PCB manufacturing method and PCB
By filling the PCB with conductive paste and using high-temperature lamination technology, a variety of copper thickness patterns are formed, which solves the problems of complex traditional processes and difficulty in ensuring pattern accuracy, and achieves the effects of simplifying the process and improving copper thickness reliability.
Patent Information
- Application Number
- CN202411154840.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-18
AI Technical Summary
When the existing technology realizes low-loss transmission of high-frequency and high-speed signals in PCB signal lines, it is difficult to guarantee the pattern accuracy. Especially when the copper thickness is thin, the reliability of the non-antenna area cannot be guaranteed, and the traditional process is complex and difficult to achieve diversity. Thick copper design.
By filling the substrate with conductive paste and solidifying it, the substrate and sub-board are pressed together at high temperature to form a PCB with various copper thickness patterns, simplifying the process route and avoiding the traditional local copper reduction and multiple etching or thinning of the traditional thick copper foil. The complex process of copper foil plating.
It realizes the production of multiple copper thickness patterns on the same layer of PCB, simplifies the process flow, improves pattern accuracy and copper thickness reliability, and reduces production difficulty and cycle time.
Smart Images

Figure CN118804486A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of PCB (Printed Circuit Board), and in particular to a PCB manufacturing method and a PCB. Background Art
[0002] As the field of communication electronics gradually develops towards high frequency and high speed of signals, higher requirements are placed on the low-loss transmission of high frequency and high speed signals in signal lines in PCBs. Taking antenna products as an example, it is necessary to control the graphics accuracy as much as possible to obtain better performance. However, when the etching copper thickness reaches a certain thickness, the graphics accuracy is difficult to guarantee. In order to obtain high-precision antenna graphics, the copper thickness at the antenna position needs to be reduced as much as possible. However, if the copper thickness is too thin, the reliability of non-antenna areas (such as digital areas) and mounting areas cannot be guaranteed.
[0003] In order to maximize the functions of digital power supply, antenna and other modules of antenna products, the concept of local pattern copper thickness differentiation is proposed. The traditional process route to achieve local pattern copper thickness differentiation mostly adopts thick copper foil local copper reduction and multiple pattern etching, or thin copper foil electroplating and multiple pattern etching. However, the above process route is complicated, the production cycle is long and the production difficulty is extremely high, and there are limitations in realizing diversified copper thickness design. Summary of the invention
[0004] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes a PCB manufacturing method and a PCB, which can obtain a PCB with multiple copper thickness patterns on the same layer and effectively simplify the process route.
[0005] A PCB manufacturing method according to an embodiment of the present application includes the following steps:
[0006] Providing a substrate, the substrate having a first end surface, the first end surface being provided with one or more grooves, the grooves being filled with a conductive paste and cured, wherein the conductive paste in the grooves is flush with the first end surface;
[0007] Providing a daughter board, stacking the daughter board and the substrate, and making the first end surface located on a side of the substrate close to the daughter board, so that the substrate and the daughter board are aligned and pressed together;
[0008] The substrate is removed to obtain a target PCB.
[0009] Furthermore, it also includes: providing a copper foil layer and an adhesive layer, laminating the copper foil layer to the first end surface and pressing it at low temperature, and then removing the copper foil layer outside the overlapping area with the conductive paste; the step of aligning and pressing the substrate and the sub-board includes: arranging the substrate, the adhesive layer and the sub-board in sequence and pressing them as a whole at high temperature.
[0010] Furthermore, a first circuit pattern is provided at a position of the sub-board corresponding to the conductive paste, and when the substrate and the sub-board are pressed together at high temperature, the first circuit pattern directly contacts the cured conductive paste.
[0011] Furthermore, the first end surface of the substrate has grooves with various depths.
[0012] Furthermore, the step of providing a daughter board includes: processing the first circuit pattern on the daughter board, wherein the thickness of the first circuit pattern is smaller than the thickness of the target circuit pattern.
[0013] Furthermore, the substrate is made of foaming material, UV viscosity-reducing material or magnetic fluid material.
[0014] Furthermore, the substrate is made of foam material, and the step of removing the substrate includes: treating the foam material with alkaline solution.
[0015] Furthermore, the substrate is made of UV viscosity-reducing material, and the step of removing the substrate includes: irradiating the substrate with a UV light source to reduce the viscosity of the UV viscosity-reducing material in the substrate and the conductive paste, and then peeling off the substrate.
[0016] Furthermore, the conductive paste is filled into the groove by screen printing, sputtering or printing.
[0017] Furthermore, the step of aligning and pressing the substrate and the sub-board includes: providing a limit frame and pins, the limit frame having a limit groove, and the substrate is partially arranged in the limit groove, wherein the depth of the limit groove is less than the thickness of the substrate, and the depth of the limit groove is greater than the depth of any one of the grooves.
[0018] Furthermore, the pins are distributed simultaneously in the limit frame and the finished hollow area in the substrate unit, and the total height of the pins is greater than 60% of the total height of the substrate and the sub-board, and the total height of the pins is less than 80% of the total height of the substrate and the sub-board.
[0019] The PCB in another embodiment of the present application is manufactured using the PCB manufacturing method as described above.
[0020] The PCB manufacturing method and PCB of the embodiment of the present application have at least the following beneficial effects: the conductive paste is filled in the groove of the substrate and solidified, the solidified conductive paste is pressed into the sub-board through the substrate, and then the substrate is removed. At this time, the solidified conductive paste is bonded to the sub-board, so that the sub-board of the target PCB has the solidified conductive paste. Among them, the solidified conductive paste constitutes the target circuit pattern of the sub-board in the target PCB, and the shape and thickness of the conductive paste are related to the depth of the groove in the substrate. By controlling and changing the depth of different grooves in the substrate, multiple circuit patterns of the same thickness or different thicknesses can be obtained at one time. Compared with the method of using thick copper foil local copper reduction + multiple pattern etching or thin copper foil electroplating + multiple pattern etching in the traditional process, the PCB manufacturing method of the embodiment of the present application can effectively simplify the manufacturing process of PCBs with circuit patterns of different thicknesses on the same layer.
[0021] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present application is further described below with reference to the accompanying drawings and embodiments, wherein:
[0023] Figure 1 A schematic diagram of a PCB manufacturing method according to an embodiment of the present application;
[0024] Figure 2 This is a schematic diagram of the structure of a sub-board in a PCB manufacturing method according to an embodiment of the present application;
[0025] Figure 3 A schematic diagram of manufacturing a substrate in a PCB manufacturing method according to an embodiment of the present application;
[0026] Figure 4 This is a schematic diagram of the structure of laminating and pressing a sub-board and a substrate in a PCB manufacturing method according to an embodiment of the present application;
[0027] Figure 5 This is a schematic structural diagram of a sub-board in a PCB manufacturing method according to another embodiment of the present application;
[0028] Figure 6 A schematic diagram of manufacturing a substrate in a PCB manufacturing method according to another embodiment of the present application;
[0029] Figure 7 A schematic diagram of the structure of laminating and pressing a sub-board and a substrate in a PCB manufacturing method in another embodiment of the present application.
[0030] Reference numerals:
[0031] 100, substrate; 110, groove; 120, conductive paste; 130, copper foil layer;
[0032] 200, daughter board; 210, first circuit pattern;
[0033] 300, bonding layer;
[0034] 410, limit frame; 420, pin. DETAILED DESCRIPTION
[0035] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0036] In the description of the present application, it should be understood that descriptions involving orientation, such as up, down, front, back, left, right, etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0037] In the description of this application, "several" means more than one, "more" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number itself, and "above", "below", "within", etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0038] In the description of this application, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in this application based on the specific content of the technical solution.
[0039] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0040] See also Figure 1 and Figure 2 , Figure 1 A schematic diagram of a PCB manufacturing method according to an embodiment is shown. Figure 2 A structural schematic diagram of each step in a PB production method according to an embodiment is shown.
[0041] like Figure 1 and Figure 2 As shown, an embodiment of the present application discloses a PCB manufacturing method, comprising the following steps:
[0042] S110: providing a substrate 100, wherein the substrate 100 has a first end surface, and one or more grooves 110 are arranged on the first end surface, and a conductive paste 120 is filled in the grooves 110 and cured, wherein the conductive paste 120 in the grooves 110 is flush with the first end surface.
[0043] It should be noted that when there are multiple grooves 110 , the shapes and depths of the grooves 110 may be the same or different, which is not limited here.
[0044] S120: providing a sub-board 200, and stacking the sub-board 200 and the substrate 100, with the first end surface located on a side of the substrate 100 close to the sub-board 200, so that the substrate 100 and the sub-board 200 are aligned and pressed together;
[0045] S130: removing the substrate 100 to obtain a target PCB.
[0046] The number of the grooves 110 is set according to the number of circuit patterns with different copper thicknesses, and the depth of each groove 110 is related to the copper thickness of the corresponding circuit pattern.
[0047] In the embodiment of the present application, the conductive paste 120 is filled in the groove 110 of the substrate 100 and cured, and the cured conductive paste 120 is pressed into the sub-board 200 through the substrate 100, and then the substrate 100 is removed. At this time, the cured conductive paste 120 is pressed and bonded to the sub-board 200, so that the sub-board 200 of the target PCB has the cured conductive paste 120. Among them, the cured conductive paste 120 constitutes the target circuit pattern of the target PCB, and the shape and thickness of the conductive paste 120 are related to the depth of the groove 110 in the substrate 100. By controlling and changing the depth of different grooves 110 in the substrate 100, multiple circuit patterns of the same thickness or different thicknesses can be obtained at one time. Compared with the manufacturing method of using thick copper foil local copper reduction + multiple pattern etching or thin copper foil electroplating + multiple pattern etching in the traditional process, the PCB manufacturing method of the embodiment of the present application can effectively simplify the manufacturing process of PCBs with circuit patterns of different thicknesses on the same layer.
[0048] In some embodiments of the present application, see Figures 1 to 4The PCB manufacturing method also includes: providing a copper foil layer 130 and an adhesive layer 300, laminating the copper foil layer 130 on the first end surface and pressing at low temperature, and then removing the copper foil layer 130 outside the overlapping area of the copper foil layer 130 and the conductive paste 120; aligning the substrate 100 and the sub-board 200 and pressing at high temperature. This step includes: the substrate 100, the adhesive layer 300 and the sub-board 200 are arranged in sequence and pressed at high temperature as a whole.
[0049] In the above embodiment, when the copper foil layer 130 and the conductive paste 120 are pressed together at low temperature, the conductive paste 120 in the groove 110 can be sintered at low temperature. During the sintering process, the conductive material of the conductive paste 120 forms an alloy with the surface copper foil to ensure the bonding strength.
[0050] In a possible implementation, when removing the copper foil layer 130 outside the overlapping area between the copper foil layer 130 and the conductive paste 120 , the copper foil layer 130 may be processed by laser cutting to remove the ultra-thin copper foil at the non-groove 110 position.
[0051] In the above embodiment, after the conductive paste 120 in each groove 110 is cured, the copper foil layer 130 is attached to the first end surface of the substrate 100, and then the copper foil layer 130 in the projection area of each groove 110 along the thickness direction of the substrate 100 is retained, and the remaining copper foil layers 130 are removed. Among them, the copper foil layer 130 can play a supporting role for the conductive paste 120, which helps to improve the bonding force between the cured conductive paste 120 and the adhesive layer 300, thereby reducing the risk of bonding reliability between the conductive paste 120 and the adhesive layer 300, that is, it is conducive to reducing the bonding failure between the conductive paste 120 and the adhesive layer 300. In addition, the arrangement of the copper foil layer 130 and the adhesive layer 300 can add layers to the structure of the sub-board 200. When the copper foil layer 130 is added to a single side of the sub-board 200, it is convenient to make an arbitrary odd-numbered layered PCB structure, which can effectively solve the warping problem caused by making an odd-numbered PCB by traditional processes.
[0052] In a possible implementation manner, the conductive paste 120 is copper paste.
[0053] It is worth understanding that the copper foil layer 130 in this solution is an ultra-thin copper foil, which plays a role in receiving and preventing the sintered copper paste from directly bonding with the adhesive material, which may cause a risk of bonding reliability. It is worth understanding that the mechanism of low-temperature sintering of copper paste is that the copper paste forms an alloy with the metal during the sintering process to ensure the bonding strength. The high-temperature pressing of the copper foil and the adhesive material is mainly a physical combination, and its bonding strength can also be guaranteed. In this way, the bonding strength between the solidified copper paste and the sub-board 200 can be effectively guaranteed.
[0054] It should be pointed out that in the above-mentioned embodiment, if the sintered copper paste is directly pressed with the bonding material, there will be a higher reliability risk, such as differential pattern peeling, because no alloy is formed on the contact surface.
[0055] In some other embodiments, the conductive paste 120 may also be silver paste or paste made of other conductive metals and alloys, which is not limited here.
[0056] In some solutions, copper foil is directly bonded to the surface of the foam material, and then the circuit pattern is made by traditional etching. When the above solution is applied to the production of differentiated copper thickness circuit patterns, it is necessary to go through multiple electroplating, multiple etching and other processes, which will have many technical difficulties and the process flow is extremely complicated. For example, under the action of multiple high-temperature and wet processes, the bonding strength between the foam material and the copper foil is difficult to ensure, and the risk of copper foil peeling is extremely high, which affects the yield of pattern production; differentiated graphics with different copper thicknesses cannot be produced at the same time. Each graphic with a copper thickness needs to go through at least one film bonding / exposure / development / electroplating. The control of the accuracy of the graphic position is extremely difficult. There will be problems such as loose film bonding between circuit patterns with different copper thicknesses, which will lead to the problem of copper plating failure, and ultimately lead to the copper thickness of the edge of the graphic not meeting the requirements and the graphic deformation.
[0057] In the PCB manufacturing method of the embodiment of the present application, the circuit pattern with differentiated copper thickness is directly formed through a one-time processing, rather than being manufactured through multiple electroplating / etching processes of copper foil, and there is no problem of pattern accuracy deviation caused by bonding force and multiple alignments.
[0058] In one embodiment of the present application, the copper foil layer 130 is specifically made of ultra-thin copper foil. Exemplarily, the thickness of the copper foil layer 130 is 3 μm, and the thickness of the copper foil layer 130 does not affect the overall thickness of the circuit pattern. Therefore, the depth of the groove 110 in the substrate 100 is directly set to the thickness of the target circuit pattern. The copper thickness of the target circuit pattern with different copper thicknesses is presented by the grooves 110 with different depths.
[0059] In some embodiments of the present application, see Figures 5 to 7 A first circuit pattern 210 is disposed at a position of the daughter board 200 corresponding to the conductive paste 120 . When the daughter board 200 and the substrate 100 are pressed together at high temperature, the first circuit pattern 210 directly contacts the conductive paste 120 .
[0060] In the above embodiment, compared with the solution of pressing and bonding the conductive paste 120 and the sub-board 200 through the copper foil layer 130 and the adhesive material, the ultra-thin copper foil and the adhesive material are eliminated at the same time, and the conductive paste 120 is directly contacted with the first circuit pattern 210 of the sub-board 200. Through the mechanism of low-temperature sintering of the conductive paste 120, the conductive paste 120 forms an alloy with the copper surface of the first circuit pattern of the sub-board 200 during the sintering process, thereby obtaining a circuit pattern with differentiated copper thickness.
[0061] It is worth understanding that, due to the absence of the adhesive layer 300 , when the above PCB manufacturing method is used to manufacture a PCB with differentiated copper thickness, generally no additional layers are added.
[0062] In the above embodiment, the thickness of the first circuit pattern 210 at each position on the daughter board 200 is the same. That is, the first circuit pattern 210 at each position on the daughter board 200 can be obtained by uniform etching, which helps to improve the manufacturing efficiency of the daughter board 200.
[0063] It should be pointed out that the differentiation between each target circuit pattern in the target PCB (i.e., the thickness of the target circuit pattern at each position) is reflected by the depth of each groove 110 in the substrate 100, and each groove 110 of different depths can be filled with the conductive paste 120 at one time, which is conducive to simplifying the manufacturing process of the PCB with circuit patterns with differentiated copper thickness and improving the manufacturing efficiency.
[0064] In a possible implementation, the step of providing the sub-board 200 includes: processing the first circuit pattern 210 on the sub-board 200, wherein the thickness of the first circuit pattern 210 is less than the thickness of the target circuit pattern. Specifically, the thickness of the target circuit pattern is equal to the sum of the thickness of the first circuit pattern 210 and the depth of the groove 110. In other words, the depth of the groove 110 is the thickness of the target circuit pattern minus the thickness of the first circuit pattern 210 at the corresponding position.
[0065] In some embodiments of the present application, the substrate 100 is made of a foaming material, a UV viscosity-reducing material, or a magnetic fluid material.
[0066] In a possible implementation manner, the substrate 100 is made of a foam material, and the step of removing the substrate 100 includes: treating the foam material with an alkaline solution.
[0067] In one possible implementation, the substrate 100 is made of a UV viscosity-reducing material, and the step of removing the substrate 100 includes: irradiating the substrate 100 with a UV light source to reduce the viscosity of the UV viscosity-reducing material in the substrate 100, and then peeling off the substrate 100, and then obtaining a PCB with circuit patterns of multiple copper thicknesses on the same layer.
[0068] In some embodiments of the present application, the conductive paste 120 is filled into the groove 110 by screen printing, sputtering or printing.
[0069] In some embodiments of the present application, the step of aligning and pressing the substrate 100 and the sub-board 200 includes: providing a limit frame 410 and a pin 420, the limit frame 410 has a limit groove, and the substrate 100 is partially disposed in the limit groove, wherein the depth of the limit groove is less than the thickness of the substrate 100, and the depth of the limit groove is greater than the depth of any groove 110.
[0070] Specifically, the limiting frame 410 is mainly used to suppress the lateral deformation of the substrate 100 during the pressing process, thereby reducing the lateral force on the cured conductive paste 120 during the pressing process, helping to ensure the accuracy of the positioning of the conductive paste 120 and avoiding the positioning deviation of the conductive paste 120.
[0071] In some embodiments of the present application, the pins 420 are distributed in the hollowed-out area of the finished product in the limiting frame 410 and the substrate 100 unit at the same time, and the total height of the pins 420 is greater than 60% of the total height of the substrate 100 and the sub-board 200, and the total height of the pins 420 is less than 80% of the total height of the substrate 100 and the sub-board 200. In this way, the alignment accuracy of the substrate 100 and the sub-board 200 at various positions can be further improved, which helps to reduce the situation where the substrate 100 and the sub-board 200 produce lateral offsets during the lamination process, resulting in position deviations between the final circuit pattern and the target circuit pattern.
[0072] Another aspect of the present application discloses a PCB manufactured by the PCB manufacturing method as described above.
[0073] The PCB of the embodiment of the present application is made by the aforementioned PCB manufacturing method. Compared with the traditional process of using thick copper foil local copper reduction + multiple pattern etching or thin copper foil electroplating + multiple pattern etching, the PCB manufacturing method of the embodiment of the present application can effectively simplify the manufacturing process of PCBs with circuit patterns of different thicknesses on the same layer. At the same time, the circuit pattern in the PCB of the embodiment of the present application is directly formed by one-time processing, not by multiple electroplating / etching of copper foil, and there is no problem of pattern accuracy deviation caused by bonding force and multiple alignment.
[0074] In some selectable embodiments, the function / operation mentioned in the block diagram may not occur in the order mentioned in the operation diagram. For example, depending on the function / operation involved, the two boxes shown in succession can actually be executed substantially simultaneously or the boxes can sometimes be executed in reverse order. In addition, the embodiment presented and described in the flow chart of the application is provided by way of example, for the purpose of providing a more comprehensive understanding of technology. The disclosed method is not limited to the operation and logic flow presented herein. Selectable embodiments are expected, wherein the order of various operations is changed and the sub-operation of a part described as a larger operation is performed independently.
[0075] The embodiments of the present application are described in detail above in conjunction with the accompanying drawings, but the present application is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present application. In addition, the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
Claims
1. A PCB manufacturing method, characterized in that: The steps include: Providing a substrate, the substrate having a first end surface, the first end surface being provided with one or more grooves, the grooves being filled with a conductive paste and cured, wherein the conductive paste in the grooves is flush with the first end surface; Providing a daughter board, stacking the daughter board and the substrate, and making the first end surface located on a side of the substrate close to the daughter board, so that the substrate and the daughter board are aligned and pressed together; The substrate is removed to obtain a target PCB.
2. The PCB manufacturing method according to claim 1, characterized in that: Also includes: Providing a copper foil layer and an adhesive layer, laminating the copper foil layer on the first end surface and laminating at low temperature, and then removing the copper foil layer except for the overlapping area with the conductive paste; The step of aligning and pressing the substrate and the sub-board comprises: arranging the substrate, the adhesive layer and the sub-board in sequence and pressing the whole of them at high temperature.
3. The PCB manufacturing method according to claim 1, characterized in that: A first circuit pattern is arranged at a position of the sub-board corresponding to the conductive paste. When the substrate and the sub-board are pressed together at high temperature, the first circuit pattern directly contacts the cured conductive paste.
4. The PCB manufacturing method according to claim 1, characterized in that: The first end surface of the substrate is provided with grooves of various depths.
5. The PCB manufacturing method according to any one of claims 1 to 4, characterized in that: The substrate is made of foaming material, UV viscosity-reducing material or magnetic fluid material.
6. The PCB manufacturing method according to claim 5, characterized in that: The substrate is made of foam material, and the step of removing the substrate includes: treating the foam material with alkali solution.
7. The PCB manufacturing method according to claim 5, characterized in that: The substrate is made of UV viscosity-reducing material. The step of removing the substrate includes: irradiating the substrate with a UV light source to reduce the viscosity of the UV viscosity-reducing material in the substrate and the conductive paste, and then peeling off the substrate.
8. The PCB manufacturing method according to claim 1, characterized in that: The conductive paste is filled into the groove by screen printing, sputtering or printing.
9. The PCB manufacturing method according to claim 1, characterized in that: The step of aligning and pressing the substrate and the sub-board includes: providing a limit frame and pins, the limit frame having a limit groove, and the substrate is partially arranged in the limit groove, wherein the depth of the limit groove is less than the thickness of the substrate, and the depth of the limit groove is greater than the depth of any one of the grooves.
10. A PCB, characterized in that: The PCB is manufactured by the PCB manufacturing method according to any one of claims 1 to 9.