Neutral inorganic molding sand casting material and preparation method thereof

By using materials such as quartz sand, water glass, and hybrid modified malt protein binders in the molding sand, a high-strength inorganic binder is formed, which solves the problems of harmful substance emissions and insufficient fire resistance in the existing molding sand, and achieves a better Environmentally friendly and high-performance casting material.

CN118808538AInactive Publication Date: 2024-10-22SHAANXI SCI TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411037287.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing molding sand contains a lot of organic binders and bentonite, and harmful compounds such as benzene, toluene, ethylbenzene, xylene, etc. are produced during the casting process, posing environmental pollution risks and lacking fire resistance and mechanical properties.

Method used

Neutral inorganic sand casting materials are used, including quartz sand, nanocellulose whiskers, water glass, hybrid modified malt protein binder and inert doped zirconia modified nanocore-shell materials, through carboxylated silicon powder The esterification reaction forms a high-strength ternary inorganic binder, which improves the compaction rate and fire resistance of the molding sand.

Benefits of technology

It significantly reduces the emission of toxic gases, improves the compaction rate and mechanical properties of molding sand, reduces the internal stress and sand sticking defects of castings, and improves the environmental performance and service life of casting materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004971438940000121
    Figure BDA0004971438940000121
Patent Text Reader

Abstract

The invention discloses a neutral inorganic molding sand casting material and a preparation method thereof, and relates to the technical field of molding sand casting materials. The preparation method comprises the following steps: preparing a ternary inorganic system adhesive composition composed of water glass, hydroxylation modified silica fume, a hybrid modified malt protein adhesive and an inert doped zirconium oxide modified nano core-shell material, grinding quartz sand, sieving, mixing the quartz sand, nano cellulose whiskers and the ternary inorganic system adhesive composition, and carrying out hot pressing to obtain the quartz sand. And preparing the neutral inorganic molding sand casting material. The prepared neutral inorganic molding sand casting material can reduce emission of toxic gas in the casting process, and can be stored and used for a long time; the compaction rate can be kept at a moderate level, and a casting is not prone to generating internal stress or cracking; the fire resistance is good, and the casting is not prone to burnt-on sand defects; and the strength is moderate, box collapse is not prone to occurring in the molding, carrying and box assembling processes, and the casting surface is not prone to being washed and damaged by liquid metal in the casting process, so that the defects of sand holes, sand inclusion and the like of a casting are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of molding sand casting materials, in particular to a neutral inorganic molding sand casting material and a preparation method thereof. Background Art

[0002] The main properties of molding sand include strength, plasticity, air permeability, refractoriness, yieldability, fluidity, compactness and collapsibility. 1. Strength refers to the ability of molding sand and sand core to resist external force damage, including compression, tension and shear strength; 2. Plasticity refers to the ability of molding sand to deform under the action of external force and to maintain the shape given by the external force after the external force is removed; 3. Air permeability refers to the ability of gas to pass through the compacted molding sand and the internal gaps of the molding sand; 4. Refractory refers to the ability of molding sand to withstand high temperature heat; 5. Yield refers to the ability of molding sand to be compressed when the casting condenses and shrinks; 6. Fluidity refers to the ability of molding sand to move relative to each other under the action of gravity or external force; 7. Collapsibility refers to the degree to which the mold is easy to collapse when the sand is dropped to clean the casting after casting is completed.

[0003] Many years of foundry practice and more accurate analysis methods have shown that although the molding sand containing more organic binders and binders based on bentonite has many technical advantages, there are many risks associated with the emission of harmful compounds. During the casting production process, due to the high temperature of the contact between the casting alloy and the molding sand, the organic components of the sand undergo thermal decomposition. In fact, several harmful compounds are formed, including gaseous and dusty substances such as benzene, toluene, ethylbenzene, xylene, polycyclic aromatic hydrocarbons and greenhouse gases: CO, CO2, NO x , SO2 and TVOC. Summary of the invention

[0004] The purpose of the present invention is to provide a neutral inorganic sand casting material and a preparation method thereof, so as to solve the problems raised in the background technology and provide a strategic adjustment direction for reference for the sustainable development of the foundry industry.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A neutral inorganic sand casting material comprises the following raw materials in parts by weight:

[0007] 80-120 parts of quartz sand;

[0008] Nanocellulose whiskers 0.2-0.8 parts;

[0009] 2.8-4.4 parts of water glass;

[0010] Hybrid modified malt protein adhesive 0.8-1.2 parts;

[0011] 0.1-0.5 parts of inert doped zirconium oxide modified nano core-shell material;

[0012] 1-2 parts of carboxylated silicon powder.

[0013] The carboxylated silicon micropowder is prepared by uniformly dispersing equimolar silane coupling agent and succinic anhydride in N,N-dimethylformamide solution for homogenization, adding silicon micropowder dispersion liquid dispersed by ultrasound for further homogenization, and washing by centrifugation.

[0014] It should be noted that the carboxylation of the surface of silica powder is to provide carboxyl groups for the subsequent establishment of a ternary inorganic binder system with water glass as the core, and for the self-generated ester self-hardening.

[0015] Furthermore, the modulus of water glass is 2.6-3.1, the silicon dioxide content in water glass is 29.3-33.5%, and the sodium oxide content is 9.8-13.6%.

[0016] Further, the preparation steps of the hybrid modified malt protein adhesive are as follows:

[0017] A1. Add acrylpimaric acid, epichlorohydrin and benzyltriethylammonium chloride into a flask, stir at 115-120°C for 2h under nitrogen atmosphere, cool to 60°C, add sodium hydroxide and calcium oxide, continue stirring at 60°C for 3h, filter with a diatomaceous earth filter, vacuum distill at 100°C, react the reduced pressure distillation product with dopamine hydrochloride at 80°C for 1h to obtain an organic antibacterial skeleton;

[0018] A2. Add ethanol to wheat germ powder, stir at room temperature for 15 minutes, add an organic antibacterial skeleton, stir vigorously for 20 minutes, and distill under reduced pressure to obtain a hybrid modified malt protein adhesive.

[0019] Furthermore, in step A1, the mass ratio of acrylpimaric acid epichlorohydrin, benzyltriethylammonium chloride, sodium hydroxide, calcium oxide and dopamine hydrochloride is 50:150:1.52:10.68:14.98:7.9.

[0020] It should be noted that, through the ring-opening reaction, an organic antibacterial skeleton with a unique hybrid enhanced structure of rosin acid derivatives and dopamine hydrochloride (DOPA) was constructed, and the organic antibacterial skeleton was added to the malt protein alcohol solution, and a strong cross-linked network was formed through various interactions such as covalent bonds, hydrogen bonds and metal coordination bonds. Due to the introduction of hydrophobic rings and the formation of cross-linked network structures, the interaction between the active groups in the compound and -OH, -COOH and -NH2 in the malt protein reduced the clutter between molecules and increased the residual rate and moisture absorption rate of the adhesive. Wheat germ powder contains rich protein and polysaccharide nutrients. When it acts as an adhesive, it is easily infected by spoilage bacteria, and the protein structure is destroyed to produce harmful gases such as hydrogen sulfide, resulting in the loss of bonding performance, the destruction of the bonding structure, and the decrease of bonding strength and durability. Therefore, the addition of a tightly cross-linked organic antibacterial skeleton with antibacterial and anticorrosive functions makes the malt protein adhesive have anti-mildew ability and antibacterial properties, which is of great significance for improving storage performance and ensuring long-term use.

[0021] Furthermore, in step A2, the usage ratio of wheat germ powder, ethanol and organic antibacterial skeleton is (22.5-37.5) g: (80-100) mL: (0.9-2.7) g.

[0022] It should be noted that the gliadin in wheat germ powder is soluble in organic solvents and can form an interpenetrating cross-linked macromolecular polymer network with the organic antibacterial skeleton. The hybrid modified malt protein adhesive with wheat germ powder as the main raw material, as a part of the inorganic binder system in the subsequent treatment, can not only keep the compaction rate of the molding sand at a moderate level, but also reduce the generation and emission of toxic gases during the casting process compared to organic binders. At the same time, the phenolic hydroxyl groups on the organic antibacterial skeleton can provide hydroxyl groups for the self-generation of esters and self-hardening of the ternary inorganic system binder.

[0023] Furthermore, the steps for preparing the inert doped zirconium oxide modified nano core-shell material are as follows:

[0024] B1. Grind the yttrium oxide doped zirconia powder, sieve it with a 600 mesh sieve under dry conditions, blend it with water glass, let it stand for 30 minutes, heat it from room temperature to 1550°C, calcine it at 1550°C for 2 hours, cool it to room temperature at 10°C / min, use an air abrasion device to abrade the sample with Al2O3 particles with a particle size of 50μm at 0.2MPa (20s, 10mm), and dry it at 100°C in an inert atmosphere for 1 hour to obtain a pre-treated yttrium doped zirconia powder;

[0025] B2. Disperse the pretreated yttrium-doped zirconia powder in polydimethylsiloxane alcohol, homogenize for 4-6 hours, filter, wash, dry at room temperature for 24 hours, and then dry in a vacuum environment at 100° C. for 3 hours to obtain an inert doped zirconia modified nano core-shell material.

[0026] 7. A neutral inorganic sand casting material according to claim 6, characterized in that the yttria content in the yttria-doped zirconium oxide powder in step B1 is 8.3-8.8%.

[0027] It should be noted that when zirconium oxide is used in an inorganic bonding system, it can improve the mechanical properties of casting materials by preventing sodium silicate from agglomerating. Sodium silicate softens at about 900°C, cannot tightly bind to sand particles and shrinks. Yttria-doped zirconium oxide powder with a high melting point and excellent high-temperature stability can significantly limit the thermal expansion behavior of molding sand during warm casting, promote sand shrinkage, and improve the compactness of molding sand casting materials.

[0028] Furthermore, in step B1, the dosage ratio of yttria-doped zirconia powder to water glass is (0.8-3.2) mg:30 mL.

[0029] It should be noted that yttria-doped zirconia is stable and difficult to modify on the surface. It needs to be pre-treated with water glass to generate a silica phase and roughen the surface before silanization. Micromechanical adhesion depends on surface roughness. The surface texture consists of tiny irregularities, such as bumps and dents. The higher the surface roughness, the higher the bond strength, providing retention and stability through mechanical interlocking and adhesive chemical bonding. The water glass pre-treatment operation slightly increases the surface roughness of yttria-doped zirconia, changes its surface properties, improves bond strength, and allows the use of polydimethylsiloxane alcohol to silanize and functionalize its surface.

[0030] Furthermore, in step B2, the ratio of the pre-treated yttrium-doped zirconium oxide powder to polydimethylsiloxane alcohol is (0.05-0.2) mg:3 mL.

[0031] It should be noted that the surface-generated silica yttria-doped zirconium oxide powder is in-situ polymerized in polydimethylsiloxane alcohol, and the surface hydroxyl groups of the core-shell structure can provide hydroxyl groups for the self-esterification and self-hardening of the ternary inorganic system binder. At the same time, polydimethylsiloxane alcohol covers the silica phase more evenly, and from the perspective of molecular dynamics, it can limit the mobility of silica after sodium silicate loses water, and disperse and fix the silica in the molding sand matrix.

[0032] Furthermore, a method for preparing a neutral inorganic sand casting material comprises the following specific steps:

[0033] S1. Grind quartz sand using a ball mill and pass it through a 150-250 mesh sieve;

[0034] S2, mixing water glass, hybrid modified malt protein binder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder at room temperature for 24-48 hours to obtain a ternary inorganic system binder composition;

[0035] S3. Mix the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 1-10 minutes to obtain a neutral inorganic sand casting material.

[0036] It should be noted that, under low temperature conditions, the hydroxyl groups connected to the hybrid modified malt protein binder and the inert doped zirconium oxide modified nano core-shell material in the ternary inorganic system binder composition react with the carboxyl groups on the carboxylated silicon micropowder to generate ester bonds through esterification reaction, which are partially hydrolyzed when combined with water glass to generate organic acids or alcohols, thereby increasing the modulus of the water glass. When the viscosity of the water glass exceeds the critical value, it loses fluidity and solidifies. As the reaction proceeds, the water glass further loses water and hardens. The ternary inorganic system binder composition uses the ester hardening method of self-generated esters to obtain fine water glass gel particles. This is because the silicon hydroxyl groups on the carboxylated silicon micropowder and the surface of the polysilicic acid are bonded by hydrogen bonds, that is, the carboxylated silicon micropowder is bound to the high polysilicate particles through hydrogen bonds to inhibit the growth of the particles, and the hardened system finally formed has a higher strength. The hydroxyl groups on the hybrid modified malt protein adhesive and the inert doped zirconium oxide modified nano core-shell material are partially reacted and partially esterified, and alcohol is self-generated and adsorbed on the surface of silica gel particles, which hinders the latter from increasing. The finer the particles, the more bonding points there are per unit volume of silica gel, which can improve the bonding strength of water glass. At the same time, the alcohol hydrolyzed by the ester hardening of the self-generated ester has strong water absorption, which can make the water glass dehydrate quickly during the curing process, greatly improve the curing speed, and improve the hardness and permeability, which affects the structure of silica gel and is conducive to improving the bonding strength, curing rate, viscosity and flow properties and other properties of water glass.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] The present invention uses pure natural wheat germ powder as a raw material to participate in the inorganic adhesive system, which can reduce the emission of toxic gases. The organic antibacterial skeleton of the special hybrid reinforcement structure is prepared through the ring-opening reaction, so that the malt protein adhesive has anti-mildew ability and antibacterial properties, improves storage performance and ensures long-term use, can keep the compaction rate of the molding sand at a moderate level, and the casting is not easy to generate internal stress or cracking.

[0039] The present invention adopts yttria-doped zirconium oxide powder, which can significantly limit the thermal expansion behavior of molding sand during warm casting, promote sand grain shrinkage, improve the compactness of molding sand casting materials, and improve the mechanical properties of casting materials, so that the molding sand has good refractory properties and the casting is not prone to sand sticking defects. The surface of yttria-doped zirconium oxide is pre-treated with water glass to generate a silicon dioxide phase and a rough surface, and then silanized. Increasing the surface roughness and improving the bonding strength can limit the mobility of silicon dioxide after sodium silicate loses water, and disperse and fix the molding sand matrix silicon dioxide.

[0040] In the ternary inorganic system binder composition prepared by the present invention, the hybrid modified malt protein binder, the inert doped zirconium oxide modified nano core-shell material and the carboxylated silicon powder are partially esterified, and the ester bond is partially hydrolyzed when combined with water glass, and the water glass further dehydrates and hardens. The ester hardening method using the self-generated ester is used to ensure that the hardening system has a high strength and improve the bonding strength of the water glass. At the same time, the ester hardening hydrolysis of the self-generated ester can make the water glass dehydrate quickly during the curing process, greatly improve the hardening speed, and also improve the hardness and permeability, which is conducive to improving the bonding strength, curing rate, viscosity and other properties of the water glass. Compared with organic binders, the ternary inorganic bonding system has a significant contribution to reducing harmful air emissions and improving indoor air conditions in the workplace, and can reduce harmful substances in foundry sand and reduce the amount of foundry sand to be landfilled. The present invention adopts a ternary inorganic system binder composition and utilizes the self-hardening of autogenous ester to prepare molding sand with moderate strength. It is not easy to cause box collapse during the molding, transportation and box assembling processes. During the casting process, the surface of the mold is not easily damaged by liquid metal, causing defects such as sand holes and sand inclusions in the casting. DETAILED DESCRIPTION

[0041] The following will be described clearly and completely in conjunction with the technical solutions of the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The preparation steps of carboxylated silicon powder are as follows:

[0043] 0.44 g of silane coupling agent KH-550 and 0.2 g of succinic anhydride were uniformly dispersed in 10 mL of N, N-dimethylformamide, and magnetically stirred at 300 r / min for 3 h. Then, 20 mL of 10 mg / mL silicon micropowder dispersion was added to the system after ultrasonic dispersion, and 2 mL of deionized water was added at the same time. The mixture was magnetically stirred at 600 r / min for 5 h, centrifuged, and washed to obtain carboxylated silicon micropowder.

[0044] The preparation steps of hybrid modified malt protein adhesive are as follows:

[0045] A1. Add 50 g of acrylpimaric acid, 150 g of epichlorohydrin and 1.52 g of benzyltriethylammonium chloride into a flask, stir at 117° C. for 2 h under a nitrogen atmosphere, cool to 60° C., add 10.68 g of sodium hydroxide and 14.98 g of calcium oxide, continue stirring at 60° C. for 3 h, filter with a diatomaceous earth filter, vacuum distill at 100° C., react the reduced pressure distillation product with 7.9 g of dopamine hydrochloride at 80° C. for 1 h to obtain an organic antibacterial skeleton;

[0046] A2, 30g wheat germ powder was added to 90mL ethanol, and stirred at room temperature for 15min. Then, 1.8g organic antibacterial skeleton was added, and the mixture was stirred vigorously for 20min, and vacuum distilled to obtain a hybrid modified malt protein adhesive.

[0047] The preparation steps of inert doped zirconium oxide modified nano core-shell material are as follows:

[0048] B1. Grind the yttrium oxide doped zirconia powder, sieve it with a 600 mesh sieve under dry conditions, blend 2 mg with 30 mL of water glass, let it stand for 30 min, heat it from room temperature to 1550° C., calcine it at 1550° C. for 2 h, cool it to room temperature at 10° C. / min, use an air abrasion device to abrade the sample with Al2O3 particles with a particle size of 50 μm at 0.2 MPa (20 s, 10 mm), and dry it at 100° C. in an inert atmosphere for 1 h to obtain a pre-treated yttrium doped zirconia powder;

[0049] B2. Disperse 0.125 mg of pre-treated yttrium-doped zirconia powder in 3 mL of polydimethylsiloxane alcohol, homogenize for 4-6 hours, filter, wash, dry at room temperature for 24 hours, and then dry in a vacuum environment at 100° C. for 3 hours to obtain an inert doped zirconia modified nano core-shell material.

[0050] Example 1

[0051] A neutral inorganic sand casting material is made from the following raw materials in parts by weight:

[0052] 100 parts of quartz sand;

[0053] 3.6 parts of water glass;

[0054] 1 part of hybrid modified malt protein adhesive;

[0055] 0.3 parts of inert doped zirconium oxide modified nano core-shell material;

[0056] 0.5 parts of nanocellulose whiskers (aspect ratio of 500:1);

[0057] 1.5 parts of carboxylated silicon powder.

[0058] A method for preparing a neutral inorganic sand casting material comprises the following specific steps:

[0059] S1, use a ball mill to grind quartz sand and pass it through a 200 mesh sieve;

[0060] S2, mixing water glass, hybrid modified malt protein binder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder at room temperature for 24 hours to obtain a ternary inorganic system binder composition;

[0061] S3. Mix the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 5 minutes to obtain a neutral inorganic sand casting material.

[0062] Example 2

[0063] A neutral inorganic sand casting material is made from the following raw materials in parts by weight:

[0064] 80 parts of quartz sand;

[0065] 2.8 parts of water glass;

[0066] 0.8 parts of hybrid modified malt protein adhesive;

[0067] 0.1 part of inert doped zirconium oxide modified nano core-shell material;

[0068] Nanocellulose whiskers (aspect ratio of 500:1) 0.2 parts;

[0069] 1 part of carboxylated silicon powder.

[0070] A method for preparing a neutral inorganic sand casting material comprises the following specific steps:

[0071] S1, use a ball mill to grind quartz sand and pass it through a 200 mesh sieve;

[0072] S2, mixing water glass, hybrid modified malt protein binder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder at room temperature for 24 hours to obtain a ternary inorganic system binder composition;

[0073] S3. Mix the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 5 minutes to obtain a neutral inorganic sand casting material.

[0074] Example 3

[0075] A neutral inorganic sand casting material is made from the following raw materials in parts by weight:

[0076] 120 parts of quartz sand;

[0077] 4.4 parts of water glass;

[0078] 1.2 parts of hybrid modified malt protein adhesive;

[0079] 0.5 parts of inert doped zirconium oxide modified nano core-shell material;

[0080] Nanocellulose whiskers (aspect ratio of 500:1) 0.8 parts;

[0081] 2 parts of carboxylated silicon powder.

[0082] A method for preparing a neutral inorganic sand casting material comprises the following specific steps:

[0083] S1, use a ball mill to grind quartz sand and pass it through a 200 mesh sieve;

[0084] S2, mixing water glass, hybrid modified malt protein binder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder at room temperature for 24 hours to obtain a ternary inorganic system binder composition;

[0085] S3. Mix the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 5 minutes to obtain a neutral inorganic sand casting material.

[0086] Comparative Example 1

[0087] A neutral inorganic sand casting material is made from the following raw materials in parts by weight:

[0088] 100 parts of quartz sand;

[0089] 3.6 parts of water glass;

[0090] 1 part wheat germ powder;

[0091] 0.3 parts of inert doped zirconium oxide modified nano core-shell material;

[0092] 0.5 parts of nanocellulose whiskers (aspect ratio of 500:1);

[0093] 1.5 parts of carboxylated silicon powder.

[0094] A method for preparing a neutral inorganic sand casting material comprises the following specific steps:

[0095] S1, use a ball mill to grind quartz sand and pass it through a 200 mesh sieve;

[0096] S2, mixing water glass, wheat germ powder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder at room temperature for 24 hours to obtain a ternary inorganic system binder composition;

[0097] S3. Mix the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 5 minutes to obtain a neutral inorganic sand casting material.

[0098] The difference between this comparative example and Example 1 is that the hybrid modified malt protein adhesive is not added, but unmodified wheat germ powder is added.

[0099] Comparative Example 2

[0100] A neutral inorganic sand casting material is made from the following raw materials in parts by weight:

[0101] 100 parts of quartz sand;

[0102] 3.6 parts of water glass;

[0103] 1 part of hybrid modified malt protein adhesive;

[0104] 0.3 parts of yttria-doped zirconium oxide;

[0105] 0.5 parts of nanocellulose whiskers (aspect ratio of 500:1);

[0106] 1.5 parts of carboxylated silicon powder.

[0107] A method for preparing a neutral inorganic sand casting material comprises the following specific steps:

[0108] S1, use a ball mill to grind quartz sand and pass it through a 200 mesh sieve;

[0109] S2, mixing water glass, hybrid modified malt protein binder, yttria-doped zirconium oxide and carboxylated silicon powder at room temperature for 24 hours to obtain a ternary inorganic system binder composition;

[0110] S3. Mix the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 5 minutes to obtain a neutral inorganic sand casting material.

[0111] The difference between this comparative example and Example 1 is that inert doped zirconium oxide modified nano core-shell material is not added, but unmodified yttria doped zirconium oxide is added.

[0112] Comparative Example 3

[0113] A neutral inorganic sand casting material is made from the following raw materials in parts by weight:

[0114] 100 parts of quartz sand;

[0115] 3.6 parts of water glass;

[0116] 1 part wheat germ powder;

[0117] 0.3 parts of yttria-doped zirconium oxide;

[0118] 0.5 parts of nanocellulose whiskers (aspect ratio of 500:1);

[0119] 1.5 parts of silicon powder.

[0120] A method for preparing a neutral inorganic sand casting material comprises the following specific steps:

[0121] S1, use a ball mill to grind quartz sand and pass it through a 200 mesh sieve;

[0122] S2, mixing water glass, wheat germ powder, yttria-doped zirconium oxide and silicon powder at room temperature for 24 hours to obtain a ternary inorganic system binder composition;

[0123] S3. Mix the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 5 minutes to obtain a neutral inorganic sand casting material.

[0124] The difference between this comparative example and Example 1 is that no hybrid modified malt protein binder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder are added, but unmodified wheat germ powder, yttria doped zirconium oxide and silicon powder are used.

[0125] test:

[0126] 1. Molding sand performance test

[0127] The test method refers to the following standards:

[0128] GB / T 2684-2009 Test methods for foundry sand and mixtures;

[0129] JB / T 13038-2017 "Mixed binders for green sand casting";

[0130] JIS Z2601-1993 "Determination of properties of foundry sand";

[0131] JB / T 13082-2017 "Inorganic binder coated wet sand for non-ferrous alloy casting".

[0132] The test results are shown in Table 1.

[0133] 2. Adhesive performance test:

[0134] The test object is the ternary inorganic system binder composition prepared in step S2 of Example 1

[0135] The test method refers to the following standards:

[0136] JB / T 13038-2017 "Mixed binders for green sand casting";

[0137] The test results are shown in Table 2.

[0138] 3. Test Results Summary

[0139]

[0140] Table 1

[0141] Instant tensile strength (MPa) 24h tensile strength (MPa) Viscosity (MPa·s) Adhesive composition 1.1 1.8 103

[0142] Table 2

[0143] IV. Conclusion and Discussion

[0144] 1. As shown in Table 1, the various properties of Examples 1-3 are better than those of Comparative Examples 1-3, with a compaction rate between 35% and 40%, moderate strength, less loss on ignition, air permeability above 95%, and a crushing index between 80% and 90%, which meet the standards of excellent molding sand.

[0145] 2. As can be seen from Table 1, the various properties of Comparative Example 3 are relatively backward compared with Comparative Examples 1 and 2. This is because the ternary inorganic system binder composition in Comparative Example 3 does not add hybrid modified malt protein binder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder, and uses unmodified raw materials. The prepared molding sand has poor performance and is difficult to put into actual production.

[0146] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A neutral inorganic sand casting material, characterized by: It includes the following raw materials in parts by weight: 80-120 parts of quartz sand; 0.2-0.8 parts of nanocellulose whiskers; 2.8-4.4 parts of water glass; 0.8-1.2 parts of hybrid modified malt protein adhesive; 0.1-0.5 parts of inert doped zirconia modified nano core-shell material; 1-2 parts of carboxylated silicon powder.

2. The neutral inorganic sand casting material according to claim 1, characterized in that: The modulus of water glass is 2.6-3.1, the silicon dioxide content in water glass is 29.3-33.5%, and the sodium oxide content is 9.8-13.6%.

3. The neutral inorganic sand casting material according to claim 1, characterized in that: The preparation steps of the hybrid modified malt protein adhesive are as follows: A1. Add propylene pimaric acid, epichlorohydrin, and benzyltriethylammonium chloride to a flask, stir at 115-120°C for 2 hours under a nitrogen atmosphere, cool to 60°C, add sodium hydroxide and calcium oxide, continue stirring at 60°C for 3 hours, filter through a diatomaceous earth filter, and vacuum distill at 100°C. The reduced pressure distillation product is reacted with dopamine hydrochloride at 80°C for 1 hour to obtain an organic antibacterial skeleton; A2. Wheat germ powder was added to ethanol, stirred at room temperature for 15 minutes, and an organic antibacterial skeleton was added. The mixture was vigorously stirred for 20 minutes and distilled under reduced pressure to obtain a hybrid modified malt protein adhesive.

4. The neutral inorganic sand casting material according to claim 3, characterized in that: In step A1, the mass ratio of propylene pimaric acid, epichlorohydrin, benzyltriethylammonium chloride, sodium hydroxide, calcium oxide and dopamine hydrochloride is 50:150:1.52:10.68:14.98:7.

9.

5. The neutral inorganic sand casting material according to claim 3, characterized in that: The usage ratio of wheat germ powder, ethanol and organic antibacterial skeleton in step A2 is (22.5-37.5) g: (80-100) mL: (0.9-2.7) g.

6. The neutral inorganic sand casting material according to claim 1, characterized in that: The preparation steps of inert doped zirconia modified nano core-shell material are as follows: B1. Grind yttrium oxide-doped zirconia powder, sieve it through a 600-mesh sieve under dry conditions, blend it with water glass, let it stand for 30 minutes, heat it from room temperature to 1550°C, calcine it at 1550°C for 2 hours, cool it to room temperature at a rate of 10°C / min, abrade the sample using an air abrasion device, and dry it under an inert atmosphere at 100°C for 1 hour to obtain pre-treated yttrium oxide-doped zirconia powder; B2. Disperse the pretreated yttrium-doped zirconia powder in polydimethylsiloxane, homogenize for 4-6 hours, filter, wash, dry at room temperature for 24 hours, and then dry in a vacuum environment at 100° C. for 3 hours to obtain an inert doped zirconia modified nano core-shell material.

7. The neutral inorganic sand casting material according to claim 6, characterized in that: The yttrium oxide content in the yttrium oxide-doped zirconia powder in step B1 is 8.3-8.8%.

8. The neutral inorganic sand casting material according to claim 6, characterized in that: In step B1, the usage ratio of yttria-doped zirconia powder and water glass is (0.8-3.2) mg:30 mL.

9. The neutral inorganic sand casting material according to claim 6, characterized in that: In step B2, the ratio of the pre-treated yttrium-doped zirconia powder to polydimethylsiloxane alcohol is (0.05-0.2) mg:3 mL.

10. A method for preparing the neutral inorganic sand casting material according to any one of claims 1 to 9, characterized in that: The specific steps are: S1. Grind quartz sand using a ball mill and pass it through a 150-250 mesh sieve; S2, mixing water glass, hybrid modified malt protein binder, inert doped zirconium oxide modified nano core-shell material and carboxylated silicon powder at room temperature for 24-48 hours to obtain a ternary inorganic system binder composition; S3. Mixing the treated quartz sand, nanocellulose whiskers and the ternary inorganic system binder composition at room temperature for 1-10 minutes to prepare a neutral inorganic molding sand casting material.