Catalytic reaction system and catalytic filler for high-boiling cracking conversion of polycrystalline silicon and organic silicon

By loading active groups on the MCM-41 molecular sieve and combining it with a reactor system designed with a spiral channel, the problems of low gas-liquid reactor efficiency and insufficient catalyst stability in the existing technology are solved, and high-efficiency polycrystalline silicon and organic silicon are achieved. Boiling cracking conversion improves the stability of the catalyst and reaction efficiency.

CN118807828APending Publication Date: 2024-10-22NINGXIA SHENGLAN CHEM ENVIRONMENTAL PROT TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410803292.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing gas-liquid reactor has low reaction efficiency, low catalyst stability and activity, and low utilization rate, and cannot effectively improve the efficiency of the high-boiling cracking conversion process of polycrystalline silicon and organic silicon.

Method used

MCM-41 structure mesoporous molecular sieve containing 0.1-0.5% rutile TiO2 and ZrO2 is used as catalytic filler, loading R2P-, R2OP-, R2N- and other active groups, and fixed on the molecular sieve through -C-Si-O- chemical bond , combined with a reactor system designed with spiral channels, to optimize the active sites of the catalyst and reaction conditions.

Benefits of technology

It improves the rate and efficiency of the catalytic reaction, enhances the stability and utilization of the catalyst, optimizes product distribution, reduces the generation of by-products, extends the continuous operation cycle of the reactor, and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807828A_ABST
    Figure CN118807828A_ABST
Patent Text Reader

Abstract

The invention relates to a catalytic filler for high-boiling cracking conversion of polycrystalline silicon and organic silicon, the catalytic filler comprises a molecular sieve and an active group, and the active group and the molecular sieve are combined by a-C-Si-O-chemical bond. The invention also provides a reactor system loaded with the catalytic filler, which comprises a catalyst stacking module loaded with the catalytic filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photovoltaic raw materials, and in particular relates to a catalytic reaction system and catalytic filler for high-boiling cracking conversion of polysilicon and organic silicon. Background Art

[0002] Polysilicon is the most important raw material for the photovoltaic cell industry. Silicone materials are widely used in aerospace, military, electronic and electrical, chemical industries and other fields due to their excellent dielectric properties, high temperature resistance, physiological inertness, moisture resistance, insulation, and weather aging resistance. The production process of silicone and polysilicon produces high-boiling materials polysilane, which can undergo bond breaking reaction with hydrogen chloride under the action of catalysts. The reaction is usually carried out in a gas-liquid reactor with a catalyst.

[0003] However, the prior art has the following deficiencies: the reaction efficiency of the existing gas-liquid reactor is low, the stability and activity of the catalyst itself are low, and the utilization rate of the catalyst in the equipment is low. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art, namely, the low reaction efficiency of the existing gas-liquid reactor, the low stability and activity of the catalyst itself, and the low utilization rate of the catalyst in the equipment.

[0005] The present invention provides a catalytic filler for high-boiling cracking and conversion of polysilicon and organosilicon, characterized in that the catalytic filler comprises a molecular sieve and an active group, and the active group and the molecular sieve are bonded by a -C-Si-O- chemical bond.

[0006] Specifically, the molecular sieve is a medium-pore molecular sieve of MCM-41 structure containing 0.1-0.5% rutile TiO2, 0.1-0.5% ZrO2 and the remainder SiO2.

[0007] Specifically, the active group includes a combination of one or more of the four groups R2P-, R2OP-, R2N-, and RHN-, and R is an alkyl group of CnH3n-1.

[0008] Specifically, the value of n is 1-4.

[0009] A reactor system for high-boiling cracking and conversion of polysilicon and organosilicon loaded with the catalytic filler comprises a catalyst stacking module loaded with the catalytic filler.

[0010] Specifically, the reactor system further includes: a vaporizer, a vertical reactor and a condenser.

[0011] Specifically, the vertical reactor has a cylindrical inner cavity.

[0012] Specifically, a vaporizer is arranged at the lower part of the vertical reactor, and a high-boiling material inlet is arranged in the vaporizer. The high-boiling material is vaporized in the vaporizer, and the output port of the vaporizer is connected to an input port at the bottom of the reactor, and the vaporized high-boiling material enters the bottom of the reactor through the input port.

[0013] Specifically, another inlet is provided at the bottom of the vertical reactor, which is connected to a hydrogen chloride pipeline, and hydrogen chloride enters from the bottom of the vertical reactor via the hydrogen chloride pipeline and the other inlet.

[0014] Specifically, the catalyst stacking module has a material inlet and a material outlet at the upper and lower ends respectively.

[0015] The present invention provides the following technical effects:

[0016] 1) By loading specific active groups (R2P-, R2OP-, R2N-, RHN-) on the molecular sieve, active sites can be designed for the key steps in the polysilicon cracking process to improve the rate and efficiency of the catalytic reaction. The active groups can directly participate in or promote the formation and transformation of reaction intermediates, thereby accelerating the cracking process. Different active groups can lead to different reaction paths. By selecting specific group combinations (such as R2N-promoting the formation of specific CN bonds, R2P-participating in specific addition or elimination reactions), the distribution of products can be optimized, the selectivity of target products can be improved, and the generation of by-products can be reduced.

[0017] 2) MCM-41 molecular sieve containing 0.1-0.5% rutile TiO2 and ZrO2 provides excellent thermal stability and structural stability. Rutile TiO2 helps to improve the oxidation resistance of the molecular sieve, while the addition of ZrO2 enhances the mechanical strength and high temperature resistance of the molecular sieve, which helps to maintain the activity and structural integrity of the catalyst in long-term catalytic reactions.

[0018] 3) The stable combination of the mesoporous structure of the molecular sieve and the -C-Si-O-bond ensures that the gas-liquid phase reactants can effectively approach the active center and promote efficient mass transfer at the three-phase interface. At the same time, the open structure of the molecular sieve is conducive to the uniform distribution of thermal energy, preventing local overheating and maintaining the stability of the reaction conditions. The -C-Si-O-chemical bond provides a stable way to fix the active groups on the surface of the molecular sieve to prevent the loss or migration of active sites during the reaction. The -C-Si-O-chemical bond helps the active groups to be evenly dispersed on the surface of the molecular sieve, avoiding aggregation, thereby improving the catalytic efficiency. The -C-Si-O-chemical bond usually has high thermal stability, which helps to maintain the structure and performance of the catalyst under high temperature reaction conditions. The -C-Si-O-chemical bond may participate in the electron transfer process of the R2P-, R2OP-, R2N-, and RHN-active groups, thereby increasing the kinetics of the reaction.

[0019] 4) As the gas rises from the inlet along the spiral channel, its residence time on the catalyst is optimized. Compared with the straight-through design, the spiral design extends the path of the gas in the catalyst layer, thereby achieving a longer effective reaction contact time without increasing the volume of the reactor, which is conducive to complete reaction. Since the upper and lower parts of the second spiral channel involve the rotation direction conversion of the gas rotation and rise, the fluid shear stress and eddy current in the second spiral channel are large, requiring a larger conversion space. Setting a larger second rotating channel height has a relatively low gas flow velocity and a longer residence time. Under the action of shear stress and eddy current, the material and catalyst are mixed more fully, which is beneficial to the reaction process.

[0020] 5) The spiral ascending channel design increases the contact time, surface area and reaction pressure of the gas and the catalyst, although it improves the reaction efficiency. However, there are higher requirements for the stability of the catalyst. If the catalyst bonding is not firm, it is easy to cause failure. The solid catalyst provided by the present application, its active group is firmly bonded to the molecular sieve through the -C-Si-O- bond, ensuring the stability and efficient utilization of the active center. This combination not only enhances the catalytic activity, but also promotes more efficient mass transfer between the gas-solid-liquid three phases, especially for those complex reactions that require multi-phase participation, such as the interaction between gaseous hydrogen chloride and liquid or vapor reactants on the catalyst surface, which greatly improves the catalytic efficiency. The addition of rutile TiO2 and ZrO2 enhances thermal stability. The two are combined in the spiral channel reactor, which can more effectively manage the reaction temperature and heat transfer, help control the reaction rate, reduce side reactions, and optimize the reaction kinetics. The catalyst of the molecular sieve matrix has good mechanical stability, combined with the self-cleaning effect of the spiral channel design, which helps to reduce carbon deposition and catalyst blockage, extend the continuous operation cycle, and reduce maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to clearly illustrate the technical solution of the present invention, the drawings of specific implementation methods are briefly introduced below.

[0022] Figure 1 Schematic diagram of the reactor provided by the present invention

[0023] Figure 2 This is a structural diagram of the catalyst stacking module of the reactor provided by the present invention. DETAILED DESCRIPTION

[0024] The present invention will be described in more detail below with reference to the accompanying drawings, in which preferred embodiments of the present invention are shown, and it should be understood that those skilled in the art can modify the present invention described herein and still achieve the beneficial effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art, and not as a limitation of the present invention.

[0025] For the sake of clarity, not all features of the actual embodiments are described. In the following description, well-known functions and structures are not described in detail because they would obscure the present invention with unnecessary details. It should be recognized that in the development of any actual embodiment, a large number of implementation details must be made to achieve the specific goals of the developer.

[0026] In order to make the purpose and features of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the accompanying drawings are all in a very simplified form and use non-precise ratios, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0027] The present invention provides a gas-solid-liquid three-phase reaction system with higher reaction efficiency, which comprises an improved gas-liquid-solid three-phase reactor containing a solid catalyst (including a catalyst stacking structure in the reactor) and an improved solid catalyst. By combining the improved catalyst with the improved reactor, a mass transfer interface is provided for the gas reactant hydrogen chloride on the inner and outer surfaces of the solid catalyst, and a reaction interface for the liquid reactant or steam to contact hydrogen chloride on the catalyst surface is provided, thereby improving the reaction efficiency, the stability and activity of the catalyst itself, and the utilization rate of the catalyst.

[0028] The solid catalyst and the reactor provided by the present invention are described in detail below.

[0029] Solid Catalyst

[0030] The solid catalyst is composed of a molecular sieve and an active group loaded on the molecular sieve, wherein the molecular sieve is a medium-pore molecular sieve of MCM-41 structure containing 0.1-0.5% rutile TiO2, 0.1-0.5% ZrO2 and the rest SiO2.

[0031] The active group (X) includes a combination of one or more of the four groups R2P-, R2OP-, R2N-, and RHN-. n H 3n-1 The alkyl group is preferably n=1-4.

[0032] The active group (X) is bonded to the MCM-41 molecular sieve using a -C-Si-O- chemical bond, forming an XC-Si-O-MCM41 structure.

[0033] The above solid catalyst has the following effective effects:

[0034] By loading specific active groups (R2P-, R2OP-, R2N-, RHN-) on molecular sieves, active sites can be designed for key steps in the polysilicon cracking process to improve the rate and efficiency of the catalytic reaction. Active groups can directly participate in or promote the formation and conversion of reaction intermediates, thereby accelerating the cracking process. Different active groups can lead to different reaction paths. By selecting specific group combinations (such as R2N-promoting the formation of specific CN bonds, R2P-participating in specific addition or elimination reactions), the distribution of products can be optimized, the selectivity of target products can be improved, and the generation of by-products can be reduced.

[0035] MCM-41 molecular sieve containing 0.1-0.5% rutile TiO2 and ZrO2 provides excellent thermal stability and structural stability. Rutile TiO2 helps to improve the oxidation resistance of the molecular sieve, while the addition of ZrO2 enhances the mechanical strength and high temperature resistance of the molecular sieve, which helps to maintain the activity and structural integrity of the catalyst in long-term catalytic reactions.

[0036] The stable combination of the mesoporous structure of the molecular sieve and the -C-Si-O-bond ensures that the gas-liquid phase reactants can effectively approach the active center and promote efficient mass transfer at the three-phase interface. At the same time, the open structure of the molecular sieve is conducive to the uniform distribution of thermal energy, preventing local overheating and maintaining the stability of the reaction conditions. The -C-Si-O-chemical bond provides a stable way to fix the active groups on the surface of the molecular sieve to prevent the loss or migration of active sites during the reaction. The -C-Si-O-chemical bond helps the active groups to be evenly dispersed on the surface of the molecular sieve, avoiding aggregation, thereby improving the catalytic efficiency. The -C-Si-O-chemical bond usually has high thermal stability, which helps to maintain the structure and performance of the catalyst under high temperature reaction conditions. The -C-Si-O-chemical bond may participate in the electron transfer process of the R2P-, R2OP-, R2N-, and RHN-active groups, thereby increasing the kinetics of the reaction.

[0037] The preparation method of the above-mentioned solid catalyst comprises:

[0038] 1. Preparation of molecular sieves

[0039] Select silicon source material, template, dopant and solvent. Among them, the silicon source material is tetraethyl orthosilicate (TEOS), the template is hexadecyltrimethylammonium bromide (CTAB), the dopant is rutile TiO2 and ZrO2 precursors, tetrabutyl titanate (TBT) and tetrabutyl zirconate (TBOT) are used as soluble precursors, the concentration range is controlled at 0.1%-0.5% total solid mass ratio, and the solvent is water and ethanol (or isopropanol) for dissolution and pH adjustment.

[0040] The schematic raw material ratio can be: silicon source (tetraethyl orthosilicate, TEOS): 20% of the total solid mass, used to form the main component of the SiO2 skeleton; template (cetyltrimethylammonium bromide, CTAB): 2%-3% of the total solid mass, preferably 2.5%; rutile TiO2 precursor (tetrabutyl titanate, TBT) accounts for 0.45%-2.5% of the total solid mass, and ZrO2 precursor (tetrabutyl zirconate, TBOT) accounts for 0.27%-1.34% of the total solid mass. The mass ratio of the total amount of solvent (water and ethanol) to the total solid mass is 3:1, and the mass ratio of water to ethanol is 4:1-3:1.

[0041] The silicon source, template, rutile TiO2 and ZrO2 precursors are added to the solvent in proportion and fully mixed using a magnetic stirrer.

[0042] The mixed solution is transferred into a sealed reactor and hydrothermally crystallized at a temperature of 120°C to 150°C for 24 to 48 hours. In the temperature range of 120°C to 150°C, the orderly growth of the molecular sieve can be effectively promoted, while avoiding excessive temperature that causes structural collapse or excessive crystallization, affecting the regularity and size of the pores. The hydrothermal crystallization time is 24 to 48 hours. A shorter time may not be enough to form a complete and orderly molecular sieve structure, while a too long time may cause excessive crystal growth and affect the uniformity of the pore size.

[0043] After crystallization, the reaction mixture is cooled to room temperature, the solid is separated by filtration, and washed alternately with deionized water and ethanol to remove unreacted substances and templates. The washing frequency should be at least 3 times, and each washing should be thorough to ensure that the residue is minimal. Dry naturally or dry at low temperature (such as 50°C) in an oven. The dried sample is gradually heated to a high temperature in a nitrogen atmosphere. The specific heating curve is: first keep at a lower temperature (such as 300°C) for 2 hours to remove organic matter; then heat to 500-600°C and keep warm for 2-4 hours to form and stabilize rutile TiO2 and ZrO2 in the molecular sieve structure.

[0044] 2. Silanization treatment

[0045] 3-chloropropyltrimethoxysilane or 3-aminopropyltriethoxysilane is selected as the silane coupling agent. The molecular sieve and the silane coupling agent are mixed in anhydrous ethanol solvent, the mass ratio of the molecular sieve to the silane coupling agent is 3:10-3:17, heated to room temperature to 60°C, and the reaction time is 10-20 hours.

[0046] 3. Active group bonding

[0047] According to the required X group (R2P-, R2OP-, R2N-, RHN-), select a suitable organic compound as a precursor. R2P-selects di-n-butylphosphine chloride (DBPC) as a precursor, R2OP-selects dimethoxy (methyl)phosphonic acid (DMMP) as a precursor, R2N-selects N, N-dimethylammonium chloride (DMAC) as a precursor, and RHN-selects alkyl isonitrile as a precursor.

[0048] The silanized molecular sieve is mixed with the active group precursor in a solvent. Schematically, the silanized molecular sieve: active group precursor can be 5:9-5:18, which can be optimized according to specific parameters such as the precursor type. The mass ratio of the solvent to the active group precursor is: 5:1-10:1. Acetic acid (2wt%) is added as a catalyst to promote the reaction. It is carried out under nitrogen protection to avoid oxidation, the temperature range is from room temperature to 100°C, and the reaction time is 9-15 hours.

[0049] The bonded molecular sieves were dried in a vacuum, and then infrared spectroscopy (FTIR) was used to confirm the formation of -C-Si-O- chemical bonds.

[0050] -C-Si-O- chemical bonds provide a stable way to fix active groups on the surface of molecular sieves, preventing the loss or migration of active sites during the reaction. -C-Si-O- chemical bonds help to evenly disperse active groups on the surface of molecular sieves and avoid aggregation, thereby improving catalytic efficiency. -C-Si-O- chemical bonds usually have high thermal stability, which helps to maintain the structure and performance of the catalyst under high temperature reaction conditions. -C-Si-O- chemical bonds may participate in the electron transfer process of R2P-, R2OP-, R2N-, and RHN-active groups, thereby increasing the kinetics of the reaction.

[0051] Example 1

[0052] Silicon source (tetraethyl orthosilicate, TEOS): 20% of the total solid mass, used to form the main component of the SiO2 skeleton; template (hexadecyltrimethylammonium bromide, CTAB): 2.5% of the total solid mass; rutile TiO2 precursor (tetrabutyl titanate, TBT) accounts for 2.5% of the total solid mass, and ZrO2 precursor (tetrabutyl zirconate, TBOT) accounts for 1.34% of the total solid mass. The mass ratio of the total amount of solvent (water and ethanol) to the total solid mass is 3:1, and the mass ratio of water to ethanol is 4:1. Add the silicon source, template, rutile TiO2 and ZrO2 precursor to the solvent in proportion and mix them thoroughly using a magnetic stirrer.

[0053] The mixed solution was transferred into a sealed reactor and hydrothermally crystallized at 120°C for 24 hours. After the crystallization was completed, the reaction mixture was cooled to room temperature, the solid was separated by filtration, and washed alternately with deionized water and ethanol to remove unreacted substances and templates, and then naturally air-dried. The dried sample was gradually heated to a high temperature in a nitrogen atmosphere. The specific heating curve was: 300°C for 2 hours, 500°C for 4 hours.

[0054] The molecular sieve and 3-chloropropyltrimethoxysilane coupling agent were mixed in anhydrous ethanol solvent, with the mass ratio of the molecular sieve to the silane coupling agent being 3:10, and the mixture was heated to 60° C. and the reaction time was 10 hours.

[0055] Select di-n-butylphosphine chloride (DBPC), dimethoxy (methyl) phosphonic acid (DMMP), N, N-dimethylammonium chloride (DMAC) as precursors, and the mass ratio of the three is 1:1:1. Mix the silanized molecular sieve with the active group precursor in a solvent, the active group precursor can be 5:9, the mass ratio of the solvent to the active group precursor is: 5:1, and add acetic acid (2wt%) as a catalyst to promote the reaction. It is carried out under nitrogen protection to avoid oxidation, the temperature range is from room temperature to 100°C, and the reaction time is 9 hours. The doping concentrations of TiO2 and ZrO2 are both 0.5% by X-ray fluorescence spectroscopy (XRF), and the formation of -C-Si-O- chemical bonds is confirmed by infrared spectroscopy (IR). Thus, the catalyst in Example 1 is obtained.

[0056] Reactor system

[0057] The present invention also provides a reactor system, preferably, the reactor system can be used in conjunction with the above-mentioned solid catalyst. The above-mentioned solid catalyst is installed in a catalyst stacking module in the reactor system.

[0058] like Figure 1As shown, the reactor system provided by the present invention includes: a vaporizer, a vertical reactor and a condenser. The vertical reactor includes a catalyst stacking module. Among them, a vaporizer is arranged at the lower part of the vertical reactor, and the vaporizer is provided with a high-boiling material inlet, and the high-boiling material is vaporized in the vaporizer. The output port of the vaporizer is connected to an input port at the bottom of the reactor, and the vaporized high-boiling material enters the bottom of the reactor from the input port. Another input port at the bottom of the vertical reactor is connected to a hydrogen chloride pipeline, and hydrogen chloride enters from the bottom of the vertical reactor via the hydrogen chloride pipeline and the above-mentioned other inlet. After the high-boiling material and hydrogen chloride are mixed at the bottom of the vertical reactor, they pass through the catalyst stacking module and flow to the top of the vertical reactor. A condenser is arranged at the top of the vertical reactor, and a part of the condensed material refluxes to the top of the tower. The vaporized high-boiling material, hydrogen chloride, and condensed reflux material form a gas-solid-liquid three-phase reaction on the surface of the catalyst filler, and a cracking product is obtained from the top of the tower. The solid catalyst provides a mass transfer interface for the gaseous reactant hydrogen chloride on the inner and outer surfaces, and also provides a reaction interface for the liquid reactant or steam to contact hydrogen chloride on the catalyst surface, thereby improving the reaction efficiency, the stability and activity of the catalyst itself, and the utilization rate of the catalyst.

[0059] The reactor system provided by the present invention includes a catalyst stacking module, such as Figure 2 As shown, the catalyst stacking module has a spiral gas ascending channel, which is formed by arranging a spiral partition plate 34 coaxial with the cylindrical inner cavity of the vertical reactor and having a radius roughly similar to that of the vertical reactor, so as to divide the cylindrical inner cavity 4 of the vertical reactor into a spiral ascending channel. The solid catalyst is fixedly filled in the spiral ascending channel, and the high-boiling material and hydrogen chloride react under the catalysis of the active groups in the solid catalyst during the ascending process through the spiral channel.

[0060] The catalyst stacking module has a material inlet 1 and a material outlet 2 at the upper and lower ends, respectively. The material inlet 1 and the material outlet 2 have the shape of a conical surface, respectively, and the bottom surface openings of the conical surface are respectively oriented toward the feeding and discharging directions, that is, toward the bottom surface and toward the top surface. Corresponding openings (not shown) are provided at the positions of the inlet and outlet of the spiral ascending channel corresponding to the conical surface shapes of the material inlet 1 and the material outlet 2. The conical surface has a gas guiding function at the material inlet 1 and the material outlet 2, respectively. At the material inlet 1, as the material flows into the conical surface and flows upward, the gas volume is reduced, which plays a certain role in increasing the gas pressure (the increase in the material gas pressure is conducive to the contact between the material and the catalyst). At the material outlet 2, the gas product flows upward, the gas volume is relatively increased, and the gas pressure is slightly reduced, which can achieve a slight negative pressure extraction effect on the product gas, which is conducive to the outflow of the product.

[0061] As the gas rises from the inlet along the spiral channel, its residence time on the catalyst is optimized. Compared with the straight-through design, the spiral design prolongs the path of the gas in the catalyst layer, thereby achieving a longer effective reaction contact time without increasing the reactor volume, which is conducive to complete reaction.

[0062] Specifically, the spiral channel can be divided into three parts from bottom to top, namely, the first spiral channel 31, the second spiral channel 32, and the third spiral channel 33. The first spiral channel 31, the second spiral channel 32, and the third spiral channel 33 are separated by the first spiral baffle, the second spiral baffle, and the third spiral baffle in the cylindrical inner cavity of the vertical reactor at the corresponding position. In addition, the rotation directions of the two adjacent spiral channels in the first spiral channel 31, the second spiral channel 32, and the third spiral channel 33 are opposite, that is, under the condition of looking down vertically from the top of the reactor, the rotation directions of the first spiral channel 31 and the second spiral channel 32 are clockwise and counterclockwise (or counterclockwise and clockwise), respectively, and the rotation directions of the second spiral channel 32 and the third spiral channel 33 are counterclockwise and clockwise (or clockwise and counterclockwise), respectively. In order to realize the corresponding rotation directions of the first spiral channel 31, the second spiral channel 32 and the third spiral channel 33, the first spiral partition plate, the second spiral partition plate and the third spiral partition plate are arranged as spirally ascending partition plates twisted in corresponding directions around the inner wall axis.

[0063] The multiple reversals of the opposite rotation direction in the spiral ascending path can induce stronger shearing and eddy effects between the gas and the solid catalyst and possible liquid reactants, greatly enhancing the mass transfer and heat transfer efficiency between gas, solid and liquid. This means that the reactant molecules can contact the catalyst surface more frequently, speeding up the reaction rate and improving the conversion efficiency.

[0064] The channel heights of the first spiral channel 31, the second spiral channel 32, and the third spiral channel 33 remain unchanged and are constant values. However, the channel heights of the first spiral channel 31, the second spiral channel 32, and the third spiral channel 33 can be set to different values. Among them, the channel height of the second spiral channel 32 (i.e., the distance between the two corresponding layers of the second spiral partition in the vertical direction) is greater than the channel heights of the first spiral channel 31 and the third spiral channel 33 (i.e., the distance between the two corresponding layers of the first or third spiral partition in the vertical direction).

[0065] The design achieves the following technical effects by setting spiral channels of different heights, that is, the first spiral channel 31, the second spiral channel 32, and the third spiral channel 33 have spiral partitions with different spacings: Since the upper and lower parts of the second spiral channel 32 are involved in the rotation direction conversion of the gas rotation and rise, the fluid shear stress and vortex in the second spiral channel 32 are large, requiring a larger conversion space. The gas flow velocity is relatively low when the second rotating channel height is set larger, and the residence time is longer. Under the action of shear stress and vortex, the material and catalyst are mixed more fully, which is beneficial to the reaction process.

[0066] In contrast, the first and third spiral channels 31, 33 have smaller channel heights because: in channels with smaller heights, the gas pressure is greater and the gas flow rate is faster, which is suitable for the rapid reaction and high mass transfer rate required in the initial stage of the reaction in the first spiral channel, and after the third spiral channel receives more liquid reactants refluxed from the condenser, it requires a greater gas pressure and flow rate to promote the final stage of the solid-liquid-gas three-phase reaction.

[0067] Preferably, the channel heights of the first spiral channel 31 and the third spiral channel 33 are the same or different. Considering the cost of equipment manufacturing, the channel heights of the first spiral channel 31 and the third spiral channel 33 can be made to be the same height. Considering that the reflux liquid reactant in the third spiral channel requires a greater gas pressure and more gas materials for synergistic reaction, the height of the third spiral channel can be set to be different from the height of the first spiral channel, that is, the height of the third spiral channel is less than the height of the first spiral channel.

[0068] Preferably, the stacking density of the solid catalyst in the first and third spiral channels is greater than that in the second spiral channel. The stacking density of the solid catalyst in the second spiral channel is set smaller so that the material and the catalyst are mixed more fully, which is beneficial to the reaction process.

[0069] Synergistic effect of solid catalyst and reactor system

[0070] The solid catalyst and reactor system provided by the present invention both have their own beneficial effects and can be used separately in industry.

[0071] However, it is preferred that the solid catalyst of the present application is used in combination with a reactor. By applying the solid catalyst provided by the present invention to the above reactor system, the following additional synergistic technical effects are achieved:

[0072] 1. The spiral ascending channel design increases the contact time, surface area and reaction pressure of the gas and the catalyst, although it improves the reaction efficiency. However, there are higher requirements for the stability of the catalyst. If the catalyst bonding is not firm, it is easy to cause failure. The solid catalyst provided by the application, its active group is firmly bonded to the molecular sieve through -C-Si-O-bonds, ensuring the stability and efficient utilization of the active center. This combination not only enhances the catalytic activity, but also promotes more efficient mass transfer between the gas-solid-liquid three phases, especially for those complex reactions that require multiphase participation, such as the interaction between gaseous hydrogen chloride and liquid or vapor reactants on the catalyst surface, which greatly improves the catalytic efficiency.

[0073] 2. The addition of rutile TiO2 and ZrO2 enhances thermal stability. The combination of the two in the spiral channel reactor can more effectively manage reaction temperature and heat transfer, help control reaction rate, reduce side reactions, and optimize reaction kinetics. The catalyst based on the molecular sieve matrix has good mechanical stability. Combined with the self-cleaning effect of the spiral channel design, it helps to reduce carbon deposition and catalyst blockage, extend the continuous operation cycle, and reduce maintenance costs.

[0074] In summary, the present invention can achieve the following technical effects:

[0075] 1) By loading specific active groups (R2P-, R2OP-, R2N-, RHN-) on the molecular sieve, active sites can be designed for the key steps in the polysilicon cracking process to improve the rate and efficiency of the catalytic reaction. The active groups can directly participate in or promote the formation and transformation of reaction intermediates, thereby accelerating the cracking process. Different active groups can lead to different reaction paths. By selecting specific group combinations (such as R2N-promoting the formation of specific CN bonds, R2P-participating in specific addition or elimination reactions), the distribution of products can be optimized, the selectivity of target products can be improved, and the generation of by-products can be reduced.

[0076] 2) MCM-41 molecular sieve containing 0.1-0.5% rutile TiO2 and ZrO2 provides excellent thermal stability and structural stability. Rutile TiO2 helps to improve the oxidation resistance of the molecular sieve, while the addition of ZrO2 enhances the mechanical strength and high temperature resistance of the molecular sieve, which helps to maintain the activity and structural integrity of the catalyst in long-term catalytic reactions.

[0077] 3) The stable combination of the mesoporous structure of the molecular sieve and the -C-Si-O-bond ensures that the gas-liquid phase reactants can effectively approach the active center and promote efficient mass transfer at the three-phase interface. At the same time, the open structure of the molecular sieve is conducive to the uniform distribution of thermal energy, preventing local overheating and maintaining the stability of the reaction conditions. The -C-Si-O-chemical bond provides a stable way to fix the active groups on the surface of the molecular sieve to prevent the loss or migration of active sites during the reaction. The -C-Si-O-chemical bond helps the active groups to be evenly dispersed on the surface of the molecular sieve, avoiding aggregation, thereby improving the catalytic efficiency. The -C-Si-O-chemical bond usually has high thermal stability, which helps to maintain the structure and performance of the catalyst under high temperature reaction conditions. The -C-Si-O-chemical bond may participate in the electron transfer process of the R2P-, R2OP-, R2N-, and RHN-active groups, thereby increasing the kinetics of the reaction.

[0078] 4) As the gas rises from the inlet along the spiral channel, its residence time on the catalyst is optimized. Compared with the straight-through design, the spiral design extends the path of the gas in the catalyst layer, thereby achieving a longer effective reaction contact time without increasing the volume of the reactor, which is conducive to complete reaction. Since the upper and lower parts of the second spiral channel involve the rotation direction conversion of the gas rotation and rise, the fluid shear stress and eddy current in the second spiral channel are large, requiring a larger conversion space. Setting a larger second rotating channel height has a relatively low gas flow velocity and a longer residence time. Under the action of shear stress and eddy current, the material and catalyst are mixed more fully, which is beneficial to the reaction process.

[0079] 5) The spiral ascending channel design increases the contact time, surface area and reaction pressure of the gas and the catalyst, although it improves the reaction efficiency. However, there are higher requirements for the stability of the catalyst. If the catalyst bonding is not firm, it is easy to cause failure. The solid catalyst provided by the present application, its active group is firmly bonded to the molecular sieve through the -C-Si-O- bond, ensuring the stability and efficient utilization of the active center. This combination not only enhances the catalytic activity, but also promotes more efficient mass transfer between the gas-solid-liquid three phases, especially for those complex reactions that require multi-phase participation, such as the interaction between gaseous hydrogen chloride and liquid or vapor reactants on the catalyst surface, which greatly improves the catalytic efficiency. The addition of rutile TiO2 and ZrO2 enhances thermal stability. The two are combined in the spiral channel reactor, which can more effectively manage the reaction temperature and heat transfer, help control the reaction rate, reduce side reactions, and optimize the reaction kinetics. The catalyst of the molecular sieve matrix has good mechanical stability, combined with the self-cleaning effect of the spiral channel design, which helps to reduce carbon deposition and catalyst blockage, extend the continuous operation cycle, and reduce maintenance costs.

[0080] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A catalytic filler for high-boiling cracking and conversion of polysilicon and organosilicon, characterized by: The catalytic filler comprises a molecular sieve and an active group, wherein the active group and the molecular sieve are bonded by using a -C-Si-O- chemical bond.

2. The catalytic filler according to claim 1, characterized in that: The molecular sieve is a medium-pore molecular sieve of MCM-41 structure containing 0.1-0.5% rutile TiO2, 0.1-0.5% ZrO2 and the rest SiO2.

3. The catalytic filler according to claim 1, characterized in that: The active group includes a combination of one or more of the four groups R2P-, R2OP-, R2N-, and RHN-, and R is an alkyl group of CnH3n-1.

4. The catalytic filler according to claim 3, characterized in that: The value of n is 1-4.

5. A reactor system for high-boiling cracking and conversion of polysilicon and organosilicon loaded with the catalytic filler as claimed in claims 1 to 4, characterized in that: It comprises a catalyst stacking module, which is loaded with the catalytic filler as claimed in claims 1-4.

6. The reactor system according to claim 5, characterized in that: The reactor system further comprises: a vaporizer, a vertical reactor and a condenser.

7. The reactor system according to claim 5, characterized in that: The vertical reactor has a cylindrical inner cavity.

8. The reactor system according to claim 5, characterized in that: A vaporizer is arranged at the lower part of the vertical reactor. The vaporizer is provided with an inlet for high-boiling materials. The high-boiling materials are vaporized in the vaporizer. The output port of the vaporizer is connected to an input port at the bottom of the reactor. The vaporized high-boiling materials enter the bottom of the reactor through the input port.

9. The reactor system according to claim 8, characterized in that: Another inlet is arranged at the bottom of the vertical reactor, which is connected to a hydrogen chloride pipeline. Hydrogen chloride enters from the bottom of the vertical reactor via the hydrogen chloride pipeline and the other inlet.

10. The reactor system according to claim 5, characterized in that: The catalyst stacking module has a material inlet and a material outlet at the upper and lower ends respectively.

Citation Information

Patent Citations

  • Method for preparing catalyst for cracking organosilicon high-boiling product

    CN101298051A

  • System and method for synthesizing ethoxysilane in gas phase

    CN108383865A

  • Treatment system and method of high-boiling-point residues from low-temperature hydrogenation system

    CN109081351A

  • Organic amine catalyst for cracking organic silicon high-boiling residues and preparation method thereof

    CN116020554A

  • Method for preparing carboxylic acid through olefin oxidative cracking

    CN116178132A