Thin film resistor and preparation method thereof
Through wet photolithography process and low-temperature electron beam evaporation technology, the phase change problem of thin film resistors during high-temperature etching process is solved, the preparation stability and the reliability of the resistor are improved, and the conductive performance is optimized.
Patent Information
- Application Number
- CN202410836150.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-18
AI Technical Summary
High-temperature etching during the preparation process of traditional thin-film resistors causes phase transformation of tantalum nitride thin-film resistors, causing damage and reduced reliability.
The wet photolithography process is used to replace high-temperature etching. By depositing a dielectric layer and a tantalum nitride resistance layer on the substrate, magnetron sputtering and low-temperature electron beam evaporation processes are used to form the resistance layer, and rapid thermal annealing is performed to adjust nitrogen and protect gas ratio to optimize conductive properties.
The stability of the preparation process is improved, the phase change of the thin film resistor in the high-temperature etching cavity is avoided, the reliability and conductive performance of the resistor are enhanced, and energy loss is reduced.
Smart Images

Figure CN118800539A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of electronic component preparation, and specifically relates to a thin film resistor and a preparation method thereof. Background Art
[0002] In recent years, the rapid development of electronic information technology has continuously put forward new requirements for electronic component technology, and resistor technology has also been developed in a new way, from traditional wire wound resistors, metal film resistors, graphite resistors and chip thick film resistors to the current thin film resistors. Tantalum nitride (TaNx 0.1≤x≤1.25, abbreviated as TaN) resistors are now widely used in microelectronics, power machinery, aerospace and other fields because of their high precision and stable resistance value, high hardness, good wear resistance, low noise, good temperature stability and relatively high power level processing.
[0003] However, in the traditional preparation process, the tantalum nitride thin film resistor is etched by a high-temperature etcher, which causes the thin film resistor to undergo phase change in the high-temperature etching chamber, causing damage to the thin film resistor, resulting in poor reliability or even loss of function of the tantalum nitride thin film resistor. Therefore, how to avoid phase change during the preparation process of the thin film resistor, which causes damage or defects to the thin film resistor, is an urgent problem to be solved. Summary of the invention
[0004] The present application provides a thin film resistor and a method for preparing the same, which can prevent the thin film resistor from undergoing phase change during the preparation process, thereby preventing damage or defects, and has high reliability.
[0005] In order to solve the above technical problems, in a first aspect, the present application provides a method for preparing a thin film resistor, the method comprising the following steps:
[0006] Depositing a dielectric layer on a substrate, and providing a first photoresist layer on the dielectric layer;
[0007] Removing a portion of the first photoresist to expose the first region of the dielectric layer;
[0008] forming a tantalum nitride resistance layer on the first photoresist layer by magnetron sputtering;
[0009] Stripping the first photoresist layer and the tantalum nitride resistor layer formed on the first photoresist layer, and retaining the tantalum nitride resistor layer formed in the first region;
[0010] Disposing a second photoresist layer on the dielectric layer and the tantalum nitride resistance layer;
[0011] Removing a portion of the second photoresist to expose the second region of the dielectric layer and an adjacent region of the tantalum nitride resistance layer;
[0012] Depositing a metal layer on the dielectric layer and the tantalum nitride resistance layer;
[0013] The second photoresist layer and the metal layer formed on the second photoresist layer are stripped off, and the metal layer formed in the second region and the adjacent region is retained.
[0014] As a further improvement of the present application, the step of performing magnetron sputtering on the first photoresist layer to form a tantalum nitride resistance layer includes:
[0015] Using metal tantalum as a target material and nitrogen as a reaction gas, the metal tantalum target material is bombarded by magnetron sputtering in a mixed gas of nitrogen and a protective gas to form the tantalum nitride resistance layer on the first photoresist layer.
[0016] As a further improvement of the present application, the first region and the second region are provided on a side of the dielectric layer facing away from the substrate;
[0017] The first region includes a plurality of first sub-regions arranged along a first direction, the second region includes a plurality of second sub-regions arranged along the first direction, a plurality of the first sub-regions and the second sub-regions are alternately arranged along the first direction, and the first sub-region is connected to an adjacent second sub-region.
[0018] As a further improvement of the present application, the adjacent region is provided on a side of the tantalum nitride resistance layer facing away from the dielectric layer;
[0019] The adjacent region includes a plurality of adjacent sub-regions arranged along a first direction, and the second sub-region is connected to the adjacent adjacent sub-regions.
[0020] As a further improvement of the present application, the step of depositing a metal layer on the dielectric layer and the tantalum nitride resistance layer comprises:
[0021] A metal layer is deposited on the dielectric layer and the tantalum nitride resistor layer using a low-temperature electron beam evaporation process; wherein the temperature of the electron beam evaporation process is 25-40 degrees Celsius, and the thickness of the second photoresist layer is greater than the thickness of the metal layer.
[0022] As a further improvement of the present application, the thickness of the second photoresist layer is greater than or equal to three times the thickness of the metal layer.
[0023] As a further improvement of the present application, after stripping the second photoresist layer and the metal layer formed on the second photoresist layer, the method further includes:
[0024] In a vacuum argon environment, rapid thermal annealing is performed on the retained substrate, the dielectric layer, the tantalum nitride resistor layer and the metal layer; wherein the time of the rapid thermal annealing does not exceed 30 minutes.
[0025] As a further improvement of the present application, the step of depositing a dielectric layer on a substrate includes:
[0026] A SiO2 dielectric layer is deposited on the substrate by a plasma enhanced chemical vapor deposition process; wherein the thickness of the SiO2 dielectric layer is 1.5 microns.
[0027] As a further improvement of the present application, the first photoresist layer and the tantalum nitride resistor layer formed on the first photoresist layer are stripped by a wet stripping process;
[0028] And, the second photoresist layer and the metal layer formed on the second photoresist layer are stripped by a wet stripping process.
[0029] In a second aspect, the present application provides a thin film resistor, the thin film resistor comprising:
[0030] substrate;
[0031] A dielectric layer is disposed on the substrate;
[0032] A tantalum nitride resistor layer is disposed in a first region on the substrate;
[0033] The metal layer is arranged in the second area on the substrate and in the adjacent area on the tantalum nitride resistor layer. The tantalum nitride resistor layer is connected to the metal layer, and the thickness of the metal layer is greater than the thickness of the tantalum nitride resistor layer.
[0034] The thin film resistor and the preparation method thereof provided in the present application have the following beneficial effects:
[0035] The present application deposits a dielectric layer on a substrate, arranges a first photoresist on the dielectric layer, removes the first photoresist in a partial area through exposure, pre-baking, developing, and post-baking steps, and exposes the first area of the dielectric layer, forms a tantalum nitride resistor layer on the first photoresist layer by magnetron sputtering, removes the first photoresist layer and the tantalum nitride resistor layer formed on the first photoresist layer through a wet stripping process, continues to arrange a second photoresist layer on the dielectric layer and the tantalum nitride resistor layer, and similarly removes the second photoresist in a partial area through exposure, pre-baking, developing, and post-baking steps. The present application replaces the traditional high temperature photolithography process with a wet photolithography process. The etching process avoids the phase change of the thin film resistor in the high-temperature etching chamber, improves the stability of the preparation process, and avoids defects and damage to the thin film resistor during the preparation process; during the preparation process, the conductive properties of the tantalum nitride thin film resistor can be effectively adjusted by adjusting the ratio between nitrogen and protective gas; the thin film resistor that has completed two wet photolithography processes is subjected to rapid thermal annealing treatment to reduce the contact resistance formed between the metal layer and the tantalum nitride resistor layer, which can reduce the energy loss generated by the current in the thin film resistor and effectively improve the conductive properties and reliability of the thin film resistor. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only part of the embodiments of the present application, rather than all the embodiments. For ordinary technicians in this field, without paying creative work, other drawings obtained based on these drawings all fall within the scope of protection of this application.
[0037] Figure 1 A flow chart of a method for preparing a thin film resistor provided in an embodiment of the present application;
[0038] Figure 2 for Figure 1 A schematic diagram of the structure of a substrate in the method for preparing a thin film resistor is shown;
[0039] Figure 3 for Figure 1 A schematic diagram of the structure of a deposited dielectric layer in a method for preparing a thin film resistor is shown;
[0040] Figure 4 for Figure 1 A schematic diagram of the structure of spin coating the first photoresist layer in the method for preparing a thin film resistor;
[0041] Figure 5 for Figure 1 A schematic structural diagram of removing a portion of the first photoresist in the thin film resistor manufacturing method shown;
[0042] Figure 6 for Figure 1 A schematic diagram of the structure of a tantalum nitride resistor layer formed by magnetron sputtering in a method for preparing a thin film resistor is shown;
[0043] Figure 7 for Figure 1 A schematic diagram of the structure of stripping the first photoresist layer in the method for preparing a thin film resistor;
[0044] Figure 8 for Figure 1 A schematic diagram of the structure of spin coating the second photoresist layer in the method for preparing the thin film resistor shown;
[0045] Fig. 9 for Figure 1 A schematic diagram of a structure in which a portion of the second photoresist is removed in the method for preparing a thin film resistor;
[0046] Fig.10 for Figure 1 A schematic diagram of the structure of depositing a metal layer in a method for preparing a thin film resistor is shown;
[0047] Fig.11 for Figure 1 A schematic diagram of the structure of stripping the second photoresist layer in the thin film resistor manufacturing method shown;
[0048] Description of reference numerals:
[0049] 1-substrate; 2-dielectric layer; 21-first region; 211-first sub-region; 22-second region; 221-second sub-region; 23-edge region; 3-first photoresist layer; 4-tantalum nitride resistor layer; 41-adjacent region; 411-adjacent sub-region; 5-second photoresist layer; 6-metal layer. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0051] In order to make the description of the disclosed content more detailed and complete, the following is an illustrative description of the implementation methods and specific examples of the present application; however, this is not the only form of implementing or applying the specific embodiments of the present application. The implementation methods cover the features of multiple specific embodiments and the method steps and their sequences for constructing and operating these specific embodiments. However, other specific embodiments can also be used to achieve the same or equal functions and step sequences. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0052] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the numbers used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein.
[0053] In the description of the embodiments of the present application, unless otherwise specified, " / " means or, for example, A / B can mean A or B; "and / or" in the text is merely a description of the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. In addition, in the description of the embodiments of the present application, "multiple" refers to two or more than two, and other quantifiers are similar. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present application, and are not used to limit the present application, and the embodiments of the present application and the features in the embodiments may be combined with each other without conflict.
[0054] Please refer to Figure 1-Figure 11 The present application provides a thin film resistor and a method for preparing the same, which can avoid phase change of the thin film resistor during the preparation process, causing damage or defects, has high reliability, and improves the manufacturing yield of the thin film resistor.
[0055] Please refer to Figure 1 , is a flow chart of a method for preparing a thin film resistor provided in an embodiment of the present application, the method comprising the following steps:
[0056] Step S1: depositing a dielectric layer 2 on a substrate 1, and providing a first photoresist layer 3 on the dielectric layer 2;
[0057] As an optional implementation, the above-mentioned substrate 1 can be set to any substrate form of a silicon wafer substrate, a glass substrate, a ceramic substrate, and a diamond substrate. The above are all feasible, and this application does not further limit the specific setting form of the substrate 1.
[0058] Please refer to Figure 2 ,for Figure 1 The schematic diagram of the structure of the substrate 1 in the thin film resistor preparation method is shown. In the present application, the substrate 1 is preferably set to be in the form of a silicon wafer substrate.
[0059] As an optional implementation, the above-mentioned step of depositing the dielectric layer 2 on the substrate 1 includes:
[0060] The SiO2 dielectric layer 2 is deposited on the substrate 1 by chemical vapor deposition process or physical vapor deposition process.
[0061] In the embodiment of the present application, the substrate 1 can be set as a silicon wafer substrate, the silicon wafer substrate is insulated, and the SiO2 dielectric layer 2 is deposited on the silicon wafer substrate by CVD (Chemical Vapor Deposition) and PVD (Physical Vapor Deposition) processes; wherein, the physical vapor deposition process refers to a process in which a material is vaporized into atoms, molecules or ionized into ions by physical methods under vacuum conditions, and a layer with certain special properties is deposited on the surface of the material or substrate through a gas phase process; the chemical vapor deposition process mainly utilizes one or several gas phase compounds or single substances containing thin film elements to chemically react on the surface of the substrate to generate a thin film.
[0062] Please refer to Figure 3 ,for Figure 1 The schematic diagram of the structure of the deposited dielectric layer 2 in the thin film resistor preparation method shown in the figure, the present application preferably deposits a SiO2 dielectric layer 2 of a preset thickness on the substrate 1 by a PECVD (Plasma Enhanced Chemical Vapor Deposition) process. Among them, the plasma enhanced chemical vapor deposition process is a method for preparing semiconductor thin film materials and other material films by chemically reacting and depositing them on a substrate after ionizing them by glow discharge in a deposition chamber. The activity of chemical vapor reaction substances is enhanced by plasma activation, the surface reaction rate is increased, and the film deposition temperature is significantly reduced by high-energy ions, which has the advantages of low deposition temperature and fast deposition rate.
[0063] In the embodiment of the present application, the thickness of the above-mentioned substrate 1 is preferably set to 650-700 microns, the substrate 1 is set to a 6-inch silicon wafer, the crystal phase is set to (100), the flat edge (Flat) of the silicon wafer is set to 57.5 mm, and the thickness of the SiO2 dielectric layer 2 is set to 1.5 microns. Of course, it is also feasible to set the above-mentioned substrate 1 and dielectric layer 2 to other thicknesses and forms, and the present application does not impose further restrictions on this.
[0064] Of course, the above methods of preparing the dielectric layer 2 by either physical vapor deposition or chemical vapor deposition are all feasible. In principle, as long as a dense dielectric layer 2 with a uniform preset thickness can be prepared on the substrate 1, any preparation method selected is feasible, and technical personnel in this field should be aware of this.
[0065] For further information, please refer to Figure 4 ,for Figure 1The schematic diagram of the structure of spin coating the first photoresist layer 3 in the thin film resistor preparation method shown in the figure, after depositing a SiO2 dielectric layer 2 of a preset thickness on a silicon wafer substrate, the present application further requires spin coating photoresist on the dielectric layer 2 to form a first photoresist layer 3 on the dielectric layer 2.
[0066] Step S2: removing the first photoresist in a partial area to expose the first area 21 of the dielectric layer 2;
[0067] Please refer to Figure 5 ,for Figure 1 The schematic diagram of the structure in which part of the first photoresist is removed in the method for preparing a thin film resistor is shown. In the present application, a first region 21, a second region 22 and an edge region 23 are arranged on the side of the dielectric layer 2 facing away from the substrate 1. It can be observed that the first region 21 includes a plurality of first sub-regions 211 arranged along the first direction, the second region 22 includes a plurality of second sub-regions 221 arranged along the first direction, and the first sub-regions 211 and the second sub-regions 221 are alternately arranged, and the first sub-region 211 is connected to the adjacent second sub-region 221, that is, there is no gap between the first sub-region 211 and the second sub-region 221.
[0068] For further information, please refer to Figure 7 ,for Figure 1 The schematic diagram of the structure of stripping the first photoresist layer 3 in the thin film resistor preparation method shown in the figure, the present application provides edge regions 23 at both ends of the dielectric layer 2 facing away from the substrate 1, and the above-mentioned multiple first sub-regions 211 and second sub-regions 221 are alternately arranged between the two edge regions 23, while satisfying the positional relationship of the alternating arrangement of the first sub-regions 211 and the second sub-regions 221.
[0069] In the embodiment of the present application, the second sub-region 221 is disposed in connection with the adjacent edge region 23 , the first sub-region 211 is disposed in connection with the adjacent second sub-region 221 , and so on, the first region 21 and the second region 22 are alternately disposed between the two edge regions 23 .
[0070] In a specific embodiment provided in this application, please continue to refer to Figure 5 and Figure 7In the present application, two first sub-regions 211, three second sub-regions 221 and two edge regions 23 are arranged on the side of the dielectric layer 2 facing away from the substrate 1. It can be observed that in the present application, the two edge regions 23 are arranged at the opposite ends of the side of the dielectric layer 2 facing away from the substrate 1, two of the second sub-regions 221 are arranged adjacent to the two edge regions 23, two first sub-regions 211 are arranged adjacent to the two second sub-regions 221, and the remaining second sub-region 221 is arranged between the two first sub-regions 211. At this time, the dielectric layer 2 facing away from the substrate 1 is arranged with the edge region 23, the second sub-region 221, the first sub-region 211, the second sub-region 221, the first sub-region 211, the second sub-region 221 and the edge region 23 arranged in sequence along the first direction. Those skilled in the art should be aware of the arrangement of the above-mentioned edge regions 23, the first region 21 and the second region 22.
[0071] Of course, in practice, more first sub-regions 211 and second sub-regions 221 may be provided, but in principle, the first sub-regions 211 and the second sub-regions 221 should be alternately provided, and the positional relationship of the second sub-region 221 adjacent to the edge region 23 should be satisfied.
[0072] It can be understood that the present application does not further limit the specific number of the above-mentioned first sub-areas 211 and the second sub-areas 221, and does not elaborate on the arrangement of different numbers of first sub-areas 211 and second sub-areas 221. In principle, it is required that a number of first sub-areas 211 and a number of second sub-areas 221 are alternately arranged between two edge areas 23, and the second sub-area 221 is arranged adjacent to the edge area 23. The present application does not elaborate on this.
[0073] It should be noted that, since the specific widths of the first sub-region 211 and the second sub-region 221 are determined according to the shape of the tantalum nitride resistor layer 4 actually required, the widths between the several first sub-regions 211 of the above-mentioned first region 21 may be the same or different, the widths between the several second sub-regions 221 of the second region 22 may be the same or different, the widths between the first sub-regions 211 and the second sub-regions 221 may be the same or different, and the widths between the several first sub-regions 211 and the several second sub-regions 221 may be gradually increased, gradually decreased, or first increased and then decreased, or first decreased and then increased, with equal widths or no regularity between the widths, and the above settings are all feasible.
[0074] In the embodiment of the present application, the two edge regions 23 are arranged at opposite ends of the dielectric layer 2 on the side facing away from the substrate 1, and the ends of the two edge regions 23 are flush with the ends of the opposite ends of the dielectric layer 2 in a direction perpendicular to the substrate 1, that is, one end of one edge region 23 away from the adjacent second sub-region 221 is flush with one end of the dielectric layer 2, and the other end of the edge region 23 away from the adjacent second sub-region 221 is flush with the other end of the dielectric layer 2. At this time, the projection of the dielectric layer 2 in the direction perpendicular to the substrate 1 should cover the projection of the two edge regions 23 in the direction of the substrate 1.
[0075] After determining the positions of the first region 21, the second region 22, and the edge region 23, the photoresist spun on the dielectric layer 2 can be processed through exposure, pre-baking, development, and post-baking steps to remove the first photoresist in some regions and obtain the desired first photoresist layer 3.
[0076] Photoresist, also known as photoresist, has photochemical sensitivity. Development is a key step in producing the first photoresist layer 3 of the desired pattern on the dielectric layer 2. Specifically, the soluble area on the photoresist can be dissolved by a developer, so that the desired first photoresist layer is developed on the side of the dielectric layer 2 facing away from the substrate 1, so that the first photoresist layer 3 after development covers the second area 22 and the edge area 23 on the dielectric layer 2, and exposes the first area 21 set on the dielectric layer 2. Then, a post-baking step is performed to enhance the adhesion of the first photoresist layer 3 to the dielectric layer 2 and the surface of the substrate 1, thereby improving the stability of subsequent processes and avoiding defects and damage during the process.
[0077] It should be noted that the first area 21 exposed on the above-mentioned dielectric layer 2, and the second area 22 and the edge area 23 covered with the first photoresist layer 3 on the dielectric layer 2 need to be determined based on the shape of the required tantalum nitride resistor layer 4, so the present application does not further limit the specific width and number of the first sub-area 211 and the second sub-area 221; it can be observed that at this time, the processed first photoresist layer 3 covers the second area 22 and the edge area 23 on the dielectric layer 2, exposing the first area 21 on the dielectric layer 2.
[0078] Step S3: forming a tantalum nitride resistance layer 4 on the first photoresist layer 3 by magnetron sputtering;
[0079] As an optional implementation, the above-mentioned magnetron sputtering is performed on the first photoresist layer 3 to form the tantalum nitride resistance layer 4, including:
[0080] Using metal tantalum as a target material and nitrogen as a reaction gas, the metal tantalum target material is bombarded by magnetron sputtering in a mixed gas of nitrogen and a protective gas to form the tantalum nitride resistance layer 4 on the first photoresist layer 3 .
[0081] Exemplarily, the preparation of the tantalum nitride resistor layer 4 can be achieved by processes such as magnetron reactive sputtering, electron beam evaporation, and LP-MOCVD (Low Pressure Metalorganic Chemical Vapor Phase Deposition); the present application preferably prepares the required tantalum nitride (TaN) resistor layer by magnetron reactive sputtering, specifically using metal tantalum as a target material and nitrogen (N2) as a reaction gas, and bombarding the metal tantalum target by magnetron sputtering in a mixture of nitrogen and protective gas.
[0082] As an optional implementation, on the first photoresist layer 3 after removing part of the area, argon (Ar) is used as a protective gas and nitrogen is used as a reaction gas, so that the nitrogen is combined with tantalum atoms excited by plasma bombardment of the metal tantalum target to form the required tantalum nitride resistance layer 4.
[0083] Specifically, the size of x in the TaNx resistor layer can be adjusted by adjusting the ratio between the above-mentioned nitrogen and the protective gas. The conductive properties of the tantalum nitride thin film resistor can be adjusted by controlling the nitrogen content. In principle, the smaller the nitrogen content, the stronger the conductive properties of the tantalum nitride thin film resistor formed. The ratio between nitrogen and the protective gas can be adjusted according to actual needs, and this application does not impose further restrictions on this.
[0084] Please refer to Figure 6 ,for Figure 1 The schematic diagram of the structure of forming the tantalum nitride resistor layer 4 by magnetron sputtering in the thin film resistor preparation method shown in the figure can set the thickness of the tantalum nitride resistor layer 4 to 80-100 nanometers.
[0085] Step S4: stripping the first photoresist layer 3 and the tantalum nitride resistor layer 4 formed on the first photoresist layer 3, and retaining the tantalum nitride resistor layer 4 formed in the first region 21;
[0086] As an optional implementation manner, the above-mentioned stripping of the first photoresist layer 3 and the tantalum nitride resistor layer 4 formed on the first photoresist layer 3 includes:
[0087] The first photoresist layer 3 and the tantalum nitride resistor layer 4 formed on the first photoresist layer 3 are stripped off by a wet stripping process.
[0088] In the embodiments of this application, please continue to refer to Figure 7The first photoresist layer 3 and the tantalum nitride resistor layer 4 formed on the first photoresist layer 3 can be stripped by wet stripping (Lift-off), such as by wet stripping with a stripping solution such as acetone or NMP (N-Methylpyrrolidone), by immersing the above-prepared substrate 1, dielectric layer 2, first photoresist layer 3, tantalum nitride resistor layer 4 formed in the first region 21 of dielectric layer 2, and tantalum nitride resistor layer 4 formed on the first photoresist layer 3 in the stripping solution.
[0089] Since the first photoresist layer 3 covers the second area 22 and the edge area 23 on the dielectric layer 2, the tantalum nitride resistor layer 4 on the first photoresist layer 3 will be stripped synchronously during the stripping process, retaining the tantalum nitride resistor layer 4 formed on the first area 21 and exposing the second area 22 and the edge area 23 of the dielectric layer 2.
[0090] The present application can make the stripping process between the first photoresist layer 3 and the dielectric layer 2 more complete and thorough through wet stripping, thereby improving the device performance of the final thin-film resistor; of course, the above acetone or NMP stripping solution is only an example, and the present application does not further limit the specific material of the stripping solution.
[0091] Step S5: disposing a second photoresist layer 5 on the dielectric layer 2 and the tantalum nitride resistor layer 4;
[0092] When the first photoresist layer 3 and the tantalum nitride resistor layer 4 formed on the first photoresist layer 3 are wet-stripped, the tantalum nitride resistor layer 4 formed in the first region 21 of the dielectric layer 2 can be obtained. Figure 7 As shown, at this time, the second region 22 and the two edge regions 23 on the dielectric layer 2 are in an exposed state, and a second photolithography process needs to be performed on the dielectric layer 2 and the tantalum nitride resistor layer 4 .
[0093] For details, please refer to Figure 8 ,for Figure 1 The schematic diagram of the structure of the second photoresist layer 5 spin-coated in the thin film resistor preparation method shown in the figure, the present application spin-coats the second photoresist layer 5 on the second region 22, the edge region 23 of the dielectric layer 2 and the tantalum nitride resistor layer 4, and similarly processes the photoresist spin-coated on the above-mentioned dielectric layer 2 and the tantalum nitride resistor layer 4 through the steps of exposure, pre-baking, developing and post-baking to remove the second photoresist in a partial region and obtain the desired second photoresist layer 5.
[0094] Step S6: removing the second photoresist in a partial area to expose the second area 22 of the dielectric layer 2 and the adjacent area 41 of the tantalum nitride resistor layer 4;
[0095] As an optional implementation, the adjacent region 41 is provided on the side of the tantalum nitride resistance layer 4 facing away from the dielectric layer 2;
[0096] The adjacent region 41 includes a plurality of adjacent sub-regions 411 arranged along the first direction, and the second sub-region 221 is connected to the adjacent sub-region 411 .
[0097] In the embodiment of the present application, the second photoresist in a partial area is removed through exposure, pre-baking, development, and post-baking steps to obtain the required second photoresist layer 5, and expose the second area 22 of the dielectric layer 2 and the adjacent area 41 on the tantalum nitride resistor layer 4.
[0098] Please refer to Fig. 9 ,for Figure 1 The schematic diagram of the structure in which part of the second photoresist is removed in the thin film resistor preparation method shown in the figure, the present application provides an adjacent region 41 on the side of the tantalum nitride resistor layer 4 facing away from the dielectric layer 2, and the adjacent region 41 includes a plurality of adjacent sub-regions 411 arranged along the first direction, and it can be observed that the second sub-region 221 is connected to the adjacent sub-region 411.
[0099] As an optional implementation, the present application sets the width of the adjacent sub-region 411 to be smaller than the width of the first sub-region 211 .
[0100] Preferably, the width of the adjacent sub-region 411 is set to be less than half of the width of the first sub-region 211. It can be observed that two adjacent sub-regions 411 are correspondingly arranged above a first sub-region 211, and the two adjacent sub-regions 411 are arranged on opposite sides of the first sub-region 211, and a gap is arranged between the two adjacent sub-regions 411, and one end of one adjacent sub-region 411 connected to the second sub-region 221 is flush with one end of the first sub-region 211, and the other adjacent sub-region 411 is connected to one end of the second sub-region 221 and is flush with the other end of the first sub-region 211.
[0101] That is to say, the projections of two adjacent sub-regions 411 located on the same first sub-region 211 in the direction perpendicular to the substrate 1 overlap with the two end edges of the projections of the corresponding first sub-region 211 in the direction perpendicular to the substrate 1, that is, the projection of the first sub-region 211 in the direction perpendicular to the substrate 1 covers the projections of the corresponding two adjacent sub-regions 411 in the direction perpendicular to the substrate 1.
[0102] Further, it can be observed that the second sub-region 221 is connected to the adjacent adjacent sub-region 411 without any gap; specifically, both ends of the second sub-region 221 located between the two first sub-regions 211 are connected to the adjacent adjacent sub-regions 411, and one end of the second sub-region 221 located between the edge region 23 and the first sub-region 211 is connected to the adjacent adjacent sub-region 411, and the other end is connected to the adjacent edge region 23.
[0103] It should be understood that the specific width and number of the above-mentioned adjacent sub-regions 411 are determined according to the actual required shape of the lead electrode, that is, according to the shape of the metal layer 6 finally required. This application does not impose further restrictions on the specific width and number of the above-mentioned adjacent sub-regions 411.
[0104] After the width and position of the adjacent sub-region 411 are determined, the second photoresist layer 5 is etched through the above-mentioned steps of exposure, pre-baking, developing, post-baking, etc. to remove the second photoresist layer 5 on the second sub-region 221 and the adjacent sub-region 411, and the second region 22 of the dielectric layer 2 and the adjacent region 41 disposed on the tantalum nitride resistor layer 4 are exposed. Fig. 9 shown.
[0105] Step S7: depositing a metal layer 6 on the dielectric layer 2 and the tantalum nitride resistor layer 4;
[0106] As an optional implementation, the above-mentioned depositing of the metal layer 6 on the dielectric layer 2 and the tantalum nitride resistance layer 4 includes:
[0107] The metal layer 6 is deposited on the dielectric layer 2 and the tantalum nitride resistor layer 4 by using a low-temperature electron beam evaporation process; wherein the temperature of the electron beam evaporation process is 25-40 degrees Celsius.
[0108] As an optional implementation, the thickness of the second photoresist layer 5 is greater than the thickness of the metal layer 6 .
[0109] Preferably, the thickness of the second photoresist layer 5 is set to be greater than or equal to three times the thickness of the metal layer 6 .
[0110] In the embodiment of the present application, the metal layer 6 is preferably deposited on the dielectric layer 2 and the tantalum nitride resistor layer 4 by a low-temperature electron low-temperature electron beam evaporation process. Fig.10 ,for Figure 1 The schematic structural diagram of depositing the metal layer 6 in the method for preparing the thin film resistor is shown. It can be observed that the thickness of the second photoresist layer 5 is greater than the thickness of the deposited metal layer 6 .
[0111] Exemplarily, the temperature of the low-temperature electron low-temperature electron beam evaporation process can be set to room temperature, such as 25-40 degrees Celsius, and the time for depositing the metal layer 6 can be controlled within 2-3 hours. This application does not further limit the temperature and time in the specific deposition process.
[0112] It can be observed that Fig.10 The thickness of the metal layer 6 deposited in the first region 21 of the dielectric layer 2 is smaller than the thickness of the second photoresist layer 5 in the adjacent edge region 23 .
[0113] Preferably, the thickness of the second photoresist layer 5 may be set to be greater than or equal to three times the thickness of the metal layer 6 , so as to deposit the required metal layer 6 in the second region 22 of the dielectric layer 2 and the adjacent region 41 of the tantalum nitride resistor layer 4 .
[0114] Step S8: stripping off the second photoresist layer 5 and the metal layer 6 formed on the second photoresist layer 5 , and retaining the metal layer 6 formed in the second region 22 and the adjacent region 41 .
[0115] In step S8, the second photoresist layer 5 and the metal layer 6 formed on the second photoresist layer 5 are also stripped by wet stripping, and the wet stripping can be performed by a stripping solution such as acetone or NMP. At this time, the above-prepared substrate 1, the dielectric layer 2, the tantalum nitride resistor layer 4 formed in the first area 21 of the dielectric layer 2, the second photoresist layer 5 formed in the tantalum nitride resistor layer 4 and the edge area 23 of the dielectric layer 2, the metal layer 6 formed in the second area 22 of the dielectric layer 2, and the metal layer 6 formed on the second photoresist layer 5 are immersed in the stripping solution.
[0116] Please refer to Fig.11 ,for Figure 1 The structural schematic diagram of stripping the second photoresist layer 5 in the thin film resistor preparation method shown in the figure, during the stripping process of the second photoresist layer 5, the metal layer 6 on the second photoresist layer 5 will be stripped synchronously, and it can be observed that the second photoresist layer 5 on the two edge areas 23 and the metal layer 6 deposited thereon, as well as the second photoresist layer 5 between the two adjacent sub-areas 411 on the same first sub-area 211 and the metal layer 6 deposited thereon are stripped synchronously to retain the metal layer 6 formed in the second area 22 and the adjacent area 41; of course, it is also feasible to use stripping solutions of other materials in the wet stripping process, and the present application does not impose further restrictions on this.
[0117] As an optional embodiment, the above-mentioned metal layer 6 can be set to a common conductive material, such as any one or more metals selected from the group consisting of Ni, Pd, Ag, Pt, Au, Cr, Cu, Ti, and Al; it can also be set to a stack formed by any one or more metals selected from the group consisting of Ni, Pd, Ag, Pt, Au, Cr, Cu, Ti, and Al; it can also be set to an alloy made from any one or more metals selected from the group consisting of Ni, Pd, Ag, Pt, Au, Cr, Cu, Ti, and Al.
[0118] It should be understood that the present application does not impose any further restrictions on the specific configuration of the metal layer 6 , which can be selected according to actual thin-film resistor preparation requirements.
[0119] As an optional implementation manner, after the second photoresist layer 5 and the metal layer 6 formed on the second photoresist layer 5 are stripped, the method further includes:
[0120] In a vacuum argon environment, rapid thermal annealing is performed on the retained substrate 1, the dielectric layer 2, the tantalum nitride resistor layer 4 and the metal layer 6; wherein the time of the rapid thermal annealing does not exceed 30 minutes.
[0121] In the embodiment of the present application, it is necessary to perform RTP (Rapid Thermal Processing) process on the substrate 1, dielectric layer 2, tantalum nitride resistor layer 4 and metal layer 6 after wet stripping. Compared with the traditional furnace tube annealing method, this thermal annealing process has the advantages of less thermal budget, less impurity movement in silicon, less contamination and shorter processing time.
[0122] The present application can reduce the contact resistance formed between the metal layer 6 and the tantalum nitride resistance layer 4 by a thermal annealing process. The contact resistance corresponds to Fig.11 The contact portion between the metal layer 6 and the tantalum nitride resistor layer 4, and in order to avoid oxidation and nitridation, the above thermal annealing process should be carried out in a vacuum or argon environment, and the thermal annealing time is preferably controlled within 30 minutes to form the desired thin film resistor.
[0123] The preparation method of the thin film resistor provided by the present application comprises the following steps: depositing a dielectric layer on a substrate, arranging a first photoresist on the dielectric layer, removing the first photoresist in a partial area through exposure, pre-baking, developing, and post-baking steps, and exposing the first area of the dielectric layer, forming a tantalum nitride resistor layer on the first photoresist layer by magnetron sputtering, stripping the first photoresist layer and the tantalum nitride resistor layer formed on the first photoresist layer through a wet stripping process, continuously arranging a second photoresist layer on the dielectric layer and the tantalum nitride resistor layer, and removing the second photoresist in a partial area through exposure, pre-baking, developing, and post-baking steps. The present application adopts a wet photolithography process to prepare a thin film resistor. It replaces the traditional high-temperature etching process, avoids the phase change of the thin film resistor in the high-temperature etching chamber, improves the stability of the preparation process, and avoids defects and damage to the thin film resistor during the preparation process; during the preparation process, by adjusting the ratio between nitrogen and protective gas, the conductive properties of the tantalum nitride thin film resistor can be effectively adjusted; the thin film resistor that has completed two wet lithography processes is subjected to rapid thermal annealing treatment, thereby reducing the contact resistance formed between the metal layer and the tantalum nitride resistor layer, which can reduce the energy loss generated by the current in the thin film resistor, and effectively improve the conductive properties and reliability of the thin film resistor.
[0124] Based on the above-mentioned method for preparing a thin film resistor, the present application also provides a thin film resistor, which can be prepared through the above-mentioned steps S1-S8, and the thin film resistor includes a substrate 1, a dielectric layer 2, a tantalum nitride resistor layer 4 and a metal layer 6.
[0125] Please continue to refer to Fig.11 In the present application, a dielectric layer 2 is disposed on a substrate 1, a first region 21 and a second region 22 are disposed on the dielectric layer 2, a tantalum nitride resistor layer 4 covers the first region 21 on the dielectric layer 2, an adjacent region 41 is disposed on the tantalum nitride resistor layer 4, a metal layer 6 is disposed on the adjacent region 41 and the second region 22 of the dielectric layer 2, the tantalum nitride resistor layer 4 is connected to the metal layer 6, and the thickness of the metal layer 6 is greater than the thickness of the tantalum nitride. The thin film resistor formed by the present application has a small contact resistance, can reduce the energy loss generated by the current in the thin film resistor, thereby improving the conductive performance and reliability of the thin film resistor.
[0126] It should be noted that the present application takes the length extension direction of the substrate 1 as the first direction, which is perpendicular to the thickness extension direction of the above-mentioned thin film resistor. It can be observed that the above-mentioned metal layer 6, tantalum nitride resistor layer 4, dielectric layer 2 and substrate 1 are arranged along the thickness extension direction.
[0127] As an optional implementation, the substrate 1 may be a silicon wafer substrate, and the thickness is preferably set to 650-700 microns.
[0128] Optionally, the dielectric layer 2 is a SiO2 dielectric layer 2, and the thickness of the SiO2 dielectric layer 2 is preferably set to 1.5 microns; the thickness of the tantalum nitride resistor layer 4 is preferably set to 80-100 nanometers, and the thickness of the metal layer 6 is preferably greater than the thickness of tantalum nitride.
[0129] Of course, the thickness setting range in the above example is only used as a preferred implementation mode and does not constitute any limitation on the present application. The thickness of the substrate 1, dielectric layer 2, tantalum nitride resistor layer 4 and metal layer 6 can be adjusted accordingly according to actual needs, and the present application does not impose any limitation on this.
[0130] For other details about the above-mentioned thin film resistor implementing the above-mentioned technical solution, please refer to the description of the thin film resistor preparation method provided in the above-mentioned application embodiment, which will not be repeated here.
[0131] The embodiments described above are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.
Claims
1. A method for preparing a thin film resistor, characterized in that: The following steps are involved: Depositing a dielectric layer on a substrate, and providing a first photoresist layer on the dielectric layer; Removing a portion of the first photoresist to expose the first region of the dielectric layer; forming a tantalum nitride resistance layer on the first photoresist layer by magnetron sputtering; Stripping the first photoresist layer and the tantalum nitride resistor layer formed on the first photoresist layer, and retaining the tantalum nitride resistor layer formed in the first region; Disposing a second photoresist layer on the dielectric layer and the tantalum nitride resistance layer; Removing a portion of the second photoresist to expose the second region of the dielectric layer and an adjacent region of the tantalum nitride resistance layer; Depositing a metal layer on the dielectric layer and the tantalum nitride resistance layer; The second photoresist layer and the metal layer formed on the second photoresist layer are stripped off, and the metal layer formed in the second region and the adjacent region is retained.
2. The method for preparing a thin film resistor according to claim 1, characterized in that: The method of performing magnetron sputtering on the first photoresist layer to form a tantalum nitride resistance layer comprises: Using metal tantalum as a target material and nitrogen as a reaction gas, the metal tantalum target material is bombarded by magnetron sputtering in a mixed gas of nitrogen and a protective gas to form the tantalum nitride resistance layer on the first photoresist layer.
3. The method for preparing a thin film resistor according to claim 1, characterized in that: The first region and the second region are arranged on a side of the dielectric layer facing away from the substrate; The first region includes a plurality of first sub-regions arranged along a first direction, the second region includes a plurality of second sub-regions arranged along the first direction, a plurality of the first sub-regions and the second sub-regions are alternately arranged along the first direction, and the first sub-region is connected to an adjacent second sub-region.
4. The method for preparing a thin film resistor according to claim 3, characterized in that: The adjacent area is provided on the side of the tantalum nitride resistance layer facing away from the dielectric layer; The adjacent region includes a plurality of adjacent sub-regions arranged along a first direction, and the second sub-region is connected to the adjacent adjacent sub-regions.
5. The method for preparing a thin film resistor according to claim 1, characterized in that: The step of depositing a metal layer on the dielectric layer and the tantalum nitride resistance layer comprises: A metal layer is deposited on the dielectric layer and the tantalum nitride resistor layer using a low-temperature electron beam evaporation process; wherein the temperature of the electron beam evaporation process is 25-40 degrees Celsius, and the thickness of the second photoresist layer is greater than the thickness of the metal layer.
6. The method for preparing a thin film resistor according to claim 5, characterized in that: The thickness of the second photoresist layer is greater than or equal to three times the thickness of the metal layer.
7. The method for preparing a thin film resistor according to claim 1, characterized in that: After stripping the second photoresist layer and the metal layer formed on the second photoresist layer, the method further includes: In a vacuum argon environment, rapid thermal annealing is performed on the retained substrate, the dielectric layer, the tantalum nitride resistor layer and the metal layer; wherein the time of the rapid thermal annealing does not exceed 30 minutes.
8. The method for preparing a thin film resistor according to claim 1, wherein: The step of depositing a dielectric layer on the substrate comprises: A SiO2 dielectric layer is deposited on the substrate by a plasma enhanced chemical vapor deposition process; wherein the thickness of the SiO2 dielectric layer is 1.5 microns.
9. The method for preparing a thin film resistor according to claim 1, characterized in that: Stripping the first photoresist layer and the tantalum nitride resistor layer formed on the first photoresist layer by a wet stripping process; And, the second photoresist layer and the metal layer formed on the second photoresist layer are stripped by a wet stripping process.
10. A thin film resistor, characterized in that: include: substrate; A dielectric layer, disposed on the substrate; A tantalum nitride resistor layer is disposed in a first region on the substrate; The metal layer is arranged in the second area on the substrate and in the adjacent area on the tantalum nitride resistor layer. The tantalum nitride resistor layer is connected to the metal layer, and the thickness of the metal layer is greater than the thickness of the tantalum nitride resistor layer.