Composite patch for rotator cuff repair and preparation method thereof
By using a freeze-drying process in rotator cuff repair to form a composite polymer braid of a porous natural polymer coating and poly-L-lactic acid degradation material, the problem of the shear force of the polymer braided patch on muscle tissue is solved and the rotator cuff is repaired. The highly efficient repair and biocompatibility improve the repair effect and speed.
Patent Information
- Application Number
- CN202411094021.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-14
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing rotator cuff repair technology, the shearing force of the polymer braided patch on the muscle tissue causes tissue damage and delayed repair, and the existing polymer coating has insufficient bonding force with the patch to effectively maintain the mechanical stability of the rotator cuff. Sexual and biological environment optimization.
A composite polymer braid is used to form a porous, sponge-like natural polymer coating through a freeze-drying process, and is combined with polyethylene terephthalate and poly-L-lactic acid materials to provide initial mechanical support and gradual degradation of growth. space to promote the integration of the patch and human tissue.
It achieves efficient rotator cuff repair, reduces tissue shear damage caused by polymer silk threads, enhances the binding force between the patch and tissue, promotes rotator cuff healing and functional recovery, and reduces the cytotoxicity of the product.
Smart Images

Figure CN118806992A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical devices, and in particular to a composite patch for rotator cuff repair and a preparation method thereof. Background Art
[0002] Rotator cuff injury is a common injury of the shoulder joint. Factors such as decreased rotator cuff quality, subacromial impingement and trauma can cause rotator cuff injury, which seriously affects the patient's quality of life. Literature reports that the prevalence rate is 13% in people aged 50-59, 20%-30% in people aged 60-80, and more than 50% in people over 80 years old. Among them, giant rotator cuff tears account for about 40% of all rotator cuff tears. If active treatment is not received after the injury, as the disease progresses and tissue degenerates, it will eventually develop into an irreparable tear.
[0003] At present, the commonly used rotator cuff injury repair techniques in clinical practice include single / double-row anchor bone suture technology and rotator cuff repair techniques through tendon transfer technology, such as pectoralis major transfer technology and latissimus dorsi transfer technology. However, some rotator cuffs cannot be repaired due to huge tears and tissue contracture. When patients have anterosuperior shoulder instability or huge rotator cuff injuries, the effect is not ideal in terms of pain or function.
[0004] With the development of arthroscopic technology, patch technology provides a new solution for rotator cuff re-tear after suture surgery. The polymer braided patch has a high initial fixation strength, which can reach the initial strength of the rotator cuff and can still maintain mechanical stability after repeated activities; it can maintain mechanical stability when loaded with cyclic loads; however, the shear force of polymer silk threads on muscle tissue can cause tissue damage and delay repair.
[0005] Currently, drugs or porous, sponge-like natural polymer coatings are added around the patch to promote body growth. The natural polymer coating has a weak bonding force with the patch, and there is no strong bonding force generated directly on the patch by the natural polymer coating.
[0006] Ideal rotator cuff repair: high initial fixation strength to achieve the initial strength of the rotator cuff; minimize the gap between the rotator cuff and the humeral head; maintain mechanical stability after repeated activities; maintain mechanical stability when loaded with cyclic loads; optimize the biological environment of the "healing site"; and low tissue shear force. Current rotator cuff repair devices do not have such properties. Summary of the invention
[0007] In order to solve the problems in the above-mentioned background technology, the present invention provides a composite patch for rotator cuff repair, which solves the problem in the prior art that the shear force of the braided body on muscle tissue in the polymer patch may cause tissue damage and delay repair.
[0008] The solution adopted by the present invention to solve its technical problem is: a composite patch for rotator cuff repair, including a composite polymer braid, which is in sheet form, and the composite polymer braid includes one or more braiding units made by a braiding process, and one surface or both surfaces of the composite polymer braid are provided with a degradable natural polymer coating, and the natural polymer coating is formed by attaching natural polymers in a natural polymer solution to the composite polymer braid through a freeze-drying process, and the natural polymer solution is a solution formed by dissolving natural polymers in physiological saline, and the natural polymer coating is porous and sponge-like.
[0009] Furthermore, the multiple weaving units are stacked in the thickness direction, the multiple weaving units have the same shape, both ends of the multiple weaving units are connected, and two weaving units are connected through a natural polymer coating.
[0010] Furthermore, the natural polymer includes animal-derived collagen and / or recombinant collagen and / or gelatin and / or chitosan and / or silk fibroin.
[0011] Further, the weaving unit is prepared by weaving process from a partially degradable polymer substrate, the polymer substrate is a composite material, the non-degradable part of the material is polyethylene terephthalate; the degradable part is one or more of polylactic acid, poly-ε-caprolactone, polydioxanone, polylactic acid-glycolic acid copolymer, poly-L-lactic acid, racemic polylactic acid, preferably poly-L-lactic acid. Among them, the mass ratio of polyethylene terephthalate and poly-L-lactic acid is 10:90-90:10, preferably 60:40-80:20. The non-degradable part of the composite material provides basic mechanical support, improves stability, and has strong anti-fatigue ability; the degradable part gradually degrades, providing growth space for human tissue regeneration, and with the initial induction regeneration effect of the collagen sponge layer, it promotes better fusion of the patch with human tissue and provides better stability for the regenerated tissue.
[0012] In the prior art, there is a method of making a patch using a material of poly-L-lactic acid wrapped with polyethylene terephthalate. Compared with the weaving process, after the poly-L-lactic acid is degraded, the bonding between human tissue and polyethylene terephthalate is poor, and the stability of tissue regeneration is not ideal.
[0013] Furthermore, the polymer substrate is a combination of polyethylene terephthalate and poly-L-lactic acid, and the natural polymer is collagen.
[0014] Furthermore, the thickness of the composite polymer braid is 0.1-1.5 mm, and the ultimate tensile load of the composite polymer braid is 200-1000N.
[0015] Furthermore, the thickness of the composite polymer braid is 0.4-0.8 mm, and the ultimate tensile load of the composite polymer braid is 500-800N.
[0016] Furthermore, the weaving process of the weaving unit is warp knitting or weft knitting.
[0017] A method for preparing a composite patch comprises the following steps:
[0018] S1. Soaking, soaking the braid in a natural polymer solution, the natural polymer concentration is 0.01-1 mg / mL, the upper surface of the composite polymer braid is 0.01-1 mm from the upper interface of the natural polymer solution, the lower surface of the composite polymer braid is 0.01-2 mm from the lower interface of the natural polymer solution, the surrounding of the composite polymer braid is 0.01-1 mm from the interface of the collagen solution, the composite polymer braid is soaked for 0.1-60 min, and the braid soaking temperature is 0-40 ° C;
[0019] S2. Preliminary freezing, freeze-drying the soaking solution in the first step, first repeatedly evacuate the container containing the soaking solution several times, and start freezing, so that the container pressure is -20pa, the negative pressure is maintained for 15-60min, the freezing cooling rate is 1℃ / min, until the temperature drops to -20℃, and the freezing time is 2h;
[0020] S3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze drying for 24h-72h, freeze drying until completely dry, the natural polymers in the natural polymer solution adhere to the composite polymer braid to form a natural polymer coating.
[0021] Furthermore, the concentration of natural polymer is 0.3-0.6 mg / mL, the upper surface of the composite polymer braid is 0.2-0.4 mm away from the upper interface of the natural polymer solution, the lower surface of the composite polymer braid is 0.4-2 mm away from the lower interface of the natural polymer solution, the immersion time of the composite polymer braid is 0.1-20 min, and the immersion temperature of the composite polymer braid is 25-35°C.
[0022] Furthermore, a method for preparing a composite patch comprises the following steps:
[0023] S1. Soaking, soaking the composite polymer braid with a thickness of 0.8 mm in a collagen solution, the collagen concentration is 0.6 mg / mL, the upper surface of the composite polymer braid is 0.2 mm away from the upper interface of the collagen solution, the lower surface of the composite polymer braid is 2 mm away from the lower interface of the collagen solution, the four sides of the composite polymer braid are 0.5 mm away from the interface of the collagen solution, the composite polymer braid is immersed for 0.1 min, and the composite polymer braid is immersed at a temperature of 30 ° C;
[0024] S2. Preliminary freezing, freeze-drying the soaking solution in the first step, first repeatedly evacuate the container containing the soaking solution several times, and start freezing, so that the container pressure is -20pa, the negative pressure is maintained for 15min, the freezing cooling rate is 1℃ / min, until the temperature drops to -20℃, and the freezing time is 2h;
[0025] S3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze dry for 48 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the composite polymer braid to form a natural polymer coating.
[0026] In summary, the beneficial effects of the present invention are as follows: by adopting the freeze-drying process, the natural polymer remaining after the ice crystals sublime form a porous, sponge-like natural polymer coating, and the bonding area between the natural polymer coating and the patch is large and the bonding strength is strong; since the coating has a porous structure, it is easier for the human body's own tissue to grow into the patch, and the patch is easier to make the rotator cuff and the humeral head tightly combined to form an overall structure, thereby accelerating the healing of the rotator cuff; more importantly, the natural polymer coating can reduce the shear damage of the polymer thread shear force to the native tissue, thereby promoting better and faster tissue reconstruction.
[0027] Moreover, the composite polymer braid is based on the combination of polyethylene terephthalate and poly (L-lactic acid), and is combined with a natural polymer coating. Based on the characteristic that the degradation rate of poly (L-lactic acid) is lower than that of the natural polymer coating, it plays a "gradual induction" role in the growth of human tissue. It can be understood that the natural polymer coating degrades quickly, first inducing the tissue to bind to the surface of the composite polymer braid, and then the poly (L-lactic acid) degrades, inducing the tissue to bind to the polyethylene terephthalate in the braid. At the same time, after the degradation of poly (L-lactic acid), gaps will appear in the polymer braid, and the growth of human tissue will fill the gaps, so the tissue can be highly fused with the braid with only polyethylene terephthalate left. In the production process, cross-linking is eliminated, the cytotoxicity of the product is reduced, and the efficiency of tissue induction growth is higher.
[0028] Therefore, compared with existing patches, the composite patch disclosed in the present application has the advantages of good repair effect and fast speed.
[0029] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a structural diagram of the present invention.
[0031] In the figure: 1. Braided body; 2. Natural polymer coating; 3. Braided unit. DETAILED DESCRIPTION
[0032] In order to make the content of the present invention more clearly understood, the present invention is further described below based on specific embodiments in conjunction with the accompanying drawings.
[0033] It should be noted that the terms "center", "upper", "lower", "front", "back", "left", "right", "inner", "outer" and the like used herein to indicate directions or positional relationships are based on directions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. Unless otherwise specified, "plurality" means two or more.
[0034] Unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0035] Referring to the accompanying drawings, a composite patch for rotator cuff repair includes a braided body 1, which is in sheet form and includes one or more braided units 3 made by a braiding process. A degradable natural polymer coating 2 is provided on one or both surfaces of the braided body 1. The natural polymer coating 2 is formed by attaching natural polymers in a natural polymer solution to the braided body through a freeze-drying process. The natural polymer solution is a solution formed by dissolving natural polymers in physiological saline. The natural polymer coating 2 is porous and sponge-like.
[0036] Furthermore, the multiple weaving units 3 are stacked in the thickness direction, the multiple weaving units 3 have the same shape, both ends of the multiple weaving units 3 are connected, and a natural polymer coating 2 is provided between two weaving units 3 to connect them.
[0037] Further, the natural polymer includes animal collagen and / or recombinant collagen and / or gelatin and / or chitosan and / or silk protein, the weaving unit is prepared by weaving process of partially degradable polymer substrate, the polymer substrate is a composite material, the non-degradable part of the material is polyethylene terephthalate; the degradable part is one or more of polylactic acid, poly-ε-caprolactone, polydioxanone, polylactic acid-glycolic acid copolymer, poly-L-lactic acid, racemic polylactic acid, preferably poly-L-lactic acid. Among them, the mass ratio of polyethylene terephthalate and poly-L-lactic acid is 10:90-90:10, preferably 60:40-80:20. The non-degradable part of the composite material provides basic mechanical support, improves stability, and has strong anti-fatigue ability; the degradable part gradually degrades, providing growth space for human tissue regeneration, and with the initial induction regeneration effect of the collagen sponge layer, it promotes better fusion of the patch with human tissue and provides better stability for the regenerated tissue. The partially degradable braided unit is combined with a natural polymer coating, and the polymer coating is located on the outer layer of the braided unit, achieving the effect of "staged degradation", that is, in the body, the degradation rate of the natural polymer coating will be faster than the degradation rate of the degradable part of the braided unit, and the macroscopic performance is gradual degradation. Since the growth of biological tissues takes time, this gradual degradation characteristic conforms to the law of tissue growth and induces the tissue to combine with the composite polymer braid.
[0038] The braided unit produced by the warp and weft weaving process will make room for tissue growth after the poly-L-lactic acid filaments are degraded, and the biological tissue will be combined with the non-degradable part of the composite polymer braid in the form of weaving. Therefore, the weaving process in this application combined with partially degradable materials can also provide a good foundation for the later combination between tissue and patch, ensuring the final repair effect.
[0039] Furthermore, the polymer substrate includes a combination of polyethylene terephthalate and poly-L-lactic acid, and the natural polymer is collagen.
[0040] Furthermore, the composite polymer braided body 1 has a thickness of 0.1-1.5 mm, and an ultimate tensile load of 200-1000N.
[0041] Furthermore, the thickness of the composite polymer braided body 1 is 0.4-0.8 mm, and the ultimate tensile load of the composite polymer braided body 1 is 500-800N.
[0042] Furthermore, the weaving process is warp knitting or weft knitting.
[0043] A method for preparing a composite patch comprises the following steps:
[0044] 1. Soaking, soaking the composite polymer braid 1 in a natural polymer solution, the natural polymer concentration is 0.01-1 mg / mL, the upper surface of the composite polymer braid 1 is 0.01-1 mm away from the upper interface of the natural polymer solution, the lower surface of the composite polymer braid 1 is 0.01-2 mm away from the lower interface of the natural polymer solution, the surrounding of the composite polymer braid 1 is 0.01-1 mm away from the interface of the collagen solution, the braid 1 is soaked for 0.1-60 min, and the composite polymer braid 1 is soaked at a temperature of 0-40°C;
[0045] 2. Preliminary freezing: freeze-dry the soaking solution in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15-60min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0046] 3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze drying for 24h-72h, freeze drying until completely dry, the natural polymer in the natural polymer solution adheres to the composite polymer braid 1 to form a natural polymer coating 2.
[0047] Furthermore, the concentration of natural polymer is 0.3-0.6 mg / mL, the upper surface of the composite polymer braid 1 is 0.2-0.4 mm away from the upper interface of the natural polymer solution, the lower surface of the composite polymer braid 1 is 0.4-2 mm away from the lower interface of the natural polymer solution, the immersion time of the composite polymer braid 1 is 0.1-20 min, and the immersion temperature of the composite polymer braid 1 is 25-35°C.
[0048] Furthermore, in step 2, repeatedly vacuuming for multiple times means repeatedly vacuuming for at least three times.
[0049] Embodiment 1:
[0050] 1. Soaking: soak the braid 1 with a thickness of 0.4 mm in a collagen solution, the collagen concentration is 0.3 mg / mL, the upper surface of the composite polymer braid 1 is 0.2 mm away from the upper interface of the natural polymer solution, the lower surface of the composite polymer braid 1 is 0.4 mm away from the lower interface of the collagen solution, and the surrounding of the composite polymer braid 1 is 0.5 mm away from the interface of the collagen solution. The braid 1 is soaked for 20 min and the soaking temperature of the composite polymer braid 1 is 25°C;
[0051] 2. Preliminary freezing: freeze-dry the soaking solution in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0052] 3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a cooling rate of 2°C / min, freeze dry for 24 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the composite polymer braid 1 to form a natural polymer coating 2.
[0053] Embodiment 2:
[0054] 1. Soaking: soaking the composite polymer braid 1 with a thickness of 0.8 mm in a collagen solution, wherein the collagen concentration is 0.6 mg / mL, the upper surface of the composite polymer braid 1 is 0.2 mm away from the upper interface of the collagen solution, the lower surface of the composite polymer braid 1 is 2 mm away from the lower interface of the collagen solution, and the surrounding of the composite polymer braid 1 is 0.5 mm away from the interface of the collagen solution. The composite polymer braid 1 is soaked for 0.1 min and the soaking temperature of the composite polymer braid 1 is 30° C.
[0055] 2. Preliminary freezing: freeze-dry the soaking solution in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0056] 3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze dry for 72 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the composite polymer braid 1 to form a natural polymer coating 2.
[0057] Embodiment three:
[0058] 1. Soaking: soaking the composite polymer braid 1 with a thickness of 0.6 mm in a collagen solution, the natural polymer concentration is 0.4 mg / mL, the upper surface of the composite polymer braid 1 is 0.3 mm away from the upper interface of the collagen solution, the lower surface of the composite polymer braid 1 is 1.1 mm away from the lower interface of the collagen solution, and the surrounding of the composite polymer braid 1 is 0.5 mm away from the interface of the collagen solution. The braid 1 is soaked for 10 min and the soaking temperature of the composite polymer braid 1 is 35°C;
[0059] 2. Preliminary freezing: freeze-dry the soaking solution in the first step. First, repeatedly evacuate the container containing the soaking solution for several times and start freezing. Make the container pressure -20pa, maintain the negative pressure for 15min, and freeze at a rate of 1℃ / min until the temperature drops to -20℃. The freezing time is 2h.
[0060] 3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze dry for 48 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the composite polymer braid 1 to form a natural polymer coating 2.
[0061] In the above three embodiments, the composite polymer braided body 1 is composed of braided units of polyethylene terephthalate yarns and poly (L-lactic acid) yarns, and the braiding process of the braided units is warp knitting or weft knitting. In each embodiment, the mass ratio of polyethylene terephthalate to poly (L-lactic acid) is divided into four groups, namely 10:90, 60:40, 80:20, and 90:10, and the test results are averaged from the four groups.
[0062] Tensile strength test: The prepared composite polymer braid 1 is cut into strips by laser to obtain a test sample. The test sample is clamped on the upper and lower clamps of the tensile testing machine, and the testing machine is started. The movement speed of the clamp is 500mm / min, and the changes in the test length and force are monitored during the entire test. The polyethylene terephthalate braid sprayed with collagen is used as the control group 1, and the polyethylene terephthalate and poly (L-lactic acid) composite braid sprayed with collagen is used as the control group 2. Among them, the mixing method of the control group 2 is to compound a poly (L-lactic acid) layer outside the polyethylene terephthalate silk thread. The results are shown in Table 1 below.
[0063] Table 1 Tensile test results
[0064]
[0065] Animal experiment: The test samples and control samples were implanted subcutaneously in rats, with 5 parallel samples in each test group and control group. The degree of vascularization was evaluated after 1 week of feeding. The implant was cut out together with the skin, photographed, and the percentage of vascularization area was analyzed by ImageJ.
[0066] Table 2 Vascularization evaluation results
[0067]
[0068]
[0069] Rabbit rotator cuff model test: The skin was cut open at the shoulder joint of the front leg of a New Zealand white rabbit to expose the shoulder muscle, and a 1 cm defect was cut with a scalpel along the vertical direction of the muscle fiber. The patch in Example 2 was used as the experimental group, and sutured and reinforced along the muscle fiber direction. Evaluation was performed at 4, 8, 12, and 24 weeks, and the tendon tissue was removed, the braid was peeled off, and the tensile performance test was performed. The polyethylene terephthalate braid sprayed with collagen was used as the control.
[0070] Table 3 Evaluation results of rabbit rotator cuff model
[0071] Time Node Control group Experimental Group Reinforcement percentage 4 weeks 29±1.5N 50±1.0N 72.4% 8 weeks 54±2.2N 93±4.8N 72.2% 12 weeks 98±3.7N 142±3.3N 44.9% 24 weeks 107±3.2N 149±6.4N 39.3%
[0072] It can be seen from the tensile strength test results that the mechanical properties of the braided body can be regulated through the design and manufacture of the braiding process to meet the needs of different application scenarios. From the animal test results, it can be seen that compared with the spraying process, the natural polymer coating produced by the freeze-drying process has a higher degree of vascularization, indicating that the natural polymer coating 2 prepared by the freeze-drying process has a porous structure, which is conducive to the growth and vascularization of human tissue. From the results of the rabbit rotator cuff model test, it can be seen that compared with the spraying process, the natural polymer coating produced by the freeze-drying process can reduce the shear damage of the polymer silk thread to the muscle under normal physiological activities in the rotator cuff area, and better promote muscle repair.
[0073] Cytotoxicity test of cross-linking reagents:
[0074] (1) Extract preparation: Weigh the sample aseptically and add complete culture medium at a ratio of 0.2 g / mL of the sample mass. Extract the test sample and reference sample at (37°C±1)°C for (24±2) h under shaking conditions of 60 r / min. Take the extract and test it immediately.
[0075] (2) The cells that have been growing vigorously for 48 h to 72 h were digested and prepared into a density of 1 × 10 5 The cell suspension of 100 μL / ml was inoculated into a 96-well plate, with 100 μL per well, and cultured in a 5% CO2 incubator at 37°C for 24 h.
[0076] (3) Discard the original culture medium of the 96-well plate, add negative control solution, positive control solution, and sample solution to 5 wells respectively, and culture in a 5% CO2 incubator at 37°C for 24 h.
[0077] (4) After the culture is completed, observe the changes in cell morphology, vacuole formation, shedding, cell lysis, and membrane integrity under a microscope. Then discard the original culture medium, add 50 μL of MTT phenol red-free MEM culture solution, continue to culture for 2 hours, discard the old solution, add 100 μL of dimethyl sulfoxide, shake for 5 minutes, and measure the absorbance at 490 nm.
[0078] (5) If the cell viability of the sample group is less than 70% of that of the blank group, the sample has potential cytotoxicity. The cell viability calculation formula is as follows:
[0079]
[0080] Where:
[0081] OD 490e ——The average absorbance of 100% extract of the sample group;
[0082] OD 490b ——Average absorbance of blank group;
[0083] OD bg ——Average value of background absorbance.
[0084] Table 4 Cytotoxicity test results
[0085]
[0086] From the results in Table 4, it can be seen that the cross-linked products have certain cytotoxicity, induce cell apoptosis, and affect cell growth, proliferation and other behaviors, thereby affecting the final repair effect, while the non-cross-linked products can avoid this shortcoming.
[0087] In this application, a non-crosslinking method is used to produce the patch, which has low cytotoxicity and fast human tissue regeneration. The patch is combined with a partially degradable composite polymer braid and a natural polymer coating on its surface to achieve gradual degradation. During the growth of human tissue, space is gradually vacated to induce the tissue to combine with the patch, so that the final repair effect achieves a highly fused effect.
[0088] The present invention adopts a freeze-drying process, and the natural polymer remaining after the ice crystals sublimate to form a porous, sponge-like natural polymer coating 2. The natural polymer coating and the patch have a large bonding area and strong bonding strength, and the porosity of the composite patch is 50-90%. Since the coating has a porous structure, it is easier for the human body's own tissue growth to enter the patch, and the patch is more likely to make the rotator cuff and the humeral head tightly bonded to form an integral structure, accelerate the healing of the rotator cuff, and at the same time, the natural polymer coating 2 can also reduce the influence of the shear force of the polymer thread on the native tissue. The present invention adopts a purely physical method to form the natural polymer coating 2, without other chemical components generated by chemical reactions, and is more in line with the specifications of medical devices. The composite polymer braid 1 of the present invention can provide a higher initial fixation strength, reaching the initial strength of the rotator cuff; can make the gap between the rotator cuff and the humeral head smaller; the composite polymer braid 1 can still maintain mechanical stability after repeated human activities; the composite polymer braid 1 can still maintain mechanical stability when loaded with cyclic loads; the porous structure of the natural polymer coating 2 can optimize the biological environment of the "healing site" and reduce the shear force of the composite polymer braid 1 on the native tissue. More importantly, the natural polymer coating can reduce the shear damage of the polymer silk thread shear force to the native tissue, thereby promoting better and faster reconstruction of the tissue. In summary, the present invention is a very good rotator cuff repair material.
[0089] Specifically, the technical effects are as follows:
[0090] 1. The present invention sets the concentration of natural polymer to 0.01-1 mg / mL, the upper surface of the braid 1 is 0.01-1 mm away from the upper interface of the natural polymer solution, the lower surface of the braid 1 is 0.01-2 mm away from the lower interface of the natural polymer solution, and the surrounding of the braid 1 is 0.01-1 mm away from the interface of the collagen solution, so that the water content in the natural polymer solution is minimized and a natural polymer coating 2 of suitable thickness can be formed. The natural polymer coating 2 can reduce the influence of the shear force of the polymer threads on the composite polymer braid 1 on the native tissue. More importantly, the natural polymer coating can reduce the shear damage of the polymer threads to the native tissue, thereby promoting better and faster reconstruction of the tissue;
[0091] 2. The present invention arranges freeze drying to make the water molecules in the natural polymer form ice crystals and then sublime, and the remaining natural polymer forms a porous, sponge-like natural polymer coating 2. The pore structure is conducive to cell adhesion and growth, and at the same time reduces the influence of the shear force of the polymer wire of the composite polymer braid 1 on the native tissue;
[0092] 3. The braided unit 3 of the present invention is prepared by a braiding process, and the braided unit 3 has high tensile strength, mechanical strength, mechanical stability and good biological activity;
[0093] 4. Compared with adding drugs or porous, sponge-like natural polymer coating 2 around the patch to promote tissue growth, the natural polymer coating 2 has a weak bonding force with the patch. The present invention soaks the weaving unit 3 and then freeze-dries it, so that the porous, sponge-like natural polymer coating 2 has a strong bonding force with the weaving unit 3 and a large bonding contact area, and the generated tissue also has a strong bonding force with the patch.
[0094] 5. The combination of non-cross-linked production method and partially degradable polymer substrate results in faster tissue growth, higher degree of fusion and better stability of tissue regeneration.
[0095] The embodiments described above are only preferred implementation modes of the present invention and cannot be used to limit the protection scope of the present invention. Any non-substantial changes and modifications made by those skilled in the art on the basis of the invention shall fall within the protection scope of the present invention.
Claims
1. A composite patch for rotator cuff repair, characterized in that: It comprises a partially degradable composite polymer braided body, wherein the composite polymer braided body comprises polyethylene terephthalate and poly-L-lactic acid; The composite polymer braided body is in sheet form; The composite polymer braided body comprises one or more braided units manufactured by a braiding process; One surface or both surfaces of the composite polymer braided body are provided with a degradable natural polymer coating; The natural polymer coating is formed by attaching natural polymers in a natural polymer solution to a composite polymer braided body through a freeze-drying process. The natural polymer solution is a solution formed by dissolving natural polymers in physiological saline. The natural polymer coating is porous and sponge-like.
2. The composite patch according to claim 1, characterized in that: The multiple weaving units are stacked in the thickness direction, the multiple weaving units have the same shape, both ends of the multiple weaving units are connected, and two weaving units are connected through a natural polymer coating.
3. The composite patch according to claim 1, characterized in that: The mass ratio of polyethylene terephthalate to poly (L-lactic acid) in the composite polymer braid is 10:90-90:
10.
4. The composite patch according to claim 3, characterized in that: The mass ratio of polyethylene terephthalate to poly (L-lactic acid) in the composite polymer braid is 60:40-80:
20.
5. The composite patch according to claim 1, characterized in that: The composite polymer braid has a thickness of 0.1-1.5 mm and an ultimate tensile load of 200-1000 N.
6. The composite patch according to claim 5, characterized in that: The thickness of the composite polymer braid is 0.4-0.8 mm, and the ultimate tensile load of the composite polymer braid is 500-800N.
7. The composite patch according to claim 1, characterized in that: The knitting process is warp knitting or weft knitting.
8. A method for preparing a composite patch, characterized in that: The following steps are involved: S1. Soaking, soaking the composite polymer braid in a natural polymer solution, wherein the concentration of the natural polymer is 0.01-1 mg / mL, the upper surface of the composite polymer braid is 0.01-1 mm away from the upper interface of the natural polymer solution, the lower surface of the composite polymer braid is 0.01-2 mm away from the lower interface of the natural polymer solution, the surrounding of the composite polymer braid is 0.01-1 mm away from the interface of the collagen solution, the composite polymer braid is soaked for 0.1-60 min, and the composite polymer braid is soaked at a temperature of 0-40 ° C; S2. Preliminary freezing, freeze-drying the soaking solution in the first step, first repeatedly evacuate the container containing the soaking solution several times, and start freezing, so that the container pressure is -20pa, the negative pressure is maintained for 15-60min, the freezing cooling rate is 1℃ / min, until the temperature drops to -20℃, and the freezing time is 2h; S3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze drying for 24h-72h, freeze drying until completely dry, the natural polymers in the natural polymer solution adhere to the composite polymer braid to form a natural polymer coating.
9. The preparation method according to claim 8, characterized in that: The natural polymer concentration is 0.3-0.6 mg / mL, the upper surface of the composite polymer braid is 0.2-0.4 mm away from the upper interface of the natural polymer solution, the lower surface of the composite polymer braid is 0.4-2 mm away from the lower interface of the natural polymer solution, the immersion time of the composite polymer braid is 0.1-20 min, and the immersion temperature of the composite polymer braid is 25-35°C.
10. The preparation method according to claim 8, characterized in that: The following steps are involved: S1. Soaking, soaking a composite polymer braid with a thickness of 0.8 mm in a collagen solution, the collagen concentration is 0.6 mg / mL, the upper surface of the composite polymer braid is 0.2 mm away from the upper interface of the collagen solution, the lower surface of the composite polymer braid is 2 mm away from the lower interface of the collagen solution, the surrounding of the composite polymer braid is 0.5 mm away from the interface of the collagen solution, the composite polymer braid is immersed for 0.1 min, and the composite polymer braid is immersed at a temperature of 30°C; S2. Preliminary freezing, freeze-drying the soaking solution in the first step, first repeatedly evacuate the container containing the soaking solution several times, and start freezing, so that the container pressure is -20pa, the negative pressure is maintained for 15min, the freezing cooling rate is 1℃ / min, until the temperature drops to -20℃, and the freezing time is 2h; S3. Freeze drying, after freezing for 2 hours, cool down to -50°C at a rate of 2°C / min, freeze dry for 48 hours, freeze dry until completely dry, the natural polymer in the natural polymer solution adheres to the composite polymer braid to form a natural polymer coating.
Citation Information
Patent Citations
Soft tissue repair stent and preparation method thereof
CN114452034A
Composite material rotator cuff patch and preparation method thereof
CN116899015A
Composite patch for rotator cuff repair and preparation method thereof
CN117919507A
Methods of improving bone-soft tissue healing using electrospun fibers
US20180221537A1