Polyester-polyurethane-poly (meth) acrylic hybrid dispersions
Through the esterification and free radical polymerization of polyester-polyurethane-poly(meth)acrylic hybrid dispersion, the problem of poor compatibility of multi-layer coatings in automotive coatings is solved, and the preparation of high-solid content coatings is achieved and simplified. It improves the process flow and improves the appearance and leveling effect of the coating.
Patent Information
- Application Number
- CN202380025138.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-04
- Filing Date
- 2023-03-02
- Publication Date
- 2024-10-18
AI Technical Summary
The poor compatibility between multiple layers of coatings in existing automotive coatings results in poor appearance and high production costs. Moreover, traditional processes require a multi-step curing process, which is time-consuming and energy-consuming.
Polyester-polyurethane-poly(meth)acrylic hybrid dispersion is used to prepare high-solid content coating compositions through esterification and free radical polymerization, which reduces the stripping process steps and improves the compatibility and leveling of the coating. Effect.
It achieves good compatibility and excellent appearance within multi-layer coatings, simplifies the production process, reduces time and costs, and improves the leveling effect of the coating.
Smart Images

Figure BDA0005024120580000321 
Figure BDA0005024120580000331 
Figure BDA0005024120580000341
Abstract
Description
[0001] The present invention relates to polyester-polyurethane-poly(meth)acrylic hybrid dispersions and methods for producing polyester-polyurethane-poly(meth)acrylic hybrid dispersions. In addition, the present invention relates to coating compositions comprising polyester-polyurethane-poly(meth)acrylic hybrid dispersions, coatings formed therefrom and substrates coated therewith. In addition, the present invention relates to the use of coating compositions comprising polyester-polyurethane-poly(meth)acrylic hybrid dispersions in automotive coatings and methods for producing multilayer coatings, wherein at least one coating is formed from a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion. Background Art
[0002] The coating of the automobile body is carried out with multi-layer coating. The multi-coat paint system comprises in particular a primer surfacer layer, which is formed on a conventional pre-coated substrate, followed by one or more basecoat layers and a clearcoat layer on top. The individual layers can be individually baked or applied in a wet-on-wet process, wherein a coating is formed on a previous coating without an intermediate curing step. A flash or drying step is required between the two coating steps, wherein the solvent of the coating composition evaporates before applying the subsequent coating. Therefore, it is essential to achieve rapid drying during the flash or drying step to prevent mixing of the coating composition after applying the subsequent coating composition. Rapid drying can be achieved, for example, by a high solids content of the coating composition.
[0003] Nowadays, it is common for automobile bodies to be coated using an integrated wet-on-wet-on-wet application, wherein at least three coating layers are applied in a wet-on-wet-on-wet method. Two integrated painting processes (IPPs) are particularly preferred, wherein integrated painting process 1 (IPP1) comprises forming a primer-surfacer layer by applying a primer-surfacer composition on a preferably electrocoated metal substrate, followed by a flashing or drying step. Subsequently, one or two basecoat compositions are applied on top of the primer-surfacer layer to form one or two basecoat layers, followed by a flashing or drying step. Subsequently, a clearcoat composition is applied on top of the basecoat layer to form a clearcoat layer, which may be followed by a flashing or drying step. Finally, all layers are cured simultaneously in a single curing step.
[0004] In the integrated painting process 2 (IPP2), the preferably electrocoated metal substrate is not coated with a primer-surfacer layer, but two basecoat compositions are applied in a wet-on-wet application to form two basecoat layers, followed by a flashing or drying step, wherein the first basecoat has the function of a primer-surfacer. Thereafter, a clearcoat composition is applied to form a clearcoat layer, followed by a curing step to cure all coating layers simultaneously. The simultaneous curing of all coating layers reduces the energy and material costs of the coating process.
[0005] There are high demands on individual coatings as well as multilayer coatings in terms of environmental issues, compatibility of the individual coatings, good appearance and weather resistance. Excellent appearance requires good compatibility of the different coatings of a multilayer coating.
[0006] Furthermore, it should be possible to produce multilayer coating systems in a simple and inexpensive manner.
[0007] EP 1 199 342 A1 describes the use of adhesive combinations containing water-miscible hydroxyurethanes for increasing the solids content of the corresponding adhesive combinations.
[0008] Polyester-polyurethane-poly(meth)acrylic hybrid dispersions are known from US Pat. No. 10,233,353 B2. However, there is still a need to improve basecoat compositions in order to achieve good compatibility between the different coating layers. Good compatibility of the different coating compositions forming the coating layers in a multilayer coating leads to an excellent appearance of the multilayer coating.
[0009] The object is to provide a coating composition with a high solid content in order to provide a coating composition which has good compatibility with other coating compositions within a multilayer coating and which can be used in an integrated painting process. Therefore, the object is to prepare a coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion with a high solid content. Another object is to provide a polyester-polyurethane-poly(meth)acrylic hybrid dispersion in which a final stripping process is not necessary, thereby reducing the time and cost of preparing such a hybrid dispersion. In addition, the multilayer coating obtained from the coating composition should exhibit an excellent appearance, in particular excellent leveling. Summary of the invention
[0010] The object has been solved by the subject matter of the present application and by its preferred embodiments disclosed in this specification.
[0011] The first subject of the present invention is a polyester-polyurethane-poly(meth)acrylic hybrid dispersion obtainable by:
[0012] a. Esterify the following:
[0013] at least one polyurethane containing carboxyl groups, the at least one polyurethane having an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups; and
[0014] at least one polyester containing hydroxyl groups, the polyester having a hydroxyl number of 50 mg KOH / g to 300 mg KOH / g,
[0015] to obtain polyester-polyurethane; followed by
[0016] b. polymerizing ethylenically unsaturated monomers comprising at least (meth)acrylic monomers by free radical polymerization in the presence of the polyester-polyurethane of step (a) to obtain poly(meth)acrylate, wherein one or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b).
[0017] The present invention further provides a process for producing the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention by:
[0018] a. Esterify the following:
[0019] at least one polyurethane containing carboxyl groups, the at least one polyurethane having an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups; and
[0020] at least one polyester containing hydroxyl groups, the polyester having a hydroxyl number of 50 mg KOH / g to 300 mg KOH / g,
[0021] to obtain polyester-polyurethane; followed by
[0022] b. polymerizing ethylenically unsaturated monomers comprising at least (meth)acrylic monomers by free radical polymerization in the presence of the polyester-polyurethane of step (a) to obtain poly(meth)acrylate, wherein one or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b).
[0023] Another object of the present invention is a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention.
[0024] Another object of the present invention is a coating formed from a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention and a substrate coated therewith.
[0025] Another object of the present invention is the use of a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention in automotive coatings.
[0026] Yet another object of the present invention is a method for producing a multilayer coating, the method comprising the following steps:
[0027] a. applying one or more basecoat compositions to a substrate to form one or more basecoat layers, wherein at least one basecoat composition comprises a polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention,
[0028] b. applying a clearcoat composition on top of the one or more basecoat layers to form a clearcoat layer,
[0029] c. simultaneously curing the one or more basecoat layers and the clearcoat layer or individually curing one or more layers obtained in steps (a) and (b) and then applying a subsequent coating or individually curing all layers obtained in steps (a) and (b).
[0030] Preferred embodiments of the polyester-polyurethane-poly(meth)acrylic hybrid dispersions and coating compositions of the invention are apparent from the following description and also from the dependent claims. DETAILED DESCRIPTION
[0031] definition
[0032] First, the terms used in the context of the present invention will be explained.
[0033] The term "hybrid dispersion" according to the present invention describes a dispersion comprising polyester-polyurethane and poly(meth)acrylate. The polyester-polyurethane can be physically mixed with the poly(meth)acrylate and / or covalently bonded to the poly(meth)acrylate.
[0034] The expression "aqueous coating composition" is known to the skilled person. It refers to a coating composition, wherein the volatile part of the coating composition is essentially based on water. In the context of the present invention, "aqueous" is therefore understood to mean that the coating composition preferably comprises a water fraction of at least 40 wt.-%, more preferably at least 50 wt.-%, most preferably at least 60 wt.-%, in each case based on the total amount of solvents present (i.e. water and organic solvents).
[0035] The term "aliphatic" is used according to the IUPAC definition and includes all acyclic or cyclic, saturated or unsaturated carbon compounds, excluding aromatic compounds.
[0036] The term "polymer" describes a substance that is composed of a plurality of monomer entities, differing in degree of polymerization, molar mass and chain length. The monomer entities may be identical or different. In the context of the present invention, a "polymer" substance also includes oligomeric substances.
[0037] In the context of the present invention, polyfunctional alcohols or isocyanates describe molecules having at least two functional groups and therefore also include difunctional alcohols or isocyanates.
[0038] The term "(meth)acrylic" describes materials which include methacrylate and / or methacrylic acid and / or acrylate and / or acrylic acid.
[0039] Polyester-polyurethane-poly(meth)acrylic hybrid dispersion
[0040] Polyester-polyurethane-poly(meth)acrylic hybrid dispersion, which can be obtained by:
[0041] a. Esterify the following:
[0042] at least one polyurethane containing carboxyl groups, the at least one polyurethane having an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups; and
[0043] at least one polyester containing hydroxyl groups, the polyester having a hydroxyl number of 50 mg KOH / g to 300 mg KOH / g,
[0044] to obtain polyester-polyurethane; followed by
[0045] b. polymerizing ethylenically unsaturated monomers comprising at least (meth)acrylic monomers by free radical polymerization in the presence of the polyester-polyurethane of step (a) to obtain poly(meth)acrylate, wherein one or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b).
[0046] In the presence of the polyester-polyurethane obtained in step (a), the ethylenically unsaturated monomers in step (b) are polymerized to obtain the poly(meth)acrylate. Thus, the polyester-polyurethane of step (a) may be physically mixed with the poly(meth)acrylate of step (b) and / or covalently bonded to the poly(meth)acrylate of step (b). The poly(meth)acrylate of step (b) may be covalently bonded to the polyester-polyurethane of step (a), for example if the polyester-polyurethane of step (a) contains ethylenically unsaturated groups and / or if free radical formation within the polyester-polyurethane of step (a) occurs by hydrogen abstraction resulting in attachment of ethylenically unsaturated (meth)acrylic monomers to the polyester-polyurethane. Thus, there is no better way to describe the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention than by the method of obtaining it.
[0047] The polyester-polyurethane-poly(meth)acrylic hybrid dispersion is obtainable by the following reaction steps (a) and (b).
[0048] Step a
[0049] The polyester-polyurethane is obtained by esterifying at least one polyurethane containing carboxyl groups, the at least one polyurethane having an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups, with at least one polyester containing hydroxyl groups, the polyester having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g.
[0050] i. Synthesis of polyurethane
[0051] At least one polyurethane is synthesized by reacting one or more diisocyanates with one or more diols and one or more carboxyl group-containing and / or carboxyl group-forming monomers.
[0052] The diols may be saturated or ethylenically unsaturated, more preferably saturated, wherein the saturated or ethylenically unsaturated diols may be substituted or unsubstituted. The diols may be aromatic or aliphatic, more preferably aliphatic. The aliphatic diols may be linear, branched or cyclic, preferably having 2 to 40 carbon atoms, more preferably 2 to 20 carbon atoms, even more preferably 2 to 16 carbon atoms, most preferably 4 to 10 carbon atoms. Preferably, at least one diol is substituted, more preferably, the substituted diol comprises one or more carboxyl groups.
[0053] Examples of suitable saturated monomeric diols are ethylene glycol, neopentyl glycol, tripropylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 2,2-bis(4-hydroxy-cyclohexyl)-propane, dimethylolpropionic acid and dimethylolbutanoic acid. The saturated monomeric diol is preferably ethylene glycol and / or dimethylolpropionic acid.
[0054] The ethylenically unsaturated diol preferably comprises at least one allyl, vinyl, acryloyl or methacryloyl group.Examples of ethylenically unsaturated monomeric diols are trimethylolpropane monoallyl ether and pentaerythritol monoallyl ether.
[0055] Preferably, the one or more diols are ethylene glycol and / or dimethylolpropionic acid.
[0056] At least one diol is reacted with one or more diisocyanates to synthesize the polyurethane. The one or more diisocyanates may be aromatic or aliphatic, more preferably aliphatic. The aliphatic diisocyanate may be linear or cyclic, more preferably cyclic.
[0057] Suitable examples of cycloaliphatic diisocyanates are isophorone diisocyanate (=5-isocyanato-1-isocyanatomethyl-1,3,3-trimethylcyclohexane), 5-isocyanato-1-(2-isocyanatoethyl-1-yl)-1,3,3-trimethylcyclohexane, 5-isocyanato-1-(3-isocyanatopropyl-1-yl)-1,3,3-trimethylcyclohexane, 5-isocyanato-(4-isocyanatobutyl-1-yl)-1,3,3-trimethylcyclohexane, 1-isocyanato-2-(3-isocyanatopropyl-1-yl)-1,3,3-trimethylcyclohexane, )cyclohexane, 1-isocyanato-2-(2-isocyanatoethyl-1-yl)cyclohexane, 1-isocyanato-2-(4-isocyanatobutyl-1-yl)cyclohexane, 1,2-diisocyanatocyclobutane, 1,3-diisocyanatocyclobutane, 1,2-diisocyanatocyclopentane, 1,3-diisocyanatocyclopentane, 1,2-diisocyanatocyclohexane, 1,3-diisocyanatocyclohexane, 1,4-diisocyanatocyclohexane, dicyclohexylmethane 2,4'-diisocyanate and 4,4'-methylenebis(cyclohexyl isocyanate).
[0058] Suitable examples of aromatic diisocyanates are 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, diphenylmethane-4,4′-diisocyanate, p-phenylene diisocyanate, biphenyl diisocyanate, 3,3′-dimethyl-4,4′-diphenylene diisocyanate and tetramethylxylene diisocyanate.
[0059] Examples of linear aliphatic diisocyanates are ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexane-1,6-diisocyanate, heptamethylene diisocyanate and 1,12-dodecane diisocyanate.
[0060] The one or more diisocyanates are preferably isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate) and / or tetramethylxylene diisocyanate.
[0061] One or more diisocyanates preferably react with one or more diols in a solvent. The solvent is preferably an organic solvent. Suitable examples of organic solvents for the present invention include heterocyclic, aliphatic or aromatic hydrocarbons, mono- or polyfunctional alcohols, ethers, esters, ketones and amides, such as N-methyl pyrrolidone, N-ethyl pyrrolidone, dimethyl formamide, toluene, xylene, butanol, ethylene glycol and butanediol and their acetates, butyl diglycol, diethylene glycol dimethyl ether, cyclohexanone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), acetone, isophorone, or a mixture thereof. Preferably, the organic solvent is methyl ethyl ketone (MEK).
[0062] The hydroxy-terminated polyurethanes thus obtained can be synthesized in a one-step process or a two-step process. In the one-step process, one or more diisocyanates are reacted with one or more diols, wherein the diols are used in excess to prepare the hydroxy-terminated polyurethanes. In the two-step process, one or more diisocyanates are first reacted with one or more diols. Subsequently, one or more diols are added to react the terminal NCO groups to prepare the hydroxy-terminated polyurethanes. In the two-step process, the one or more diols reacted with the free isocyanate groups are preferably ethylene glycol.
[0063] One or more diisocyanates are reacted with one or more diols until preferably less than 2 wt.-%, most preferably less than 1 wt.-%, of NCO groups, based on the weight of the polyurethane, are converted. The polyurethane is thus substantially free of free NCO groups, wherein the isocyanate content (NCO content) is determined by adding an excess of a 2% N,N-dibutylamine solution in xylene to a homogeneous solution of the sample in acetone / N-ethylpyrrolidone (1:1 Vol.-%) by potentiometric back titration of the amine excess with 0.1 N hydrochloric acid in accordance with DIN EN ISO 3251, DIN EN ISO 11909 and DIN EN ISO 14886.
[0064] The hydroxyl-terminated polyurethane thus obtained is reacted with one or more carboxyl-containing monomers and / or monomers containing carboxyl-forming groups. Such monomers are preferably polycarboxylic acids and their anhydrides, preferably dicarboxylic acids, tricarboxylic acids and / or their anhydrides. The term "carboxyl-forming groups" refers to the ability of the functional groups to form carboxyl groups, preferably by hydrolysis of the corresponding anhydride groups or ester groups.
[0065] The polycarboxylic acids and their anhydrides may be aromatic or aliphatic and preferably have 2 to 20 carbon atoms, more preferably 2 to 16 carbon atoms, even more preferably 4 to 12 carbon atoms, most preferably 6 to 10 carbon atoms.
[0066] Examples of suitable aliphatic dicarboxylic acids are oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, hexahydrophthalic acid and the corresponding anhydrides.
[0067] Examples of suitable aromatic dicarboxylic acids are 1,2-phthalic acid (orthophthalic acid), 1,3-phthalic acid (isophthalic acid) and 1,4-phthalic acid (terephthalic acid) and the corresponding anhydrides.
[0068] Suitable tricarboxylic acids are citric acid, isocitric acid, aconitic acid, propane-1,2,3-tricarboxylic acid, agaric acid, trimesic acid, trimellitic acid and the corresponding anhydrides.
[0069] Preferably, the hydroxyl terminated polyurethane is reacted with trimellitic anhydride.
[0070] The reaction is stopped at a constant acid value. The obtained polyurethane has at least one terminal carboxyl group, preferably the polyurethane has one or more terminal carboxyl groups and one or more carboxyl groups in the main chain, more preferably the polyurethane has at least two carboxyl groups / terminal, and most preferably the polyurethane has at least two carboxyl groups / terminal and contains one or more carboxyl groups in the main chain.
[0071] The polyurethane obtained may be linear or branched, preferably linear.
[0072] The polyurethane obtained has an acid number of greater than 200 mg KOH / g to 400 mg KOH / g, preferably greater than 205 mg KOH / g to 350 mg KOH / g, more preferably greater than 210 mg KOH / g to 300 mg KOH / g, even more preferably greater than 220 mg KOH / g to 300 mg KOH / g, most preferably 240 mg KOH / g to 300 mg KOH / g, determined according to DIN EN ISO 2114.
[0073] Preferably, the polyurethane obtained has a hydroxyl number in the range of 0 mg KOH / g to 50 mg KOH / g, more preferably 0 mg KOH / g to 46 mg KOH / g, even more preferably 0 mg KOH / g to 42 mg KOH / g, most preferably 0 mg KOH / g to 40 mg KOH / g, as determined according to R.-P. Krüger, R. Gnauck and R. Algeier (Plaste und Kautschuk [Plastics and Rubber], 20, 274 (1982)) using acetic anhydride in the presence of 4-dimethylaminopyridine as catalyst in tetrahydrofuran (THF) / dimethylformamide (DMF) solution at room temperature.
[0074] Subsequently, the polyurethane obtained is diluted with a solvent, preferably an organic solvent, to a solids content of preferably 60 to 80 wt.-%, more preferably 65 to 75 wt.-%, determined in accordance with DIN EN ISO 3251 at 130° C. for 60 min using 1.0 g weighed portions.
[0075] ii. Synthesis of polyester
[0076] The at least one polyester is synthesized by reacting one or more polyols with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic anhydrides. The at least one polyester may be saturated or ethylenically unsaturated.
[0077] The polyols may be saturated or ethylenically unsaturated, more preferably saturated, wherein the saturated or ethylenically unsaturated polyols may be substituted or unsubstituted. The polyols may be aromatic or aliphatic, more preferably aliphatic. The aliphatic polyols may be linear, branched or cyclic, preferably having 2 to 40 carbon atoms, more preferably 2 to 20 carbon atoms, even more preferably 2 to 16 carbon atoms, most preferably 4 to 10 carbon atoms.
[0078] Examples of suitable saturated monomeric polyols are ethylene glycol, neopentyl glycol, tripropylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 2,2-bis(4-hydroxy-cyclohexyl)-propane, trimethylolpropane, trimethylolethane, trimethylolhexane, glycerol, 1,2,4-butanetriol, ditrimethylolpropane, pentaerythritol and dipentaerythritol.
[0079] The ethylenically unsaturated polyol preferably comprises at least one allyl, vinyl, acryloyl or methacryloyl group.Examples of ethylenically unsaturated monomeric polyols are trimethylolpropane monoallyl ether and pentaerythritol-diallyl ether.
[0080] Preferably, the one or more polyols are neopentyl glycol, tripropylene glycol, 1,6-hexanediol and / or trimethylolpropane.
[0081] At least one polyol is reacted with one or more monomers selected from the group consisting of dicarboxylic acids, tricarboxylic acids, and cyclic anhydrides to synthesize the polyester.
[0082] The dicarboxylic acid may be aromatic or aliphatic, preferably having 2 to 50 carbon atoms, more preferably 2 to 44 carbon atoms, even more preferably 4 to 44 carbon atoms, most preferably 6 to 44 carbon atoms.
[0083] Examples of suitable aliphatic dicarboxylic acids are oxalic acid (oxalic acid), malonic acid (malic acid), succinic acid (succinic acid), glutaric acid (gum acid), adipic acid (fatty acid), pimelic acid (syrupylic acid), suberic acid (suberic acid), azelaic acid (azoloic acid), sebacic acid (sebaceous acid), maleic acid and hexahydrophthalic acid. Preferably, adipic acid (fatty acid) is used as the aliphatic dicarboxylic acid.
[0084] Examples of suitable aromatic dicarboxylic acids are 1,2-phthalic acid (orthophthalic acid), 1,3-phthalic acid (isophthalic acid) and 1,4-phthalic acid (terephthalic acid).
[0085] Another possibility is to use dimer fatty acids as polycarboxylic acids. Dimer fatty acids are mixtures produced by oligomerization of unsaturated fatty acids.12 To C 22 Fatty acids are used as starting materials. Suitable dimer fatty acids are, for example, Radiacid 0970, Radiacid 0971, Radiacid 0972, Radiacid 0975, Radiacid 0976, Radiacid 0977, Pripol 1006, Pripol 1009, Pripol 1012 and Pripol 1013, Empol 1008, Empol 1061 and Empol 1062 (WO 2015 / 028201 A1).
[0086] Preferably, the dicarboxylic acid is aromatic, more preferably isophthalic acid.
[0087] Suitable tricarboxylic acids are citric acid, isocitric acid, aconitic acid, propane-1,2,3-tricarboxylic acid, agaric acid, trimesic acid and trimellitic acid.
[0088] The cyclic anhydride preferably has 2 to 40 carbon atoms, more preferably 2 to 30 carbon atoms, even more preferably 4 to 20 carbon atoms, most preferably 6 to 18 carbon atoms.The cyclic anhydride may be saturated or ethylenically unsaturated.
[0089] Examples of suitable cyclic anhydrides are phthalic anhydride, trimellitic anhydride, maleic anhydride and its derivatives and alkenyl succinic anhydrides such as tetrapropenyl succinic anhydride. Preferably, the one or more cyclic anhydrides are phthalic anhydride, trimellitic anhydride and / or tetrapropenyl succinic anhydride.
[0090] One or more polyols are reacted with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic anhydrides at a temperature of preferably 200 to 250°C, more preferably 210 to 240°C.
[0091] The hydroxyl number of the polyesters obtained is from 50 to 300 mg KOH / g, preferably from 60 to 280 mg KOH / g, more preferably from 70 to 250 mg KOH / g, even more preferably from 100 to 250 mg KOH / g, most preferably from 120 to 250 mg KOH / g, as determined according to R.-P. Krüger, R. Gnauck and R. Algeier (Plaste und Kautschuk [Plastics and Rubber], 20, 274 (1982)) using acetic anhydride in the presence of 4-dimethylaminopyridine as catalyst in tetrahydrofuran (THF) / dimethylformamide (DMF) solution at room temperature.
[0092] Preferably, the acid number of the obtained polyester is less than 20 mg KOH / g, more preferably less than 18 mg KOH / g, even more preferably less than 15 mg KOH / g, most preferably less than 12 mg KOH / g, determined according to DIN EN ISO 2114.
[0093] The polyester obtained may be linear or branched, preferably branched.
[0094] iii. Synthesis of polyester-polyurethane (PEU) or polyester-polyurethane dispersion (PEUD)
[0095] The polyester and the polyurethane are mixed and the temperature is carefully raised to preferably 120° C. to 180° C., more preferably 130° C. to 170° C., while applying reduced pressure. Preferably, the pressure is 15 mbar to 80 mbar, more preferably 15 mbar to 70 mbar. The process can be monitored by titration and viscosity measurement at 140° C. The reaction is stopped when an acid value of preferably 10 mg KOH / g to 50 mg KOH / g, more preferably 15 mg KOH / g to 45 mg KOH / g, most preferably 20 mg KOH / g to 40 mg KOH / g and / or a viscosity of preferably 1000 mPa*s to 2400 mPa*s, more preferably 1200 mPa*s to 2200 mPa*s, most preferably 1300 mPa*s to 2000 mPa*s is reached, the viscosity being measured at a temperature of 140° C. using a CAP2000H viscometer with spindle 03 for 1250 s -1 The shear rate is determined according to DIN EN ISO 2884-1. The temperature is lowered to a temperature of preferably 60°C to 120°C, more preferably 70°C to 115°C.
[0096] The polyester-polyurethane may be neutralized with a neutralizing agent prior to the addition of one or more solvents or reacted with at least one ethylenically unsaturated monomer as outlined in step b without the addition of one or more solvents.
[0097] Suitable examples of neutralizing agents are alkylalkanolamines, such as dimethylethanolamine (DMEA), diethylethanolamine (DEEA), methyldiethanolamine (MDEA) or methylethanolamine (NMEA). Preferably, dimethylethanolamine is used as neutralizing agent.
[0098] One or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b), wherein the solvent may be present during the preparation of the polyester and / or polyurethane and / or during the esterification of the polyester and polyurethane during step (a) and / or during step (b), wherein the solvent may be present before, during and / or after the addition of the (meth)acrylic monomer and / or the free radical initiator. The at least one polyurethane and the at least one polyester in step (a) may be esterified in the presence of one or more solvents to obtain a polyester-polyurethane dispersion.
[0099] The solvent may be water or an organic solvent. Preferably, water is added to adjust the solids content and produce an aqueous polyester-polyurethane dispersion.
[0100] Preferably, the synthetic polyester-polyurethane dispersion has a solids content of ≥40 wt.-%, more preferably ≥42 wt.-%, even more preferably ≥45 wt.-%, most preferably ≥48 wt.-%, determined in accordance with DIN EN ISO 3251 at 130° C. for 60 min using 1.0 g weighed portions.
[0101] Preferably, the polyester-polyurethane dispersion exhibits a viscosity of 100 to 300 mPa*s, more preferably 110 to 290 mPa*s, even more preferably 120 to 280 mPa*s, most preferably 130 to 260 mPa*s, as measured using a Rheolab QC rotational rheometer with a cylinder cc 27 at a temperature of 23°C using 1000 s -1 The shear rate is determined according to DIN 53019-1.
[0102] Preferably, the polyester-polyurethane has an acid number in the range of 10 mg KOH / g to 50 mg KOH / g, more preferably 15 mg KOH / g to 45 mg KOH / g, even more preferably 20 mg KOH / g to 40 mg KOH / g, most preferably 25 mg KOH / g to 35 mg KOH / g, determined according to DIN EN ISO 2114.
[0103] Preferably, the polyester-polyurethane has a particle size of 50 nm to 200 nm, more preferably 70 nm to 180 nm, even more preferably 80 nm to 150 nm, most preferably 90 nm to 130 nm, as determined by measuring the hydrodynamic volume / hydrodynamic radius of the dispersion particles using photon correlation spectroscopy (PCS).
[0104] Preferably, the polyester-polyurethane has a number average molecular weight (M) of 1,000 g / mol to 3,500 g / mol, more preferably 1,200 g / mol to 3,200 g / mol, even more preferably 1,500 g / mol to 3,000 g / mol, most preferably 1,800 g / mol to 2,800 g / mol. n ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0105] Preferably, the polyester-polyurethane has a weight average molecular weight (M) of 6,000 g / mol to 50,000 g / mol, more preferably 7,000 g / mol to 48,000 g / mol, even more preferably 8,000 g / mol to 46,000 g / mol, most preferably 9,000 g / mol to 43,000 g / mol. w ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0106] Step b
[0107] In the presence of the polyester-polyurethane of step (a), ethylenically unsaturated monomers including at least a (meth)acrylic monomer are polymerized by free radical polymerization to obtain poly(meth)acrylate.
[0108] The ethylenically unsaturated monomers in step (b) are added to the polyester-polyurethane dispersion or the undiluted polyester-polyurethane of step (a) before, simultaneously with and / or after the addition of the free radical initiator. If the ethylenically unsaturated monomers are added to the polyester-polyurethane of step (a) before the addition of the free radical initiator, the ethylenically unsaturated monomers and the polyester-polyurethane of step (a) are preferably incubated at a temperature of preferably 20° C. to 30° C. for at least 10 min, more preferably at least 30 min, even more preferably at least 60 min, most preferably at least 2 hours such as for example at least 4 hours.
[0109] A solvent may be added to the polyester-polyurethane before or after the addition of the (meth) acrylic monomer or the free radical initiator to obtain a polyester-polyurethane dispersion comprising the (meth) acrylic monomer. The solvent may be water or an organic solvent. Preferably, water is added to adjust the solid content and produce an aqueous polyester-polyurethane dispersion.
[0110] The ethylenically unsaturated monomer may be a cyclic, linear or branched alkyl (meth)acrylate, a hydroxyalkyl (meth)acrylate, (meth)acrylic acid and / or a vinyl aromatic hydrocarbon, wherein the ethylenically unsaturated monomer may be monoethylenically unsaturated or polyethylenically unsaturated, wherein the functionality of the polyethylenically unsaturated monomer may be in the range of two to five. Preferably, the polyethylenically unsaturated monomer is diethylenically unsaturated or triethylenically unsaturated, most preferably diethylenically unsaturated. Preferably, the ethylenically unsaturated monomer is a monoethylenically unsaturated monomer or a mixture of a monoethylenically unsaturated monomer and a diethylenically unsaturated monomer.
[0111] Suitable cyclic, linear or branched alkyl (meth)acrylates are cyclohexyl (meth)acrylate and alkyl (meth)acrylates having up to 20 carbon atoms. Preferred monoethylenically unsaturated alkyl (meth)acrylates are tert-butyl acrylate, n-butyl acrylate, n-butyl methacrylate, methyl methacrylate, ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, most preferably tert-butyl acrylate, n-butyl acrylate, n-butyl methacrylate and ethylhexyl methacrylate.
[0112] Suitable hydroxyalkyl (meth)acrylates are those in which the hydroxyalkyl group contains up to 6 carbon atoms, preferably 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate.
[0113] Suitable diethylenically unsaturated monomers are ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,2-propylene glycol di(meth)acrylate, 1,3-propylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, allyl(meth)acrylate and divinylbenzene. Suitable multiethylenically unsaturated monomers are trimethylolpropane tri(meth)acrylate, pentaerythritol tri- and tetraacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate and ethoxylated 3-trimethylolpropane triacrylate.
[0114] Suitable vinylaromatic hydrocarbons are styrene, α-alkylstyrenes, vinyltoluene, (meth)acrylamide and (meth)acrylonitrile.
[0115] Preferably, the ethylenically unsaturated monomer in step (b) is an alkyl (meth)acrylate, more preferably tert-butyl acrylate, n-butyl acrylate, n-butyl methacrylate and ethylhexyl methacrylate.
[0116] The ethylenically unsaturated monomers of step (b) are added to the polyester-polyurethane of step (a) prior to or simultaneously with the addition of the free radical initiator.
[0117] To initiate the free radical polymerization, water-soluble or water-insoluble initiators can be used. Examples of water-soluble initiators are hydrogen peroxide, peroxodisulfate salts such as sodium peroxodisulfate, potassium peroxodisulfate and ammonium peroxodisulfate, ammonium salts of 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methyl-N-1,1-bis(hydroxymethyl)ethyl)propionamide, 2,2'-azobis(2-methyl-N-2-hydroxyethyl)propionamide). Preferably, ammonium peroxodisulfate (APS) is used as a water-soluble initiator.
[0118] Examples of water-insoluble initiators are tert-butyl-peroxy-2-ethylhexanol, tert-butyl peroxypivalate and dibenzoyl peroxide. Preferably, tert-butyl-peroxy-2-ethylhexanol is used as the water-insoluble initiator.
[0119] Preferably, the free radical polymerization is initiated by a water-insoluble initiator, more preferably by tert-butyl-peroxy-2-ethylhexanol.
[0120] The free radical initiator generates free radicals in the ethylenically unsaturated polyester-polyurethane polymer and / or in the ethylenically unsaturated monomer. Thus, a poly(meth)acrylate is obtained, which can be physically mixed with the polyester-polyurethane of step (a) or covalently bonded to the polyester-polyurethane of step (a). For example, the poly(meth)acrylate can be covalently bonded to the polyester-polyurethane of step (a) by forming a graft polymer formed by free radical copolymerization of ethylenically unsaturated monomers and ethylenically unsaturated groups in the main chain of the polyester-polyurethane of step (a), and / or H-deoxygenation on the main chain of the polyester-polyurethane of step (a).
[0121] Preferably, the solids content of the obtained polyester-polyurethane-poly(meth)acrylic hybrid dispersion is ≥40 wt.-%, more preferably ≥42 wt.-%, even more preferably ≥43 wt.-%, even more preferably ≥44 wt.-%, even more preferably ≥48 wt.-%, most preferably ≥50 wt.-%, determined in accordance with DIN EN ISO 3251 at 130° C. for 60 min using 1.0 g weighed portions.
[0122] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has a glass transition temperature of -50°C to +50°C, more preferably -48°C to 40°C, even more preferably -45°C to 35°C, most preferably -45°C to 30°C, measured according to DIN-EN-ISO 11357-1 and -2.
[0123] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a number average molecular weight (M) of 2,500 g / mol to 5,000 g / mol, more preferably 2,700 g / mol to 4,800 g / mol, most preferably 3,000 g / mol to 4,500 g / mol. n ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0124] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a weight average molecular weight (MW) of 25,000 to 550,000 g / mol, more preferably 30,000 to 500,000 g / mol, even more preferably 50,000 to 450,000 g / mol, most preferably 100,000 to 400,000 g / mol. w ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0125] The number average molecular weight (M) of the polyester-polyurethane-poly(meth)acrylic hybrid prepared using at least one multiethylenically unsaturated monomer, preferably at least one diethylenically unsaturated monomer, is n ) and weight average molecular weight (M w ) can be even higher than the number average molecular weight (M) as described in the two paragraphs above. n ) and weight average molecular weight (M w ).
[0126] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has an acid number of 5 mg KOH / g to 50 mg KOH / g, more preferably 10 mg KOH / g to 45 mg KOH / g, even more preferably 15 mg KOH / g to 40 mg KOH / g, even more preferably 15 mg KOH / g to 35 mg KOH / g, most preferably 15 mg KOH / g to 30 mg KOH / g, which is determined according to DIN EN ISO 2114.
[0127] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion has a viscosity of 5 mPa*s to 3,000 mPa*s, more preferably 10 mPa*s to 2,500 mPa*s, even more preferably 10 mPa*s to 1000 mPa*s, even more preferably 10 mPa*s to 500 mPa*s, most preferably 10 mPa*s to 200 mPa*s, the viscosity being measured using a Rheolab QC rotational rheometer at a temperature of 23° C. using 1000 s -1 The shear rate is determined according to DIN 53019-1.
[0128] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion has a particle size of 50 nm to 400 nm, more preferably 70 nm to 300 nm, even more preferably 100 nm to 250 nm, most preferably 120 nm to 220 nm, as determined by measuring the hydrodynamic volume / hydrodynamic radius of the dispersion particles using photon correlation spectroscopy (PCS).
[0129] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion comprises 45 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 55 wt.-% of the poly(meth)acrylate obtainable by step (b), more preferably 50 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 50 wt.-% of the poly(meth)acrylate obtainable by step (b), even more preferably 50 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 50 wt.-% of the poly(meth)acrylate obtainable by step (b), based on the solids content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion. 55 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 45 wt.-% of the poly(meth)acrylate obtainable by step (b), even more preferably 60 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 40 wt.-% of the poly(meth)acrylate obtainable by step (b), most preferably 65 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 35 wt.-% of the poly(meth)acrylate obtainable by step (b).
[0130] Process for producing polyester-polyurethane-poly(meth)acrylic hybrid dispersions
[0131] The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention is produced by esterifying in a first step (a): at least one polyurethane containing carboxyl groups, the at least one polyurethane having an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups; with at least one polyester containing hydroxyl groups, the polyester having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g, to obtain a polyester-polyurethane; followed by a second step (b), wherein ethylenically unsaturated monomers comprising at least a (meth)acrylic monomer are polymerized by free radical polymerization in the presence of the polyester-polyurethane of step (a) to obtain a poly(meth)acrylate, wherein one or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b).
[0132] Step (a): Preparation of polyester-polyurethane (PEU) or polyester-polyurethane dispersion (PEUD)
[0133] The polyester-polyurethane of the polyester-polyurethane-poly(meth)acrylic dispersion is produced by esterifying at least one polyurethane containing carboxyl groups, wherein the at least one polyurethane has an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups; and at least one polyester containing hydroxyl groups, wherein the polyester has a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g.
[0134] Polyurethane is synthesized by reacting one or more diisocyanates with one or more diols and one or more carboxyl-containing and / or carboxyl-forming monomers. The diols, diisocyanates and carboxyl-containing and / or carboxyl-forming monomers are the same as those described above in the synthesis of polyurethane in item i.
[0135] The one or more diisocyanates are reacted with the one or more diols until preferably less than 2 wt.-%, most preferably less than 1 wt.-%, of the NCO groups, based on the weight of the polyurethane, are converted. The polyurethane thus contains essentially no free NCO groups.
[0136] The hydroxy-terminated polyurethane thus obtained is reacted with one or more carboxyl-containing and / or carboxyl-forming group-containing monomers. Such monomers are preferably polycarboxylic acids and their anhydrides, preferably dicarboxylic acids, tricarboxylic acids and / or their anhydrides. Suitable dicarboxylic acids, tricarboxylic acids and their anhydrides have already been indicated above.
[0137] Preferably, the hydroxyl terminated polyurethane is reacted with trimellitic anhydride.
[0138] The reaction is stopped at a constant acid value. The obtained polyurethane has at least one terminal carboxyl group, preferably the polyurethane has one or more terminal carboxyl groups and one or more carboxyl groups in the main chain, more preferably the polyurethane has at least two carboxyl groups / terminal, and most preferably the polyurethane has at least two carboxyl groups / terminal and contains one or more carboxyl groups in the main chain.
[0139] The polyurethane obtained may be linear or branched, preferably linear.
[0140] The polyurethane obtained has an acid number of greater than 200 mg KOH / g to 400 mg KOH / g, preferably greater than 205 mg KOH / g to 350 mg KOH / g, more preferably greater than 210 mg KOH / g to 300 mg KOH / g, even more preferably greater than 220 mg KOH / g to 300 mg KOH / g, most preferably 240 mg KOH / g to 300 mg KOH / g, determined according to DIN EN ISO 2114.
[0141] Subsequently, the polyurethane obtained is diluted with a solvent, preferably an organic solvent, to a solids content of preferably 60 to 80 wt.-%, more preferably 65 to 75 wt.-%, determined in accordance with DIN EN ISO 3251 at 130° C. for 60 min using 1.0 g weighed portions.
[0142] At least one polyester is synthesized by reacting one or more polyols with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic anhydrides. The polyols and one or more monomers selected from the group consisting of dicarboxylic acids and cyclic anhydrides are the same as the polyols and monomers selected from the group consisting of dicarboxylic acids and anhydrides described above in the synthesis of the polyester in item ii.
[0143] One or more polyols are reacted with one or more monomers selected from the group consisting of dicarboxylic acids and cyclic anhydrides at a temperature of preferably 200°C to 250°C, more preferably 210°C to 240°C.
[0144] The polyester obtained may be linear or branched, preferably branched.
[0145] The hydroxyl number of the polyesters obtained is from 50 to 300 mg KOH / g, preferably from 60 to 280 mg KOH / g, more preferably from 70 to 250 mg KOH / g, even more preferably from 100 to 250 mg KOH / g, most preferably from 120 to 250 mg KOH / g, as determined according to R.-P. Krüger, R. Gnauck and R. Algeier (Plaste und Kautschuk [Plastics and Rubber], 20, 274 (1982)) using acetic anhydride in the presence of 4-dimethylaminopyridine as catalyst in tetrahydrofuran (THF) / dimethylformamide (DMF) solution at room temperature.
[0146] The acid number of the obtained polyester is less than 20 mg KOH / g, preferably less than 18 mg KOH / g, more preferably less than 15 mg KOH / g, most preferably less than 12 mg KOH / g, determined according to DIN EN ISO 2114.
[0147] The polyester and the polyurethane are mixed and the temperature is carefully raised to preferably 120° C. to 180° C., more preferably 130° C. to 170° C., while applying reduced pressure. Preferably, the pressure is 15 mbar to 80 mbar, more preferably 15 mbar to 70 mbar. The process is monitored by titration and viscosity measurement at 140° C. Preferably, the reaction is stopped when an acid number of preferably 10 to 50 mg KOH / g, more preferably 15 to 45 mg KOH / g, most preferably 20 mg KOH / g to 40 mg KOH / g and / or a viscosity of preferably 1000 mPa*s to 2400 mPa*s, more preferably 1200 mPa*s to 2200 mPa*s, most preferably 1300 mPa*s to 2000 mPa*s is reached, the viscosity being measured at a temperature of 140° C. using a CAP2000H viscometer with spindle 03 for 1250 s -1 The shear rate is determined according to DIN EN ISO 2884-1.
[0148] The temperature is lowered to a temperature of preferably 60°C to 120°C, more preferably 70°C to 115°C.
[0149] The polyester-polyurethane may be neutralized with a neutralizing agent prior to the addition of one or more solvents or reacted with at least one ethylenically unsaturated monomer as outlined in step (b) without the addition of one or more solvents.
[0150] Suitable examples of neutralizing agents are alkylalkanolamines, such as dimethylethanolamine (DMEA), diethylethanolamine (DEEA), methyldiethanolamine (MDEA) or methylethanolamine (NMEA). Preferably, dimethylethanolamine is used as neutralizing agent.
[0151] One or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b), wherein the solvent may be present during the preparation of the polyester and / or polyurethane and / or during the esterification of the polyester and polyurethane during step (a) and / or during step (b), wherein the solvent may be present before, during and / or after the addition of the (meth)acrylic monomer and / or the free radical initiator. The at least one polyurethane and the at least one polyester in step (a) may be esterified in the presence of one or more solvents to obtain a polyester-polyurethane dispersion.
[0152] Preferably, a solvent is added to adjust the solid content of the polyester-polyurethane dispersion. The solvent may be water or an organic solvent. Preferably, water is added to adjust the solid content and produce an aqueous polyester-polyurethane dispersion.
[0153] Preferably, the synthetic polyester-polyurethane dispersion has a solids content of ≥40 wt.-%, more preferably ≥42 wt.-%, most preferably ≥45 wt.-%, determined according to DIN EN ISO 3251 at 130° C. for 60 min using 1.0 g weighed portions.
[0154] Preferably, the polyester-polyurethane dispersion exhibits a viscosity of 100 to 300 mPa*s, more preferably 110 to 290 mPa*s, even more preferably 120 to 280 mPa*s, most preferably 130 to 260 mPa*s, as measured using a Rheolab QC rotational rheometer with a cylinder cc 27 at a temperature of 23°C using 1000 s -1 The shear rate is determined according to DIN 53019-1.
[0155] Preferably, the polyester-polyurethane has an acid number in the range of 10 mg KOH / g to 50 mg KOH / g, more preferably 15 mg KOH / g to 45 mg KOH / g, even more preferably 20 mg KOH / g to 40 mg KOH / g, most preferably 25 mg KOH / g to 35 mg KOH / g, determined according to DIN EN ISO 2114.
[0156] Preferably, the polyester-polyurethane has a particle size of 50 nm to 200 nm, more preferably 70 nm to 180 nm, even more preferably 80 nm to 150 nm, most preferably 90 nm to 130 nm, as determined by measuring the hydrodynamic volume / hydrodynamic radius of the dispersion particles using photon correlation spectroscopy (PCS).
[0157] Preferably, the polyester-polyurethane has a number average molecular weight (M) of 1,000 g / mol to 3,500 g / mol, more preferably 1,200 g / mol to 3,200 g / mol, even more preferably 1,500 g / mol to 3,000 g / mol, most preferably 1,800 g / mol to 2,800 g / mol. n ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0158] Preferably, the polyester-polyurethane has a weight average molecular weight (M) of 6,000 g / mol to 50,000 g / mol, more preferably 7,000 g / mol to 48,000 g / mol, even more preferably 8,000 g / mol to 46,000 g / mol, most preferably 9,000 g / mol to 43,000 g / mol. w ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0159] Step (b): Preparation of poly(meth)acrylate
[0160] In the presence of the polyester-polyurethane of step (a), ethylenically unsaturated monomers including at least a (meth)acrylic monomer are polymerized by free radical polymerization to obtain poly(meth)acrylate.
[0161] The ethylenically unsaturated monomers may be added to the neutralized and / or diluted polyester-polyurethane dispersion or to the undiluted polyester-polyurethane. The ethylenically unsaturated monomers in step (b) are added to the polyester-polyurethane of step (a) before or simultaneously with the addition of the free radical initiator. If the ethylenically unsaturated monomers are added to the polyester-polyurethane of step (a) before the addition of the free radical initiator, the ethylenically unsaturated monomers and the polyester-polyurethane of step (a) are preferably incubated at a temperature of preferably 20° C. to 30° C. for at least 10 min, more preferably at least 30 min, even more preferably at least 60 min, most preferably at least 2 hours such as for example at least 4 hours.
[0162] The solvent may be added to the polyester-polyurethane before or after the addition of the (meth) acrylic monomer or the free radical initiator to obtain a polyester-polyurethane dispersion comprising the (meth) acrylic monomer. The solvent may be water or an organic solvent. Preferably, water is added to adjust the solid content and produce an aqueous polyester-polyurethane dispersion.
[0163] Suitable ethylenically unsaturated monomers are indicated above. Preferably, monoethylenically unsaturated alkyl (meth)acrylate monomers are polymerized in step (b), more preferably tert-butyl acrylate, n-butyl acrylate, n-butyl methacrylate and ethylhexyl methacrylate.
[0164] To initiate the free radical polymerization, water-soluble or water-insoluble initiators can be used. Examples of water-soluble initiators are hydrogen peroxide, peroxodisulfate salts such as sodium peroxodisulfate, potassium peroxodisulfate and ammonium peroxodisulfate, ammonium salts of 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methyl-N-1,1-bis(hydroxymethyl)ethyl)propionamide, 2,2'-azobis(2-methyl-N-(2-hydroxyethyl)propionamide). Preferably, ammonium peroxodisulfate (APS) is used as a water-soluble initiator.
[0165] Examples of water-insoluble initiators are tert-butyl-peroxy-2-ethylhexanol, tert-butyl peroxypivalate and dibenzoyl peroxide. Preferably, tert-butyl-peroxy-2-ethylhexanol is used as the water-insoluble initiator.
[0166] Preferably, the free radical polymerization is initiated by a water-insoluble initiator, more preferably by tert-butyl-peroxy-2-ethylhexanol.
[0167] The free radical initiator generates free radicals within the ethylenically unsaturated polyester-polyurethane polymer and / or within the ethylenically unsaturated monomer.
[0168] Thus, a poly(meth)acrylate is obtained, which can be physically mixed with the polyester-polyurethane of step (a) or covalently bonded to the polyester-polyurethane of step (a). For example, the poly(meth)acrylate can be covalently bonded to the polyester-polyurethane of step (a) by forming a graft polymer formed by free radical copolymerization of an ethylenically unsaturated monomer and an ethylenically unsaturated group in the main chain of the polyester-polyurethane of step (a), and / or H-deoxyribonucleic acid on the main chain of the polyester-polyurethane of step (a).
[0169] Preferably, the solids content of the obtained polyester-polyurethane-poly(meth)acrylic hybrid dispersion is ≥40 wt.-%, more preferably ≥42 wt.-%, even more preferably ≥43 wt.-%, even more preferably ≥44 wt.-%, even more preferably ≥48 wt.-%, most preferably ≥50 wt.-%, determined in accordance with DIN EN ISO 3251 at 130° C. for 60 min using 1.0 g weighed portions.
[0170] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has a glass transition temperature of -50°C to +50°C, more preferably -48°C to 40°C, even more preferably -45°C to 35°C, most preferably -45°C to 30°C, measured according to DIN-EN-ISO 11357-1 and -2.
[0171] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a number average molecular weight (M) of 2,500 g / mol to 5,000 g / mol, more preferably 2,700 g / mol to 4,800 g / mol, most preferably 3,000 g / mol to 4,500 g / mol. n ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0172] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a weight average molecular weight (MW) of 25,000 to 550,000 g / mol, more preferably 30,000 to 500,000 g / mol, even more preferably 50,000 to 450,000 g / mol, most preferably 100,000 to 400,000 g / mol. w ), which was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0173] The number average molecular weight (M) of the polyester-polyurethane-poly(meth)acrylic hybrid prepared using at least one multiethylenically unsaturated monomer, preferably at least one diethylenically unsaturated monomer, is n ) and weight average molecular weight (M w ) can be even higher than the number average molecular weight (M) as described in the two paragraphs above. n ) and weight average molecular weight (M w ).
[0174] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid has an acid number of 5 mg KOH / g to 50 mg KOH / g, more preferably 10 mg KOH / g to 45 mg KOH / g, even more preferably 15 mg KOH / g to 40 mg KOH / g, even more preferably 15 mg KOH / g to 35 mg KOH / g, most preferably 15 mg KOH / g to 30 mg KOH / g, which is determined according to DIN EN ISO 2114.
[0175] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion has a viscosity of 5 mPa*s to 3,000 mPa*s, more preferably 10 mPa*s to 2,500 mPa*s, even more preferably 10 mPa*s to 1000 mPa*s, even more preferably 10 mPa*s to 500 mPa*s, even more preferably 10 mPa*s to 200 mPa*s, as measured by using a Rheolab QC rotational rheometer with a cylinder cc 27 at a temperature of 23°C for 1000 s. -1 The shear rate is determined according to DIN 53019-1.
[0176] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion has a particle size of 50 nm to 400 nm, more preferably 70 nm to 300 nm, even more preferably 100 nm to 250 nm, most preferably 120 nm to 220 nm, as determined by measuring the hydrodynamic volume / hydrodynamic radius of the dispersion particles using photon correlation spectroscopy (PCS).
[0177] Preferably, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion comprises 45 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 55 wt.-% of the poly(meth)acrylate of step (b), more preferably 50 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 50 wt.-% of the poly(meth)acrylate of step (b), even more preferably 55 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 45 wt.-% of the poly(meth)acrylate of step (b), even more preferably 60 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 40 wt.-% of the poly(meth)acrylate of step (b), most preferably 65 to 90 wt.-% of the polyester-polyurethane of step (a) and 10 to 35 wt.-% of the poly(meth)acrylate of step (b), based on the solids content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion.
[0178] Use of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention
[0179] The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention is suitable for a variety of applications. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention can be used in many coating fields, in particular in automotive coatings.
[0180] In particular, the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used in a basecoat composition or a filler coating composition, more preferably in a basecoat composition or a filler coating composition in an automotive coating. A coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used to form a basecoat layer on an untreated or pretreated substrate. In addition, a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used to form a second basecoat layer on top of the first basecoat layer.
[0181] Coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention
[0182] Another object of the present invention is a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention.
[0183] The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention can be used as a binder in any coating composition, in particular in basecoat compositions.
[0184] The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention can be used in any liquid coating composition (which may be aqueous or solvent-based), preferably in an aqueous coating composition.
[0185] The coating compositions comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersions according to the invention can be used to form one or more layers in a multilayer coating, preferably on untreated or pretreated substrates, in particular on automobile bodies or parts thereof.
[0186] The coating composition is preferably heat-curable. In addition to the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention, the heat-curable coating composition also comprises further ingredients, such as one or more further binders (A1) and / or one or more customary coating additives (A2) and / or one or more pigments and / or fillers (A3) and / or one or more solvents (A4) as additional components (A).
[0187] Additional adhesive (A1)
[0188] In addition to the polyester-polyurethane-poly(meth)acrylic hybrid dispersions according to the invention, further polymers selected from the group consisting of polyurethanes, polyureas, polyesters, polyamides, poly(meth)acrylates and / or copolymers of structural units of said polymers can be used as binders. The term "poly(meth)acrylate" refers not only to polyacrylates but also to polymethacrylates, and also to polymers comprising both methacrylates and / or methacrylic acid and / or acrylates and / or acrylic acid.
[0189] Preferred polyurethanes are described, for example, in German patent application DE 199 48 004 A1, page 4, line 19 to page 11, line 29 (polyurethane prepolymer B1), in European patent application EP 0 228 003 A1, page 3, line 24 to page 5, line 40, in European patent application EP 0 634 431 A1, page 3, line 38 to page 8, line 9, and in international patent application WO 92 / 15405, page 2, line 35 to page 10, line 32.
[0190] Preferred polyesters are described, for example, in DE 4009858 A1, column 6, line 53 to column 7, line 61 and column 10, line 24 to column 13, line 3, and Example D; or in WO 2014 / 033135 A2, page 2, line 24 to page 7, line 10 and page 28, line 13 to page 29, line 13. Likewise, the polyesters may have a dendritic structure, as described, for example, in WO 2008 / 148555 A1.
[0191] Preferred polyurethane-poly(meth)acrylate copolymers (eg (meth)acrylated polyurethanes) and their preparation are described, for example, in WO 91 / 15528 A1, page 3, line 21 to page 20, line 33 and in DE 4437535 A1, page 2, line 27 to page 6, line 22.
[0192] Preferred poly(meth)acrylates are those which can be prepared by multistage free radical emulsion polymerization of ethylenically unsaturated monomers in water and / or organic solvents. For example, seed-core-shell polymers (SCS polymers) are particularly preferred. Such polymers or aqueous dispersions containing such polymers are known, for example, from WO 2016 / 116299 A1.
[0193] Preferred polyurethane-polyurea copolymers are polyurethane-polyurea particles, preferably those with an average particle size of 40 to 2000 nm, each of which contains, in reacted form, at least one polyurethane prepolymer containing isocyanate groups (containing anionic groups and / or groups that can be converted into anionic groups) and at least one polyamine containing two primary amine groups and one or two secondary amine groups. Preferably, such copolymers are used in the form of aqueous dispersions. Such polymers can in principle be prepared, for example, by conventional polyaddition of polyisocyanates with polyols and polyamines.
[0194] At least one additional adhesive is included in the coating composition comprising the polyester-polyurethane-poly (meth) acrylic hybrid dispersion according to the present invention to crosslink the polyester-polyurethane-poly (meth) acrylic hybrid dispersion of the present invention. Suitable crosslinking adhesives are amino resins, such as urea-formaldehyde resins or melamine-formaldehyde resins or isocyanate-terminated polyurethanes or isocyanates (which can be free or blocked isocyanates) with free or blocked isocyanate groups. Blocked isocyanates refer to the reaction products of isocyanates, wherein the isocyanate functional groups have reacted with "blocking agents". Blocking of isocyanates occurs by the reaction of isocyanates with compounds containing active hydrogen. Suitable blocking agents are derivatives from oximes, lactams, phenols, active methylene, pyrazoles, mercaptans, imidazoles, amines, imines, triazoles, hydroxylamines and aliphatic or alicyclic alkyl monoalcohols. The blocked isocyanate component will not react at room temperature. The crosslinking reaction of the blocked isocyanate with the hydroxyl functional compound will be achieved using elevated temperatures.
[0195] Additives are binders that are typically used in minimal amounts and provide specific properties to the coating composition.
[0196] Coating Additives(A2)
[0197] The coating composition may contain at least one additive selected from the group consisting of reactive diluents, light stabilizers, antioxidants, defoamers, emulsifiers, surfactants, slip additives, polymerization inhibitors, initiators for free radical polymerization, catalysts, adhesion promoters, film-forming aids, wetting agents, dispersants, leveling agents, rheology control agents, sag control agents (SCA), flame retardants, corrosion inhibitors, desiccants, biocides, matting agents and dyes (which are colorants), which are soluble in the coating composition. Further examples of suitable coating additives are described, for example, in the textbook "Lackaditive" ("Additives for Coatings" by Johan Bieleman, Wiley VCH, Weinheim, 1998). The additives can be used in known and conventional amounts.
[0198] Preferred coating additives are rheology control agents, wetting agents or leveling agents.
[0199] Pigments and fillers (A3)
[0200] The coating composition according to the invention may contain a pigment, in particular if the coating composition is a basecoat composition or a filler composition. The terms "coloring pigment" and "color pigment" are interchangeable and include colored, black and white pigments. As coloring pigments, inorganic and organic pigments can be used.
[0201] Examples of white pigments are titanium dioxide, zinc white, zinc sulfide and lithopone.
[0202] Examples of black pigments are carbon black, iron manganese black and spinel black. Examples of pigments with other colors are chromium oxide, hydrated chromium oxide green, cobalt green, ultramarine green, cobalt blue, ultramarine blue, manganese blue, ultramarine violet, cobalt violet and manganese violet, iron oxide red, cadmium sulfoselenide, molybdenum chrome red and ultramarine red, iron oxide brown, mixed brown, spinel and corundum phases as well as chrome orange, iron oxide yellow, nickel titanium yellow, chrome titanium yellow, cadmium sulfide, cadmium zinc sulfide, chrome yellow and bismuth vanadate.
[0203] Possible organic pigments are azo pigments, polycyclic pigments and anthraquinone pigments.
[0204] The term "filler" is known to the person skilled in the art, for example from DIN 55943 (date: October 2001). Examples of suitable fillers are kaolin, dolomite, calcite, chalk, calcium sulfate, barium sulfate, talc, silicon dioxide (especially pyrogenic silicon dioxide), hydroxides such as aluminum hydroxide or magnesium hydroxide; in addition, reference is made to Lexikon Lackeund Druckfarben, Georg Thieme Verlag, 1998, pp. 250 ff., “Fillers”.
[0205] Solvent (A4)
[0206] In particular, the coating composition can also include a solvent. The solvent can be water or an organic solvent. Preferably, water is used as a solvent. Suitable examples of organic solvents include heterocycles, aliphatic or aromatic hydrocarbons, mono- or polyfunctional alcohols, ethers, esters, ketones and amides, such as N-Methylpyrrolidone, N-Ethylpyrrolidone, dimethylformamide, toluene, xylene, butanols, ethylene glycol and butanediol and their acetates, butyl diglycol, diethylene glycol dimethyl ether, cyclohexanone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), acetone, isophorone, or a mixture thereof. The organic solvent can be used in combination and can also be used in combination with water in the aqueous coating composition.
[0207] The content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention is preferably 2 to 30 wt.-%, more preferably 5 to 25 wt.-%, most preferably 7 to 20 wt.-%, relative to the total coating composition.
[0208] Coatings formed from coating compositions comprising polyester-polyurethane-poly(meth)acrylic hybrid dispersions according to the invention and substrates coated therewith
[0209] The coating composition for forming the coating is applied to the substrate by conventional painting methods familiar to those of ordinary skill in the art. The substrate material is selected from the group consisting of metal, polymer, wood, glass, mineral-based materials and the composite material of any of the above materials. Untreated or pretreated substrates can be used, wherein the pretreatment often depends on the chemical nature of the substrate.
[0210] The coating composition comprising the polyester-polyurethane-poly(meth)acrylate hybrid dispersion according to the invention is preferably applied by spraying pneumatically and / or electrostatically. Depending on the reactivity and duration of the crosslinking agent, the coating composition is heat curable at elevated temperatures, preferably between 60° C. and 180° C., most preferably between 80° C. and 160° C.
[0211] The present invention further provides a substrate coated with a coating formed from a coating composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention.
[0212] Multi-layer coatings and multi-layer coated substrates
[0213] Another object of the present invention is a method for producing a multilayer coating, the method comprising the following steps:
[0214] a) applying one or more basecoat compositions to a substrate to form one or more basecoat layers, wherein at least one basecoat composition comprises the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention,
[0215] b) applying a clearcoat composition on top of the one or more basecoat layers to form a clearcoat layer,
[0216] c) simultaneously curing the one or more basecoat layers and the clearcoat layer or individually curing one or more layers obtained in steps (a) and (b) and then applying a subsequent coating or individually curing all layers obtained in steps (a) and (b).
[0217] The multi-layer coated substrate can be a pretreated or untreated substrate, which can be uncoated or precoated. The individual coatings are applied by conventional painting methods familiar to those skilled in the art. The coating composition is preferably applied by spraying in a pneumatic and / or electrostatic manner, wherein at least one coating composition comprises a polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the present invention, which composition can be a basecoat composition or a filler coating composition.
[0218] The application of the basecoat composition to the substrate to form a basecoat layer and the application of the clearcoat composition on top of the basecoat layer is preferably carried out by wet-on-wet application, i.e., an application in which the previous layer is not cured or not fully cured before the next coating composition is applied. Thus, before applying the clearcoat composition, the basecoat composition can be flashed off at room temperature (25° C.) and / or alternatively, it can be dried at an elevated temperature.
[0219] Depending on the reactivity and duration of the crosslinking agent, the coating composition is heat curable at elevated temperatures, preferably between 60° C. and 180° C., most preferably between 80° C. and 160° C. The coating composition is preferably cured for 15 min to 50 min, most preferably 20 min to 40 min.
[0220] In addition, the present invention provides a substrate coated with the multilayer coating of the present invention. The substrate is selected from the group consisting of metal, polymer, wood, glass, mineral-based materials and composites of any of the above materials. Untreated or pretreated substrates can be used, wherein the pretreatment often depends on the chemical nature of the substrate. The pretreatment of the metal substrate is, for example, a zinc phosphate treatment step.
[0221] The multi-layer coatings of the invention comprising the coating compositions according to the invention exhibit an excellent appearance at low long wave values. This is achieved using polyester-polyurethane-poly(meth)acrylic hybrid dispersions with a high solids content, which is surprising since dispersions with such a high solids content usually lead to coagulation.
[0222] Furthermore, good compatibility of the basecoat compositions is achieved if at least one of the basecoat compositions comprises the polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to the invention.
[0223] Examples
[0224] method
[0225] Solid content
[0226] Unless stated otherwise, the solids content was determined in accordance with DIN EN ISO 3251 at 130° C. for 60 min using 1.0 g weighed portions.
[0227] Isocyanate content
[0228] The isocyanate content (NCO content) is determined by adding an excess of a 2% N,N-dibutylamine solution in xylene to a homogeneous solution of the sample in acetone / N-ethylpyrrolidone (1:1 vol.%) by potentiometric back titration of the amine excess with 0.1 N hydrochloric acid in accordance with DIN EN ISO 3251, DIN EN ISO 11909 and DIN EN ISO 14886. The polymer content (solids content) in the solution is used to refer to the NCO content of the polymer relative to the solids content.
[0229] Hydroxyl value
[0230] The hydroxyl number is determined according to R.-P. Krüger, R. Gnauck and R. Algeier (Plaste und Kautschuk [Plastics and Rubber], 20, 274 (1982)) using acetic anhydride in the presence of 4-dimethylaminopyridine as catalyst in tetrahydrofuran (THF) / dimethylformamide (DMF) solution at room temperature. The excess acetic anhydride remaining after acetylation is completely hydrolyzed and the acetic acid is potentiometrically back-titrated with alcoholic potassium hydroxide solution.
[0231] Acid value
[0232] The acid number is determined in accordance with DIN EN ISO 2114 in a homogeneous solution of tetrahydrofuran (THF) / water (9 parts by volume of THF and 1 part by volume of distilled water) using ethanolic potassium hydroxide solution.
[0233] Number average molecular weight and weight average molecular weight
[0234] Number average molecular weight (M n ) and weight average molecular weight (M w) was determined by gel permeation chromatography using poly(meth)acrylate standards and a tetrahydrofuran / acetic acid mixture (1 mol acetic acid / 1 liter tetrahydrofuran).
[0235] Average particle size
[0236] In the present application, the average particle size (z-average) of the particles of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion is determined by measuring the hydrodynamic volume / hydrodynamic radius of the dispersion particles using photon correlation spectroscopy (PCS).
[0237] The measurements were performed using a "Malvern Nano S90" (Malvern Instruments) at 25°C ± 1°C. The device covers a size range of 3nm to 3000nm and is equipped with a 4mW He-Ne laser at 633nm. Polyester-polyurethane-poly(meth)acrylic hybrid dispersions were diluted with particle-free deionized water as a dispersion medium to measure the polymer hybrid dispersions in a 1ml polystyrene cuvette with a suitable scattering intensity. The measurements were performed five times and repeated using a second freshly prepared sample. The average particle size (z-mean) is the arithmetic mean of the average particle size (intensity weighted) of the individual preparations. Polystyrene standards with qualified particle sizes between 50 and 3000nm were used for verification.
[0238] Viscosity
[0239] The viscosity of the polyester-polyurethane during the synthesis was measured using a CAP 2000H viscometer with spindle 03 at a temperature of 140°C for 1250 s. -1 Up to 2500s -1 The shear rate is determined according to DIN EN ISO 2884-1.
[0240] The viscosity of the final polyester-polyurethane dispersion and the final polyester-polyurethane-poly(meth)acrylic hybrid dispersion was measured using a Rheolab QC rotational rheometer with a cylinder cc 27 at a temperature of 23°C for 1000 s. -1 The shear rate is determined according to DIN 53019-1.
[0241] Glass transition temperature
[0242] The glass transition temperature is measured according to DIN-EN-ISO 11357-1 and -2. The liquid dispersion is applied to a glass substrate by knife coating (50 μm) and dried at 130 ° C for 60 minutes. Nitrogen is used to obtain a defined atmosphere. The dried sample is placed in a crucible. If a starting temperature of -90 ° C is reached, the temperature is increased to the selected limit at 10K / min and cooled to the selected limit (-90 ° C to 100 ° C) at the same rate. Afterwards, a second run with the same temperature limit is performed, and the glass transition temperature is determined during the heating step in the second run.
[0243] Appearance evaluation
[0244] The appearance of the coated substrates was evaluated using a wave scanning measuring device from Byk / Gardner.
[0245] A laser beam is directed at an angle of 60° onto the surface of the substrate coated with the multilayer coating, and the reflected light in the short wave range (0.3 to 1.2 mm) and the long wave range (1.2 to 12 mm) is determined. The lower the values of short wave (LW) and long wave (LW), the better the appearance. In addition, the clarity of the image reflected in the surface of the multilayer structure is determined using a wave scanning measurement device. This parameter is called "distinctness of image" (DOI) and the higher the value, the better the appearance.
[0246] Unless otherwise indicated, all amounts given are in parts by weight or grams and percentages are by weight.
[0247] Comparative Synthesis of Polyester-Polyurethane-Poly(Meth)Acrylic Hybrid Dispersions C1 to C3
[0248] According to Example 3 of US 10,233,353 B2 (COOH-rich polyurethane: 23.3 g dimethylolpropionic acid, 53.4 g H 12 Carboxyl-rich polyurethanes and polyesters were prepared by using Example 4 (polyester: 375 g 1,6-hexanediol, 118 g trimethylolpropane, 389 g isophthalic acid, 118 g adipic acid; acid value 10 mg KOH / g). Polyester-polyurethane dispersions were synthesized analogously to Example 5 of US 10,233,353 B2 as the basis for comparative polyester-polyurethane-poly(meth)acrylic hybrid dispersions C1 and C3. Comparative dispersion C1 is a replica of Example 6 of the above patent. The amounts in Table 1 are given in grams.
[0249] Table 1
[0250]
[0251] As shown in Table 1, polymerization at 42 wt.-% solids content resulted in coagulation and no polyester-polyurethane-poly(meth)acrylic hybrid dispersion was obtained.
[0252] Synthesis of polyester-polyurethane-poly(meth)acrylic hybrid dispersions of the present invention
[0253] Synthesis of polyester PE1 and PE2
[0254] The compounds of Table 2 were mixed in a reactor equipped with a stirrer and a dean stark device. The temperature was raised to 220° C. and carefully controlled to reduce monomer losses. The reaction was monitored by titration. Polyester PE2 having the properties shown was obtained. The condensation process of PE1 was carried out until an acid value of less than 10 mg KOH / g was reached. After cooling, the polyester PE1 was adjusted with methyl ethyl ketone (MEK) to obtain a solid content of 74 wt.-%.
[0255] Table 2
[0256]
[0257] Synthesis of polyurethanes PU1 to PU7
[0258] In a N 2 In a purged reactor, the compounds of Table 3 were reacted to obtain polyurethanes PU1 to PU7 having the properties shown.
[0259] Dimethylolpropionic acid (DMPA), isophorone diisocyanate (IPDI) and methyl ethyl ketone (MEK) were mixed for the synthesis of PU1 and the temperature was carefully raised to 77°C. The reaction was monitored by titration. After reaching a theoretical NCO content of 14.9%, cooling was applied and ethylene glycol was added. The temperature was maintained at 77°C until complete conversion of the NCO groups was detected by titration. Subsequently, trimellitic anhydride was added and the reaction was stopped at a constant acid value.
[0260] Dimethylolpropionic acid, methyl ethyl ketone, ethylene glycol and 4,4'-methylenebis(cyclohexyl isocyanate) were mixed for the synthesis of PU2 and the temperature was maintained at 77°C after the exothermic reaction. The reaction was monitored by titration. After reaching complete conversion of the NCO groups, the solid content was adjusted to 60 wt.-% by adding MEK. Subsequently, trimellitic anhydride was added and the reaction was stopped at a constant acid value.
[0261] PU1 and PU2 were diluted with MEK to obtain a solid content of about 70 wt.-%. PU3 and PU4 and PU7 were synthesized analogously to PU1. Based on the manufacture of PU2, PU5 and PU6 were obtained and diluted to a solid content of 55% or 57%, respectively.
[0262] Table 3
[0263]
[0264] Synthesis of Polyester-Polyurethane Dispersions PEUD1, PEUD2, PEUD4 and Polyester-Polyurethane PEU3
[0265] Synthesis of Polyester-Polyurethane Dispersion PEUD1
[0266] To prepare polyester-polyurethane dispersion 1, 7814.0 g of PE1 and 2218.0 g of PU2 were mixed in a reactor equipped with a stirrer. While applying reduced pressure (20 mbar), the temperature was carefully raised to a maximum of 160° C. The process was monitored by titration and viscosity measurement at 140° C. After reaching an acid number of 29 mg KOH / g and a viscosity of approximately 1800 mPa*s (CAP 2000H, spindle 03, 140° C., shear rate 1250 s -1 ) Afterwards, the temperature was lowered to 115° C. and 160 g of dimethylethanolamine were added within 10 minutes. Water was added at 90° C. to adjust the solids content of PEUD1 to 55 wt.-%. The further properties are shown in Table 4.
[0267] Synthesis of Polyester-Polyurethane Dispersion PEUD2
[0268] To prepare polyester-polyurethane dispersion 2, 1084.0 g of PE2 and 415.8 g of PU2 were mixed in a reactor equipped with a stirrer. While applying reduced pressure (40 to 60 mbar), the temperature was carefully raised to a maximum of 140° C. The process was monitored by titration and viscosity measurement at 140° C. After reaching an acid number of 32 mg KOH / g and a viscosity of approximately 1400 mPa*s (CAP 2000H, spindle 03, 140° C., shear rate 2500 s -1 ) Afterwards, the temperature was lowered to 80° C. and 46.0 g of dimethylethanolamine were added within 10 minutes. Water was added at 80° C. to adjust the solids content of PEUD2 to 45 wt.-%.
[0269] The properties of PEUD1 and PEUD2 are shown in Table 4.
[0270] Table 4
[0271]
[0272] 1 The viscosity was measured using a Rheolab QC rotational rheometer with a cylinder cc 27 at a temperature of 23 °C for 1000 s. -1 The shear rate is measured.
[0273] Synthesis of Polyester-Polyurethane PEU3
[0274] To prepare polyester-polyurethane 3, 2441.8 g of PE1 and 693.1 g of PU2 were mixed in a reactor equipped with a stirrer. While applying reduced pressure (50 to 120 mbar), the temperature was carefully raised to a maximum of 140° C. The process was monitored by titration and viscosity measurement at 140° C. After reaching an acid number of 26 mg KOH / g and a viscosity of approximately 2000 mPa*s (CAP 2000H, spindle 03, 140° C., shear rate 1250 s -1 ) Afterwards, the temperature was lowered to 82° C. and 203.0 g of n-butyl acrylate were added. A polyester-polyurethane 3 having a solids content of about 90 wt.-% was obtained.
[0275] Synthesis of Polyester-Polyurethane Dispersion PEUD4
[0276] To prepare polyester-polyurethane dispersion 4, 2168.3 g of PE1 and 831.7 g of PU2 were mixed in a reactor equipped with a stirrer. While applying reduced pressure (50 to 120 mbar), the temperature was carefully raised to a maximum of 140° C. The process was monitored by titration and viscosity measurement at 140° C. After reaching an acid number of 28 mg KOH / g and a viscosity of approximately 1800 mPa*s (CAP 2000H, spindle 03, 140° C., shear rate 1250 s -1 ) Afterwards, the temperature was lowered to 100° C. and 187.3 g of butyl diglycol were added. 60.0 g of dimethylethanolamine were added over a period of 10 minutes. Afterwards, 1925.0 g of water were slowly added at 95° C. A polyester-polyurethane dispersion 4 having a solids content of 48.2 wt.-% was obtained.
[0277] Synthesis of the polyester-polyurethane-poly(meth)acrylic hybrid dispersions B1 to B17 of the present invention by emulsion polymerization
[0278] Examples B1 to B11
[0279] B1 to B11 were synthesized in a 3.5 L steel reactor using an anchor stirrer. The stirrer was set to a low setting (50 to 100 rpm). Examples B9 and B10 used a glass reactor equipped with a stirrer at 150 rpm. The reactor was temperature regulated using heat transfer oil. Undiluted PEUD1 was used for the synthesis of B1 to B3, B5, B7 and B10, and undiluted PEUD2 was used for the synthesis of B9. For the synthesis of B4 and B6, PEUD1 was diluted with 569 g of deionized water. For the synthesis of B8, PEUD1 was neutralized with 17.2 g of dimethylethanolamine (DMEA) and diluted with 26.9 g of butyl diglycol and 792.2 g of deionized water to obtain a dispersion with 40 wt.-% solids and a neutralization level of approximately 70%. Undiluted or diluted PEUD1 or PEUD2 was heated to 80°C. The amounts in Table 5 are given in grams.
[0280] For Examples B1 to B7, one or more (meth)acrylic monomers were mixed with 2 g of tert-butyl-peroxy-2-ethylhexanol. The respective mixture was added slowly over the course of 3 hours at 80° C. 0.4 g of tert-butyl-peroxy-2-ethylhexanol was then added and stirred at 80° C. for a further 2 hours.
[0281] For Example B8, (meth)acrylic monomer and 2.4 g tert-butyl-peroxy-2-ethylhexanol were slowly added during 2.5 hours at 80° C. Then 0.4 g tert-butyl-peroxy-2-ethylhexanol was added and it was stirred at 80° C. for another 2 hours.
[0282] For example B9, the (meth)acrylic monomers were mixed with 0.3 g of tert-butyl-peroxy-2-ethylhexanol. The corresponding mixture was added slowly over the course of 3 hours at 80° C. It was then stirred at 80° C. for a further 2 hours.
[0283] For example B10, the (meth)acrylic monomers were mixed with 0.2 g of tert-butyl-peroxy-2-ethylhexanol. The corresponding mixture was added slowly over the course of 3 hours at 80° C. It was then stirred at 80° C. for 1 hour. Subsequently, 0.1 g of tert-butyl-peroxy-2-ethylhexanol was added and it was stirred at 80° C. for a further hour.
[0284] To synthesize B11, PEUD1 was diluted with 79.9 g of butyl diglycol and 257.8 g of deionized water. Subsequently, (meth)acrylic monomers and 1.3 g of tert-butyl-peroxy-2-ethylhexanol were slowly added at 80° C. over the course of 3 hours. Afterwards, the dispersion was stirred at 80° C. for a further 2 hours.
[0285] After the reaction, during the cooling period, dispersions B1 to B3, B5 and B10 were diluted with 230 g (B1, B2), 105 g (B3, B5) or 21 g (B10) of deionized water. Dispersions B4, B6 to B9 and B11 were not diluted further.
[0286] Table 5
[0287]
[0288]
[0289] The properties of dispersions B1 to B11 are shown in Table 6.
[0290] Table 6
[0291]
[0292] Examples B12 to B14
[0293] For the synthesis of dispersions B12 to B14, the same equipment as for examples B1 to B6 and B8 was used. The stirring speed was set to 150 rpm. According to Table 7, 509.7 g of polyester-polyurethane 3 were diluted with 62.9 g of (meth)acrylate and then 13.5 g of dimethylethanolamine were added. Over a period of 15 minutes, 463.4 g of water were added at 80° C. to obtain a monomer-swollen polyester-polyurethane dispersion with a theoretical solids content of about 43.7 wt.-%. Thereafter, 0.6 g of tert-butyl-peroxy-2-ethylhexanol was added over the course of 2 hours and the temperature was maintained at 80° C. for 2 hours. A further 0.3 g of tert-butyl-peroxy-2-ethylhexanol was added and stirring was continued for 1 hour.
[0294] Example B15
[0295] For the synthesis of dispersion B15, the same equipment as for Examples B1 to B6 and B8 was used. The stirring speed was set to 150 rpm. At 110° C., 1456.0 g of polyester-polyurethane 3 were diluted with 316.0 g of tert-butyl acrylate, 197.5 g of styrene and 323.9 g of n-butyl acrylate. The temperature was lowered to 95° C. and 220.0 g of butyl diglycol were added before the addition of 63.2 g of dimethylethanolamine. After 10 minutes, 3100.0 g of water were added at 80° C. to obtain a monomer-swollen polyester-polyurethane dispersion with a theoretical solids content of about 23.1 wt.-%.
[0296] 2500.0 g of this monomer-swollen polyester-polyurethane dispersion were heated to 80° C. and 8.2 g of tert-butyl-peroxy-2-ethylhexanol were added over the course of 2.5 h, and the reaction temperature was maintained at 80° C. for a further 2 h. 2.0 g of tert-butyl-peroxy-2-ethylhexanol were added and stirring was continued for 1 h.
[0297] Examples B16 and B17
[0298] For the synthesis of dispersions B16 and B17, the same equipment as for Examples B1 to B6 and B8 was used. The stirring speed was set to 150 rpm. According to Table 7, 1065.1 g of PEUD 4 was diluted with 185.7 g of water and heated to 80° C. 127.3 g of n-butyl acrylate, 73.5 g of tert-butyl acrylate and 46.0 g of styrene were added over the course of 3 hours. In parallel with the monomer dosage, 2.4 g of tert-butyl-peroxy-2-ethylhexanol (B16) or a mixture of 52.5 g of water and 4.8 g of ammonium persulfate (B17) was added to the reactor. For the synthesis of dispersion B16, 1.0 g of tert-butyl-peroxy-2-ethylhexanol was used and the reaction temperature was kept at 80° C. for another 2 hours.
[0299] Table 7
[0300]
[0301]
[0302] The acid values of dispersions B12 to B17 are shown in Table 8.
[0303] Table 8
[0304]
[0305] As is evident from Tables 5 and 7, the polyester-polyurethane-poly(meth)acrylic hybrid dispersions of the invention exhibit solid contents much greater than 40 wt.-% and no coagulation is observed. This is surprising, since a solid content of 42 wt.-% in the comparative polyester-polyurethane-poly(meth)acrylic hybrid dispersion C3 already leads to coagulation, whereas the polyester-polyurethane-poly(meth)acrylic hybrid dispersions do not coagulate even at solid contents up to about 60 wt.-% (B3).
[0306] Preparation of basecoat compositions comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersions B1 to B6 and B11 of the invention
[0307] Preparation of mill base MB1
[0308] A mill base of 19.1 parts by weight of deionized water, 0.9 parts by weight of a 10% dimethylethanolamine solution, 8.3 parts by weight of a water-based polyester with a solids content of 60.0±1.0 wt.-% (measured at 130° C. for 1 h) and an acid number of 29 to 34 mg KOH / g solid, 15 parts by weight of titanium dioxide, 0.5 parts by weight of 2-ethylhexanol, 34.4 parts by weight of barium sulfate, 1.8 parts by weight of additives, 2.6 parts by weight of carbon black and 17.4 parts by weight of a polyurethane dispersion with a solids content of 33.0±1.0 wt.-% (measured at 130° C. for 1 h) and an acid number of 19 to 23 mg KOH / g solid was prepared.
[0309] Preparation of basecoat composition
[0310] The basecoat compositions were prepared by mixing the components of Table 9. The inventive basecoat compositions BC-I1 to BC-I7 comprised the inventive polyester-polyurethane-poly(meth)acrylic hybrid dispersions B1 to B6 and B11, while the comparative basecoat compositions BC-C1, BC-C2, and BC-C3 comprised comparative aliphatic polycarbonate polyether polyurethane dispersions DLU) (BC-C1), polyurethane dispersion PEUD-1 (which is an intermediate product without adding and polymerizing ethylenically unsaturated monomers) (BC-C2) or comparative polyester-polyurethane-poly(meth)acrylic hybrid dispersion C2 (see Table 1) (which is prepared similarly to Example 5 of US10,233,353B2) (BC-C3). Typical polyurethane, polyester and polyacrylate dispersions are used as main resins in all basecoat compositions. Since the basecoat composition is a one-component composition, melamine-formaldehyde crosslinking agent is used as a typical crosslinking agent for such compositions. The basecoat composition of the present invention or the comparative basecoat composition is adjusted with water to obtain a basecoat composition with a solid content of 27.5%.
[0311] Table 9
[0312]
[0313]
[0314] 1 Polyurethane dispersion: solid content: 32% to 34%; acid value: 19 to 23 mg KOH / g solid, hydroxyl value: 17 mg KOH / g solid. Polyurethane dispersions are known from WO 2016000947 A1.
[0315] 2Aqueous polyester solution: solids content: 60%±1.0% (measured at 130° C. for 1 h); acid number: 29 to 34 mgKOH / g solid. Aqueous polyester solutions are known from DE 4009858, Example D.
[0316] 3 Polyacrylate dispersion: solid content: 25.5% to 27.5%, acid value: 16.6 to 17.6 mg KOH / g solid, hydroxyl value 16.5 to 17.5 mg KOH / g solid. Polyacrylate dispersions are known from WO 2017148796 A1.
[0317] 4 Application viscosity: 85±25mPa*s (RheolabQC, cc27, used for 1000s -1 Shear rate)
[0318] Preparation of Basecoat Composition 2 (BC2)
[0319] 26.5 parts by weight of deionized water, 3.1 parts by weight of a 10% dimethylethanolamine solution, 4.5 parts by weight of a water-based polyester having a solid content of 60.0±1.0 wt.-% (measured at 130° C. for 1 h) and an acid value of 29 to 34 mg KOH / g solid, 6.8 parts by weight of a rheological agent, 2.0 parts by weight of 2-ethylhexanol, 9.2 parts by weight of butoxypropanol, 1.0 parts by weight of dipropylene glycol methyl ether, 4.1 parts by weight of an additive, 14.0 parts by weight of carbon black, 7.5 parts by weight of a melamine resin, 3.0 parts by weight of a polyol having a solid content of 35.5±1.0 wt.-% (measured at 130° C. for 1 h) and 32 to 35 mg KOH / g solid were prepared. KOH / g solids, a first polyurethane polyacrylate dispersion with an acid number of 30.0 ± 1.0 wt.-% KOH / g solids, a second polyurethane polyacrylate dispersion with a solids content of 36.0 ± 1.0 wt.-% (measured at 130 ° C. for 1 h), a third polyurethane polyacrylate dispersion with a solids content of 44.0 ± 1.0 wt.-% (measured at 130 ° C. for 1 h) and an acid number of 30 to 32 mg KOH / g solids, and a BC2 formulation of an OH-functional aqueous polyacrylate with a solids content of 46.5 ± 1.0 wt.-% (measured at 130 ° C. for 1 h).
[0320] Application of coating composition
[0321] The spray booth was maintained at 25° C. and 70% humidity. The basecoats BC-C1 to BC-C3 and BC-I1 to BC-I7 were applied by electrostatic spray application (ESTA) to panels with an electro-dip coating (BASF Coatings GmbH, Cathoguard) in a layer thickness of approximately 25 μm. After a flash-off time of 3.5 minutes at 80° C., the basecoat BC2 was applied in a layer thickness of approximately 12 μm (BC-C1, BC-C2 and BC-I1 to BC-I6) or in a layer thickness of approximately 24 μm (BC-C3 and BC-I7). After a flash-off time of 3.5 minutes at 80° C., a clearcoat (BASF Coatings GmbH, UniGloss) was applied in a layer thickness of approximately 40 μm. Thereafter, the paint was cured at 140° C. for 30 minutes.
[0322] Coating Testing
[0323] The resulting multilayer coatings were evaluated in accordance with DIN EN ISO 2813 for appearance in longwave (LW) and shortwave (SW) and for gloss in terms of DOI (distinctness of image) by means of an orange peel meter (BYK 4840 wave scan dual, BYK-Gardner GmbH).
[0324] Table 10
[0325]
[0326]
[0327] The multi-layer coating comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion as basecoat 1 exhibits an excellent appearance in terms of low long wave values, since these values are comparable to those of the prior art multi-layer coating comprising aliphatic polycarbonate polyether polyurethane dispersions. The DOI value of the multilayer coating is lower than that of the multilayer coating comprising PEUD-1 as basecoat 1. Comparison with the multilayer coating comprising PEUD-1 as basecoat 1 shows that the additional emulsion polymerization with acrylate monomers improves the appearance of the multilayer coating, because PEUD-1 is also present in dispersions B1 to B7 according to the invention. Surprisingly, the emulsion polymerization of polyester-polyurethane with ethylenically unsaturated monomers as described above leads to an improved appearance with respect to low long-wave values. In addition, the multilayer coating comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as basecoat 1 exhibits an excellent appearance with respect to the combination of low long-wave values with low short-wave values and high DOI values.
[0328] Furthermore, the compatibility of the basecoat composition comprising the polyester-polyurethane-poly(meth)acrylic hybrid dispersion of the present invention with the second basecoat composition is improved compared to the comparative basecoat composition.
Claims
1. A polyester-polyurethane-poly(meth)acrylic hybrid dispersion, which is obtainable by the following method: (a) Esterification of the following: at least one polyurethane containing carboxyl groups, the at least one polyurethane having an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups; and at least one polyester containing hydroxyl groups, the polyester having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g, to obtain polyester-polyurethane; followed by (b) polymerizing ethylenically unsaturated monomers comprising at least (meth)acrylic monomers by free radical polymerization in the presence of the polyester-polyurethane of step (a), wherein one or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b), thereby obtaining the polyester-polyurethane-poly(meth)acrylic hybrid dispersion.
2. The polyester-polyurethane-poly(meth)acrylic acid hybrid dispersion according to claim 1, characterized in that The at least one polyurethane in step (a) has at least two carboxyl groups at each of the two ends, and / or is characterized in that The at least one polyurethane and at least one polyester in step (a) are esterified in the presence of one or more solvents to obtain a polyester-polyurethane dispersion.
3. The polyester-polyurethane-poly(meth)acrylic acid hybrid dispersion according to claim 1 or 2, characterized in that: The polyester-polyurethane obtained in step (a) has an acid number in the range of 10 to 50 mg KOH / g solids.
4. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 3, characterized in that The polyester-polyurethane dispersion obtained in step (a) has a solids content of ≥ 40 wt.-%, and / or is characterized in that The polyester-polyurethane dispersion obtained in step (a) is aqueous.
5. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 4, characterized in that The ethylenically unsaturated monomer in step (b) is added to the polyester-polyurethane of step (a) prior to or simultaneously with the addition of a free radical initiator.
6. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 5, characterized in that The free radical polymerization of the ethylenically unsaturated monomers in step (b) is initiated by a water-soluble initiator or a water-insoluble initiator.
7. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 6, characterized in that The (meth)acrylic monomer in step (b) comprises an alkyl (meth)acrylate monomer.
8. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 7, characterized in that The polyester-polyurethane-poly(meth)acrylic hybrid has a glass transition temperature of -50°C to +50°C.
9. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 8, characterized in that The solids content of the polyester-polyurethane-poly(meth)acrylic hybrid dispersion is ≥ 40 wt.-%.
10. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 9, characterized in that The polyester-polyurethane-poly(meth)acrylic hybrid comprises 45 to 90 wt.-% polyester-polyurethane and 10 to 55 wt.-% poly(meth)acrylate, based on polyester-polyurethane-poly(meth)acrylic hybrid solids.
11. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 10, characterized in that The polyester-polyurethane of step (a) is physically mixed with the poly(meth)acrylate of step (b) and / or covalently bonded to the poly(meth)acrylate of step (b).
12. The polyester-polyurethane-poly(meth)acrylic hybrid dispersion according to any one of claims 1 to 11, characterized in that The polyester-polyurethane-poly(meth)acrylic hybrid prepared using one or more monoethylenically unsaturated monomers has a number average molecular weight (M) of 2,500 g / mol to 5,000 g / mol. n ) and / or a weight average molecular weight (M) of 25,000 g / mol to 550,000 g / mol w ).
13. A method for producing a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as defined in claim 1 by: (a) Esterification of the following: at least one polyurethane containing carboxyl groups, the at least one polyurethane having an acid value of greater than 200 mg KOH / g to 400 mg KOH / g and at least one or more terminal carboxyl groups; and at least one polyester containing hydroxyl groups, the polyester having a hydroxyl value of 50 mg KOH / g to 300 mg KOH / g, to obtain polyester-polyurethane; followed by (b) polymerizing ethylenically unsaturated monomers comprising at least (meth)acrylic monomers by free radical polymerization in the presence of the polyester-polyurethane of step (a), wherein one or more solvents are present and / or used during step (a) and / or (b) and / or added after step (b), thereby obtaining the polyester-polyurethane-poly(meth)acrylic hybrid dispersion.
14. A coating composition comprising a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as defined in any one of claims 1 to 12.
15. A coating formed from the coating composition according to claim 14.
16. A substrate coated with the coating according to claim 15.
17. Use of the coating composition according to claim 14 in automotive coatings.
18. A method of making a multi-layer coating, the method comprising the steps of: a. applying one or more basecoat compositions to a substrate to form one or more basecoat layers, wherein at least one basecoat composition comprises a polyester-polyurethane-poly(meth)acrylic hybrid dispersion as defined in any one of claims 1 to 12, b. applying a clearcoat composition on top of the one or more basecoat layers to form a clearcoat layer, c. simultaneously curing the one or more basecoat layers and the clearcoat layer or individually curing one or more layers obtained in steps a. and b. and then applying a subsequent coating or individually curing all layers obtained in steps a. and b.