al2O3) raw materials are added to the reactor in sequence. Then the pH value is tested. If the test value is within the range of 2.8 to 4.0, the addition is stopped; if the pH value is too high, nitric acid is used to adjust the pH until the pH test value is within the above range; if the pH value is too low, urea is used to adjust the pH until the pH test value is within the above range; after completing the above steps, the slurry is stirred for 2.5 hours; wherein,
[0061] The mass ratio of water / surfactant / binder / alumina powder / precious metal is 69.9 / 0.1 / 6 / 25 / 0.15 (wherein the ratio of precious metal is calculated based on the mass of precious metal), and the precious metal accounts for 0.5% of the total solid content.
[0062] (2) Slurry ball milling
[0063] ①Continuous stirring: After the slurry raw materials are added, stirring is continued for 45 minutes at a stirring speed of 300r / min.
[0064] ② Ball milling: Use a ball mill to ball mill the slurry at a speed of 350r / min and a ball milling time of 1 hour.
[0065] (3) Coating
[0066] Target coating amount: 100 g / L (coating weight / carrier volume), of which the amount of precious metal used is 0.5 g / L.
[0067] Follow these steps to apply:
[0068] ① Place the empty carrier on a high-precision platform scale; ② Take the carrier and transfer it to the coating chamber; ③ Feed the slurry pump and return the material after reaching the set amount; ④ Take the carrier and transfer it to the purge chamber; ⑤ High-pressure purge the excess slurry; ⑥ Take the carrier and transfer it to the platform scale; ⑦ Until the solid coating amount reaches 100g / L;
[0069] (4) Calcination
[0070] The specific calcination curve is: the room temperature is increased to 200°C at a heating rate of 10°C / min and kept for 20 minutes, then the temperature is further increased to 400°C at a heating rate of 10°C / min and kept for 20 minutes, and finally the temperature is increased to 500°C and kept for 5-6 hours, and then the temperature is naturally cooled to room temperature to obtain an integral platinum-based VOCs oxidation catalyst 1.
[0071] (ii) installing the integrated platinum-based VOCs oxidation catalyst 1 obtained in step (i) in an RCO device;
[0072] (III) The RCO device equipped with the integral platinum-based VOCs oxidation catalyst 1 was pre-operated as follows: 50 , satisfying T 10 ≤T≤T 50 ) is introduced into the RCO device under the conditions of: 3 ) for pre-operation, and the volume space velocity of the integral platinum-based VOCs oxidation catalyst 1 is 5000h -1 ; Obtaining an activated integral platinum-based VOCs oxidation catalyst 1 ';
[0073] (IV) Formal startup of the RCO device and treatment of the aforementioned gas to be treated under the following operating conditions; wherein the water content of the operating conditions is 5wt%, and the volume space velocity of the monolithic platinum-based VOCs oxidation catalyst 1' is 40000h -1 , the treatment temperature is 150℃;
[0074] The degradation efficiency of ethylene was 83%.
[0075] Comparative Example 1 (D1)
[0076] The only difference from Example 1 (S1) is that step (iii) is not performed, and after step (ii) is performed, the processing of step (iv) is directly started;
[0077] The degradation efficiency of ethylene is 50%.
[0078] Comparative Example 2 (D2)
[0079] The only differences from Comparative Example 1 (D1) are as follows:
[0080] The treatment temperature in step (iv) is 170° C. and the degradation efficiency of ethylene is 83%.
[0081] The catalytic oxidation performance of the integrated platinum-based VOCs oxidation catalyst 1' after heating activation in Example 1 (S1) and the fresh integrated platinum-based VOCs oxidation catalyst 1 without heating activation in Comparative Example 1 (D1) is shown in FIG. Figure 1 .
[0082] Figure 1 In the present invention, the activated integral platinum-based VOCs oxidation catalyst 1' and the fresh integral platinum-based VOCs oxidation catalyst 1 are used to catalyze the oxidation of ethylene (ethylene silo tail gas) to generate carbon dioxide and water, and the conversion rate of ethylene at different reaction temperatures (50-300°C) is detected. The reaction conditions are: the space velocity is 40000h -1 The raw gas used had an oxygen concentration of 20 vol% and an initial ethylene concentration of 800 mg / m 3 , and the rest is nitrogen. Figure 1 It can be seen that when the unactivated fresh integral platinum-based VOCs oxidation catalyst 1 is used, the ethylene conversion rate reaches 10% at 130°C (T 10 ), at 150℃, it reaches 50% (T 50 ), at 225℃, it reaches 90% (T 90 ); When the activated integral platinum-based VOCs oxidation catalyst 1' is used, the ethylene conversion rate can reach 10% at 110°C (T 10 ), 20℃ lower than before activation; 50% (T 50 ), 20℃ lower than before activation; 90% (T 90 ), which was 47°C lower than that before activation.
[0083] According to the comparison between Example 1 (S1) and Comparative Example 1 (D1), under the same working conditions (i.e., the working water content is 5wt%, the volume space velocity of the integral platinum-based VOCs oxidation catalyst 1' is 40000h -1 , the treatment temperature is 150° C.), compared with the fresh integral platinum-based VOCs oxidation catalyst 1 that has not been heated and activated in comparative example 1 (D1), the integral platinum-based VOCs oxidation catalyst 1' that has been heated and activated in example 1 (S1) of the present application has an ethylene degradation efficiency (i.e., conversion rate) increased by 33%;
[0084] According to the comparison between Example 1 (S1) and Comparative Example 2 (D2), when other working conditions are the same and the degradation efficiency (i.e., conversion rate) of ethylene is also 83%, the treatment temperature in Comparative Example 2 (D2) is increased to 170°C, while the treatment temperature in Example 1 (S1) is only 150°C, which is equivalent to Comparative Example 2 (D2), which reduces the reaction temperature by 20°C.
[0085] Taking the 300,000 ton / year polyethylene project as an example, the waste gas from the ethylene silo that needs to be treated is 70,000 Nm 3 / h, the annual processing volume (calculated as 300 days) is about 500 million standard cubic meters of tail gas. A 20°C reduction in reaction temperature is equivalent to saving about 3.3 million standard cubic meters of natural gas.
[0086] Embodiment 2 (S2)
[0087] The only difference from Example 1 is:
[0088] In step (i), the noble metal solution is a palladium nitrate solution with a concentration of 15 wt% Pd (i.e., the concentration of the palladium nitrate solution is 15 wt% based on the palladium element); the prepared product is a monolithic palladium-based VOCs oxidation catalyst 2;
[0089] In step (ii), the integral VOCs palladium-based oxidation catalyst 2 obtained in step (i) is installed in the RCO device;
[0090] In step (iii), the RCO device equipped with the integral palladium-based VOCs oxidation catalyst 2 is pre-operated as follows: the gas to be treated (lack of air gas in coal mining, the main organic gas component of which is methane, the content of which is 1300 mg / m 3 ) to perform a pre-operation, the pre-operation comprising a first stage and a second stage; wherein,
[0091] In the first stage, the operating temperature T1 = 320°C (T 12 , satisfying T 10 ≤T1≤T 20 ); the running time is 3h; the oxygen concentration is 0%; the volume space velocity of the monolithic palladium-based VOCs oxidation catalyst is 2000h -1 ;
[0092] In the second stage, the operating temperature T2 = 350°C (T 40 , satisfying T 20 ≤T2≤T 50 ); operating time is 3h; oxygen concentration is 0.5%; the volume space velocity of the monolithic palladium-based VOCs oxidation catalyst is 10000h -1 ;
[0093] Obtaining an activated integral palladium-based VOCs oxidation catalyst 2';
[0094] (iv) formally starting the RCO device and treating the aforementioned gas to be treated under the following working conditions; wherein:
[0095] The water content of the working condition is 5wt%, and the volume space velocity of the integral palladium-based VOCs oxidation catalyst 2' is 40000h -1 , the treatment temperature is 500℃;
[0096] The methane degradation efficiency is 90%.
[0097] Comparative Example 3 (D3)
[0098] The only difference from Example 2 (S2) is that step (iii) is not performed, and after step (ii) is performed, the processing of step (iv) is directly started;
[0099] The methane degradation efficiency is 75%.
[0100] Comparative Example 4 (D4)
[0101] The only differences from Comparative Example 3 (D3) are as follows:
[0102] The treatment temperature in step (iv) is 550° C. and the degradation efficiency of ethylene is 80%.
[0103] The catalytic oxidation performance of the integrated palladium-based VOCs oxidation catalyst 2' after heating activation in Example 2 (S2) is compared with the fresh integrated palladium-based VOCs oxidation catalyst 2 without heating activation in Comparative Example 3 (D3). Figure 2 .
[0104] Figure 2 In the present invention, the activated integral palladium-based VOCs oxidation catalyst 2' and the fresh integral palladium-based VOCs oxidation catalyst 2 are used to catalytically oxidize methane (lack of air gas produced in coal mining) to generate carbon dioxide and water, and the conversion rate of methane at different reaction temperatures (100-550°C) is detected. The reaction conditions are: the space velocity is 40000h -1 The raw gas used had an oxygen concentration of 20 vol% and an initial methane concentration of 1300 mg / m 3 , and the rest is nitrogen. Figure 2 It can be seen that when using the unactivated fresh integral palladium-based VOCs oxidation catalyst 2, the conversion rate of methane reaches 10% at 310°C (T 10 ), at 330℃, it reaches 20% (T 20 ), at 370℃, it reaches 50% (T 50 ), reaches 75% at 500℃ (T75 ), reaches 80% at 550℃ (T 80 ); When the activated integral palladium-based VOCs oxidation catalyst 2' is used, the conversion rate of methane can reach 10% at 300°C (T 10 ), compared with the unactivated state, the temperature is reduced by 10℃; at 310℃, it can reach 20% (T 20 ), 20℃ lower than before activation; 50% (T 50 ), 30℃ lower than before activation; 90% (T 90 ), the treatment temperature is reduced by far more than 50°C compared to before activation.
[0105] According to the comparison between Example 2 (S2) and Comparative Example 3 (D3), under the same working conditions (working condition water content is 5wt%, volume space velocity is 40000h -1 , the treatment temperature is 500° C.), compared with the fresh integral palladium-based VOCs oxidation catalyst 2 that has not been heated and activated in Comparative Example 3 (D3), the degradation efficiency (i.e., conversion rate) of the integral palladium-based VOCs oxidation catalyst 2' after heating and activation in Example 2 (S2) of the present application for methane is increased by 15%;
[0106] According to the comparison between Example 2 (S2) and Comparative Example 4 (D4), even if the treatment temperature in Comparative Example 4 (D4) is increased to 550°C, its degradation efficiency (i.e., conversion rate) for methane can only reach 80%; if the degradation efficiency (i.e., conversion rate) for methane is to reach 90%, the treatment temperature must be much higher than 550°C; and the treatment temperature in Example 2 (S2) is only 500°C, and its degradation efficiency (i.e., conversion rate) for methane can reach 90%; equivalent to Comparative Example 4 (D4), Example 2 (S2) reduces the reaction temperature by more than 50°C.
[0107] Taking coal mining as an example, the scale of the lack of air gas that needs to be treated is 100000Nm 3 / h, the annual processing volume (calculated as 300 days) is about 700 million standard cubic meters of tail gas. A 50°C reduction in reaction temperature is equivalent to saving about 5 million standard cubic meters of natural gas. In addition, the higher processing temperature increases the equipment maintenance cost, accelerates the aging of the catalyst, and reduces the service life of the catalyst.
Claims
1. A method for operating an RCO device equipped with an integral VOCs oxidation catalyst, characterized in that: The operation method is to pre-operate the RCO device before formally starting it; the pre-operation is to introduce the gas to be treated into the RCO device under oxygen-deficient and heated conditions for pre-operation; Wherein, the monolithic VOCs oxidation catalyst is a noble metal supported catalyst; The gas to be treated is volatile organic gas.
2. The operating method according to claim 1, characterized in that: The operating temperature T of the pre-operation satisfies T 10 ≤T≤T 90 Preferably, T 10 ≤T≤T 50 .
3. The operating method according to claim 1 or 2, characterized in that: The running time of the pre-run is 3-9h.
4. The operating method according to any one of claims 1 to 3, characterized in that: During the pre-operation, the volume space velocity of the integrated VOCs oxidation catalyst is 1000-10000h -1 .
5. The operating method according to any one of claims 1 to 4, characterized in that: The oxygen concentration of the pre-run is 0-5%.
6. The operating method according to any one of claims 1 to 5, characterized in that: The pre-operation includes a first stage and a second stage; The operating temperature T1 of the first stage satisfies T 10 ≤T1≤T 20 ; and / or The operating temperature T2 of the second stage satisfies T 20 ≤T2≤T 50 .
7. The operating method according to claim 6, characterized in that: The running time of the first stage is 2-6 hours; and / or The running time of the second stage is 1-3h.
8. The operating method according to claim 6 or 7, characterized in that: The oxygen concentration in the first stage is 0-2%; and / or The oxygen concentration in the second stage is 0-5%.
9. The operating method according to any one of claims 6 to 8, characterized in that: In the first stage, the volume space velocity of the integral VOCs oxidation catalyst is 1000-10000h -1 ; and / or In the second stage, the volume space velocity of the integral VOCs oxidation catalyst is 1000-10000h -1 .