Release agent for liquid die forging and preparation method thereof

By using water-based liquid die forging release agents, combined with inorganic powders and organic lubricants, the quality and safety hazards of castings caused by existing release agents in the liquid die forging process are solved, and higher castings are achieved. Air tightness and density improve casting yield and mold service life.

CN118808541AActive Publication Date: 2024-10-22BYD CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410728138.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-22
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

In the existing liquid die forging process, the commonly used release agents are mainly composed of organic polymers and graphite, which makes it more difficult to clean and paint the castings in the later stage. It has poor high temperature resistance and is easy to decompose to produce carbon deposits and volatile substances, which affects the castings. The mechanical properties and molding quality are poor, but there are also potential safety hazards.

Method used

A water-based liquid release agent for die forging, combined with an appropriate amount of inorganic powder and a small amount of organic lubricant, provides good thermal insulation and lubrication effects, improves the fluidity of liquid metal, and forms airtightness and density. Castings have the advantages of green environmental protection, low cost and simple preparation method.

Benefits of technology

It improves the air tightness and density of automotive functional parts with complex shapes and structures, reduces casting defects, improves casting yield, avoids safety hazards in subsequent processing, and extends the service life of molds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004879375010000021
    Figure BDA0004879375010000021
  • Figure BDA0004879375010000071
    Figure BDA0004879375010000071
  • Figure FDA0004879374960000011
    Figure FDA0004879374960000011
Patent Text Reader

Abstract

The invention provides a release agent for liquid die forging and a preparation method of the release agent. The release agent comprises the following components in percentage by mass: 6.4-19.7% of inorganic powder; 1.7%-6.7% of an organic lubricant; and 73.6%-90% of water. According to the release agent for liquid die forging, in a liquid die forging process, the fluidity of metal liquid can be effectively improved, casting defects are reduced, the yield of castings is improved, follow-up reprocessing production is not affected, and meanwhile the release agent has the advantages of being environmentally friendly, low in cost, simple in preparation method and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of release agents, and in particular to a release agent for liquid die forging and a preparation method thereof. Background Art

[0002] Liquid die forging refers to pouring a certain amount of liquid metal directly into an open metal mold, using a punch to act on the liquid metal with a certain pressure to fill, shape, crystallize and solidify it, and producing a certain amount of plastic deformation during the crystallization process.

[0003] In the liquid die forging process, since liquid metal has a good wetting effect on the metal mold, the surface of the mold cavity is washed by high-pressure, high-speed and high-temperature liquid metal during the die-casting process, making the liquid metal easily adhere to the surface of the cavity. In order to maintain the integrity and post-processing of metal die-casting products, while ensuring the quality of castings, the service life of die-casting molds and production efficiency, a release agent can be used to form a uniform release film on the surface of the die-casting mold, so that the metal die-casting product can be demolded from the mold and successfully removed from the mold. Currently, common release agents usually use a large amount of synthetic organic matter such as silicone oil, wax, mineral oil, etc., but a large amount of synthetic organic matter will increase the difficulty of cleaning and coating the casting in the later stage, and the organic matter has poor high temperature resistance. It is easy to decompose during use to produce carbon deposits and volatile substances, which has an adverse effect on the mechanical properties and molding quality of the casting, and there are great safety hazards in the casting process. Summary of the invention

[0004] In view of this, the present application provides a release agent for liquid die forging and a preparation method thereof. The release agent for liquid die forging uses water as a matrix, and is matched with an appropriate amount of inorganic powder and a small amount of organic lubricant. While ensuring the heat insulation and thermal insulation effect of the release agent, it increases the lubrication of the liquid metal, thereby promoting the fluidity of the liquid metal in the forging die. When performing the liquid die forging process, it can help to improve the air tightness and density of automotive functional parts with complex shapes and structures, reduce casting defects, and improve the casting yield without affecting subsequent reprocessing and production. In addition, the release agent also has the advantages of being green and environmentally friendly, low cost, and simple preparation method.

[0005] In a first aspect, the present application provides a release agent for liquid die forging, comprising the following components in percentage by mass:

[0006] Inorganic powder: 6.4%-19.7%;

[0007] Organic lubricant: 1.7%-6.7%;

[0008] Water: 73.6%-90%.

[0009] In an embodiment of the present application, the inorganic powder includes a first inorganic powder and a second inorganic powder; the first inorganic powder includes one or more of talc and boron nitride; the second inorganic powder includes one or more of diatomaceous earth, calcined kaolin, dolomite powder, aluminum-rich rustite powder, mullite powder and bauxite.

[0010] In an embodiment of the present application, the mass ratio of the first inorganic powder to the second inorganic powder in the liquid die forging release agent is (1-3):1.

[0011] In an embodiment of the present application, the organic lubricant includes one or more of alkylaryl modified polysiloxane, carnauba wax, polypropylene wax, high-density oxidized polyethylene wax, epoxy soybean oil and trimethylolpropane oleate.

[0012] In the embodiment of the present application, the chemical structure of the alkylaryl modified polysiloxane is shown in formula (I):

[0013]

[0014] Wherein, 120≤m≤150, 25≤n≤30, and m and n are integers;

[0015] R 1 is a C12-C18 alkyl group; R 2 It is an aromatic group.

[0016] In the implementation manner of the present application, the thermal conductivity of the inorganic powder is 0.15W / (m·℃)-3.8W / (m·℃).

[0017] In the embodiment of the present application, the D50 particle size of the inorganic powder is 1.5 μm-2.5 μm.

[0018] In the embodiment of the present application, the liquid die forging release agent further comprises an auxiliary agent, and the mass percentage of the auxiliary agent in the liquid die forging release agent is 1.5%-10%;

[0019] The auxiliary agent includes at least one component having the following mass percentage in the liquid die forging release agent:

[0020] Suspension: 0.5%-1.0%;

[0021] Binder: 0.01%-2.0%;

[0022] Rust inhibitor: 0.4%-2.0%;

[0023] Dispersant: 0.5%-1.5%;

[0024] Wetting agent: 0.01%-0.1%;

[0025] Silicone defoamer: 0.1%-0.3%;

[0026] Silicone leveling agent: 0.1%-0.3%.

[0027] In the embodiment of the present application, the suspending agent includes one or more of bentonite, attapulgite, rectorite clay, hydrophilic modified fumed silica and xanthan gum;

[0028] The binder includes one or more of styrene acrylic resin emulsion, phenolic resin, syrup, water glass, dextrin and polysaccharide compound;

[0029] The rust inhibitor comprises triethanolamine and an organic acid, wherein the organic acid comprises one or more of n-octanoic acid, neodecanoic acid and isononanoic acid;

[0030] The dispersant includes one or more of sodium hexametaphosphate, acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer and naphthalenesulfonate formic acid condensate sodium salt;

[0031] The wetting agent includes one or more of dioctyl sulfonated succinate sodium salt and isomeric decanol polyoxyethylene ether.

[0032] In the embodiment of the present application, the rotational viscosity of the liquid die forging release agent at 25°C is 2000mPa . s-3000mPa . s.

[0033] The second aspect of the present application further provides a method for preparing the release agent for liquid die forging provided in the first aspect, comprising:

[0034] The liquid die forging release agent is obtained by mixing the various components of the liquid die forging release agent.

[0035] The third aspect of the present application further provides an automobile structural part, which is prepared by using the liquid die forging release agent provided in the first aspect. DETAILED DESCRIPTION

[0036] The present application is further described in detail below in conjunction with preferred embodiments, but the protection scope of the present application is not limited to the following specific embodiments.

[0037] In the present application, all professional terms have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present application.

[0038] With the rapid development of the new energy automobile industry, the quality requirements for automobile functional parts are getting higher and higher. Since automobile functional parts usually need to withstand impact, high temperature, high pressure, high strength, and subsequent surface treatment and heat treatment such as anodizing and passivation, the metal needs to be crystallized and solidified under pressure to avoid casting defects such as pores, shrinkage and shrinkage. Therefore, advanced liquid die forging technology is favored. Liquid die forging castings have dense structure and higher mechanical properties than low-pressure castings.

[0039] Liquid die forging refers to pouring a certain amount of metal liquid directly into an open metal mold, and applying a certain pressure to the metal liquid through a punch to fill, form, crystallize and solidify it, and produce a certain amount of plastic deformation during the crystallization process. The process is stable in filling the mold, and the metal can be directly crystallized and solidified under pressure, so the casting has the advantages of no pores, no shrinkage holes and no shrinkage. Most of the die-casting molds in the liquid die forging process are made of H13 steel. Since liquid metal has a good wetting effect on H13 steel, the surface of the mold cavity is washed by high-pressure, high-speed and high-temperature liquid metal during the die-casting process, and the liquid metal is easy to adhere to the surface of the cavity. In order to maintain the integrity and post-processing of metal die-casting products, and at the same time ensure the quality of castings, the service life of die-casting molds and production efficiency, a release agent can be used to form a uniform release film on the surface of the die-casting mold, so that the metal die-casting product can be demolded from the mold and successfully removed from the mold.

[0040] At present, release agents must be used in the liquid die forging process of precision automotive functional parts such as steering knuckles, compressor brackets, engine brackets, suspension brackets, airbag support arms, battery compartment end plates, etc. Common release agents are usually mainly composed of organic high molecular polymers and inorganic powders such as graphite, but a large amount of high molecular polymers such as silicone oil will increase the difficulty of later cleaning and coating of castings, and the high temperature resistance of polymers is poor. During use, it is easy to decompose and produce carbon deposits and volatile substances, which have an adverse effect on the mechanical properties and surface quality of castings, and there are great safety hazards in the casting process. Graphite inorganic powders will also bring a lot of dust, which will pollute the production environment and may cause safety accidents such as dust explosions.

[0041] In response to the above problems, the present application provides a release agent for liquid die forging, which uses water as a matrix, and is matched with an appropriate amount of inorganic powder and a small amount of organic lubricant. While ensuring the heat insulation and thermal insulation effect of the release agent, it increases the lubrication of the liquid metal, thereby promoting the fluidity of the liquid metal in the forging die. When performing the liquid die forging process, the liquid die forging release agent can help improve the air tightness and density of functional parts with complex shapes and structures, while reducing casting defects of castings, improving the casting yield, and not affecting subsequent reprocessing and production. In addition, the liquid die forging release agent also has the advantages of being green and environmentally friendly, low cost, and simple preparation method.

[0042] The embodiment of the present application provides a release agent for liquid die forging, comprising the following components in percentage by weight:

[0043] Inorganic powder: 6.4%-19.7%;

[0044] Organic lubricant: 1.7%-6.7%;

[0045] Water: 73.6%-90%.

[0046] The release agent for liquid die forging of the present application uses water as the matrix, which can effectively avoid the adverse effects of carbon deposits on the performance of castings caused by high-temperature decomposition caused by the prior art using a large amount of oily organic matter as the matrix, as well as the safety hazards caused by volatile flammable substances. Considering the molding method of the liquid die forging process and the high precision requirements for castings, the liquid die forging process is longer than the conventional low-pressure die casting molding process, and the metal liquid flows slower. Therefore, the release agent provided by the present application is used for a specific liquid die forging process, in which a large amount of water and inorganic powder provide good thermal insulation effects, making the metal liquid difficult to solidify, which is more conducive to the molding of castings, and the addition of a small amount of organic lubricant can further enhance the fluidity of the metal liquid, thereby obtaining a precision casting functional part with a complex shape and structure and good air tightness, compactness and yield. In some embodiments of the present application, water includes but is not limited to deionized water.

[0047] In the implementation manner of the present application, the mass percentage of inorganic powder in the release agent for liquid die forging is 6.4%-19.7%. In some specific implementations, the mass percentage of inorganic powder in the release agent for liquid die forging can be, for example, 6.4%, 6.5%, 6.6%, 6.8%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 19.5%, 19.7%. The present application controls the content of the release agent for liquid die forging within the above-mentioned appropriate range. On the one hand, the good thermal insulation effect provided by the inorganic powder with good thermal insulation performance can prevent the high-temperature molten metal liquid from cooling prematurely, resulting in insufficient filling of the casting to form defective parts or produce defects such as cold shut, thereby affecting the performance of the casting. On the other hand, inorganic powders can also play a role in high-temperature crack prevention and pore elimination during the liquid die forging process, thereby further improving the air tightness and density of the casting and improving the yield of the preparation.

[0048] In the embodiment of the present application, the inorganic powder includes a first inorganic powder and a second inorganic powder, wherein the first inorganic powder includes one or more of talc and boron nitride; the second inorganic powder includes one or more of diatomaceous earth, calcined kaolin, dolomite powder, alumina-rich mullite powder, mullite powder and bauxite. The inorganic powder in the liquid die forging release agent provided in the present application includes a first inorganic powder and a second inorganic powder, the first inorganic powder is mainly used to form an isolation coating to isolate the mold and the metal liquid, and the second inorganic powder mainly plays a role in adjusting the thermal conductivity of the liquid die forging release agent, so that the release agent coating plays a role of thermal insulation during the high-temperature liquid die forging process, improves the fluidity of the metal liquid, and promotes the molding of the casting.

[0049] In some embodiments of the present application, the first inorganic powder includes talcum powder. The volume expansion coefficient of talcum powder is very small. Adding a certain amount of talcum powder to the release agent can effectively improve the high-temperature crack resistance and mechanical strength of the release agent coating, and avoid the problem that it is difficult to demold due to rupture caused by excessive temperature and the high-temperature molten metal directly contacts the mold surface. In addition, talcum powder can also further reduce the sintering temperature of the release agent coating. In some embodiments of the present application, by selecting talcum powder as the first inorganic powder, the mechanical properties and yield rate of liquid die forging products can be further improved.

[0050] In some specific embodiments of the present application, the second inorganic powder includes diatomaceous earth. Diatomaceous earth has excellent thermal insulation properties. Adding an appropriate amount of diatomaceous earth to the release agent can effectively adjust the thermal conductivity of the release agent coating, thereby making it have good thermal insulation properties, improving the fluidity of liquid metal, and avoiding the rapid heat loss of high-temperature liquid metal during liquid die forging, thereby preventing the molten metal from cooling prematurely, resulting in incomplete filling of the molten metal in the mold, thereby causing defects such as incomplete castings or cold shuts, thereby affecting the mechanical properties of the product. Cold shut defects refer to the fact that after the molten metal is filled into the mold, the fusion at the junction of the molten metal is not good, resulting in penetrating or non-penetrating gaps in the casting. In other embodiments of the present application, the second inorganic powder includes calcined kaolin. After calcination, the crystal structure and chemical activity of kaolin change, and the content of crystal water and combined water decreases, which increases its porosity. While the physical and chemical properties are more stable, the stress absorption capacity is also improved. Adding calcined kaolin with good high-temperature performance to the release agent for liquid die forging can effectively avoid thermal cracking of the release agent coating during the high-temperature extrusion stage. At the same time, the structure with a larger porosity also effectively eliminates pores, further improving the density and yield of the product.

[0051] In some embodiments of the present application, the inorganic powder has two or more material types, wherein the first inorganic powder has one or more material types, and the second inorganic powder has one or more material types. In some embodiments of the present application, the inorganic powder includes inorganic powders with two or more different D50 particle sizes. The inorganic powder mixture obtained by compounding different types of inorganic powders or inorganic powders of the same type but different particle sizes can form a maximum density accumulation of inorganic powder mixtures of different sizes, thereby further improving the density of the release agent coating, increasing its wear resistance and thus increasing its service life.

[0052] In an embodiment of the present application, the mass ratio of the first inorganic powder to the second inorganic powder in the release agent for liquid die forging is (1-3):1. In some specific embodiments, the mass ratio of the first inorganic powder to the second inorganic powder in the release agent for liquid die forging can be, for example, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1. The present application can further make the release agent for liquid die forging have both good isolation effect and suitable thermal conductivity by reasonably regulating the mass ratio of the first inorganic powder and the second inorganic powder and controlling the content of the first inorganic powder to be slightly larger than the content of the second inorganic powder.

[0053] In the implementation manner of the present application, the thermal conductivity of the inorganic powder is 0.15W / (m0℃)-3.8W / (m0℃). In some specific implementation manners of the present application, the thermal conductivity of the inorganic powder can be, for example, 0.15W / (m0℃), 0.2W / (m0℃), 0.3W / (m0℃), 0.5W / (m0℃), 0.6W / (m0℃), 0.8W / (m0℃), 1W / (m0℃), 1.5W / (m0℃), 2W / (m0℃), 2.5W / (m0℃), 3W / (m0℃), 3.5W / (m0℃), 3.8W / (m0℃). The release agent for liquid die forging provided in the present application can further ensure the thermal insulation effect of the release agent coating during high-temperature liquid die forging by selecting inorganic powders with a thermal conductivity within the above range, thereby avoiding heat loss, further improving the fluidity of the metal liquid, and promoting casting molding.

[0054] In the implementation manner of the present application, the D50 particle size of the inorganic powder is 1.5μm-2.5μm. In some specific implementation manners of the present application, the D50 particle size of the inorganic powder can be, for example, 1.5μm, 1.6μm, 1.7, 1.8μm, 1.9μm, 2.0μm, 2.1μm, 2.2μm, 2.3μm, 2.4μm, 2.5μm. By selecting inorganic powders of suitable particle size, the coating formed by the release agent can be made denser, and the ability to withstand the scouring of high-temperature resistant metal liquid can be enhanced. At the same time, the thermal conductivity of the release agent for liquid die forging can also be optimized and adjusted.

[0055] In the implementation manner of the present application, the mass percentage of the organic lubricant in the release agent for liquid die forging is 1.7%-6.7%. In some specific implementation manners, the mass percentage of the inorganic powder in the release agent for liquid die forging can be, for example, 1.7%, 1.8%, 1.9%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 6.7%. The present application controls the content of the organic lubricant in the release agent for liquid die forging within the above-mentioned appropriate range, while ensuring that the organic lubricant can provide sufficient lubricity for the release agent coating, thereby ensuring that the metal liquid has sufficient fluidity for filling and molding, while avoiding the problems of excessive organic lubricant causing carbon deposits or reducing the thermal insulation effect of the release agent coating, thereby improving the surface finish of the casting and the molding rate of the casting.

[0056] In the embodiment of the present application, the organic lubricant includes one or more of alkylaryl modified polysiloxane, carnauba wax, polypropylene wax, high density oxidized polyethylene wax, epoxy soybean oil and trimethylolpropane oleate.

[0057] In some embodiments of the present application, the organic lubricant includes alkyl aryl modified polysiloxane and organic wax, as well as one or more of epoxy soybean oil and trimethylolpropane oleate. In the embodiments of the present application, the organic wax includes one or more of carnauba wax, polypropylene wax and high-density oxidized polyethylene wax. The addition of a small amount of alkyl aryl modified polysiloxane and organic wax can further enhance the lubrication effect of the metal liquid and the film-forming effect of the release agent coating while ensuring that it does not affect the thermal insulation effect of the release agent for liquid die forging, thereby further improving the surface quality of the casting. Different types of organic lubricants have different lubrication time. Adding two or more organic lubricants can provide lubrication at different temperature periods, so that the metal liquid maintains good fluidity throughout the liquid die forging process. Organic waxes such as carnauba wax, polypropylene wax and high-density polyethylene wax, as well as organic lubricants such as epoxy soybean oil and trimethylolpropane oleate can provide good lubricity in the low temperature section. As the temperature further increases, organic lubricants such as organic waxes are carbonized, and at this time, alkyl aryl modified polysiloxanes play their lubricating role. Therefore, the combination of alkylaryl-modified polysiloxane and organic wax can ensure good lubrication of the metal during the entire liquid die forging process and promote its flow forming.

[0058] In the embodiment of the present application, the chemical structure of the alkylaryl-modified polysiloxane is shown in formula (I):

[0059]

[0060] Wherein, 120≤m≤150, 25≤n≤30, and m and n are integers;

[0061] R 1 is a C12-C18 alkyl group; R 2 It is an aromatic group.

[0062] In some embodiments of the present application, the value of m may be, for example, 120, 125, 130, 135, 140, 145, 150, and the value of n may be, for example, 25, 26, 27, 28, 29, 30. In some embodiments of the present application, R 1 is a C12-C18 alkyl radical. 1 For example, it can be -C 12 H 25 , -C 14 H 29 , R 2 For example, it can be -CH 2 CHCH 3 Ph.

[0063] In the embodiment of the present application, the rotational viscosity of the alkylaryl modified polysiloxane at 25°C is 1050mPa.s-1500mPa.s . In some specific embodiments of the present application, the rotational viscosity of the alkylaryl-modified polysiloxane at 25° C. may be, for example, 1050 mPa. . s, 1100mPa . s, 1150mPa . s, 1200mPa . s, 1250mPa . s, 1300mPa . s、1350mPa . s、1400mPa . s, 1450mPa . s、1500mPa . s, and the rotational viscosity is tested by a rotational viscometer (such as NDJ-8S rotational viscometer). The present application can further control the viscosity of the release agent for liquid die forging by selecting an alkylaryl-modified polysiloxane with a suitable viscosity as an organic lubricant, thereby facilitating the subsequent coating of the release agent and increasing the bonding force between the release agent coating and the mold.

[0064] In the embodiment of the present application, the mass percentage of the auxiliary agent in the liquid die forging release agent is 1.5%-10%. In some specific embodiments, the mass percentage of the auxiliary agent in the liquid die forging release agent can be, for example, 1.5%, 1.6%, 1.62%, 1.7%, 1.8%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.

[0065] In the embodiment of the present application, at least one of the auxiliary agent packages is a component having the following mass percentage in the liquid die forging release agent:

[0066] Suspension: 0.5%-1.0%;

[0067] Binder: 0.01%-2.0%;

[0068] Rust inhibitor: 0.4%-2.0%;

[0069] Dispersant: 0.5%-1.5%;

[0070] Wetting agent: 0.01%-0.1%;

[0071] Silicone defoamer: 0.1%-0.3%;

[0072] Silicone leveling agent: 0.1%-0.3%.

[0073] In the implementation manner of the present application, the mass percentage of the suspending agent in the release agent for liquid die forging is 0.5%-1.0%. In some specific implementation manners of the present application, the mass percentage of the suspending agent in the release agent for liquid die forging can be, for example, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1.0%. In the implementation manner of the present application, the suspending agent includes one or more of bentonite, attapulgite, rectorite clay, hydrophilic modified fumed silica and xanthan gum. The present application selects suitable suspending agents, which have a high specific surface area. By further controlling the amount of addition, the suspending property of the release agent can be effectively improved, which plays a role of suspension thickening, so that the uniformity of the product is better.

[0074] In the implementation manner of the present application, the mass percentage of the binder in the release agent for liquid die forging is 0.01%-2.0%. In some specific implementation manners of the present application, the mass percentage of the binder in the release agent for liquid die forging can be, for example, 0.01%, 0.02%, 0.05%, 0.1%, 0.2%, 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.5%, 1.6%, 1.8%, 2.0%. In the implementation manner of the present application, the binder includes one or more of styrene acrylic resin emulsion, phenolic resin, syrup, water glass, dextrin and polysaccharide compounds. The present application adds a suitable binder to the release agent for liquid die forging, which can further increase the adhesion of the release agent coating to the mold, and improve its tear resistance and resistance to metal liquid scouring.

[0075] In an embodiment of the present application, the mass percentage of the rust inhibitor in the release agent for liquid die forging is 0.4%-2.0%. In some specific embodiments of the present application, the mass percentage of the rust inhibitor in the release agent for liquid die forging can be, for example, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%. In an embodiment of the present application, the rust inhibitor includes triethanolamine and an organic acid, and the organic acid includes one or more of octanoic acid, neodecanoic acid and isononanoic acid. The present application enhances the rust prevention ability of the release agent for liquid die forging by selecting an organic base triethanolamine and compounding it with an organic acid for synergistic rust prevention.

[0076] In the implementation manner of the present application, the mass percentage of the dispersant in the release agent for liquid die forging is 0.5%-1.5%. In some specific implementation manners of the present application, the mass percentage of the dispersant in the release agent for liquid die forging can be, for example, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%. In the implementation manner of the present application, the dispersant includes one or more of sodium hexametaphosphate, acrylic acid-2-acrylamide-2-methylpropane sulfonic acid copolymer and naphthalenesulfonate formaldehyde condensate sodium salt. Selecting the above-mentioned suitable dispersant and controlling its content in the release agent for liquid die forging can effectively disperse the various components in the release agent for liquid die forging, thereby obtaining a release agent with uniform components and uniform performance.

[0077] In the implementation manner of the present application, the mass percentage of the wetting agent in the release agent for liquid die forging is 0.01%-0.1%. In some specific implementation manners of the present application, the mass percentage of the wetting agent in the release agent for liquid die forging can be, for example, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%. In the implementation manner of the present application, the wetting agent includes one or more of sodium salt of dioctyl sulfonate succinate and isomeric decanol polyoxyethylene ether. The wetting agent can further improve the wettability of the release agent coating for liquid die forging to the metal liquid, thereby further improving its fluidity during the liquid die forging process.

[0078] In the embodiment of the present application, the mass percentage of the organosilicon defoamer in the release agent for liquid die forging is 0.1%-0.3%. In some specific embodiments, the mass percentage of the organosilicon defoamer in the release agent for liquid die forging can be, for example, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%. The organosilicon defoamer can eliminate the foam generated during the preparation process of the release agent system, so that the inorganic powder in the release agent is more evenly dispersed.

[0079] In the embodiment of the present application, the mass percentage of the organic silicon leveling agent in the liquid die forging release agent is 0.1%-0.3%. In some specific embodiments, the mass percentage of the organic silicon leveling agent in the liquid die forging release agent can be, for example, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%. The addition of the organic silicon leveling agent can make the liquid die forging release agent form a film more flat, smooth, and uniform in the mold.

[0080] In the embodiment of the present application, the rotational viscosity of the liquid die forging release agent at 25°C is 2000 mPa . s-3000mPa .In some embodiments of the present application, the rotational viscosity of the liquid die forging release agent at 25° C. may be, for example, 2000 mPa. . s, 2100mPa . s、2200mPa . s, 2300mPa . s、2400mPa . s、2500mPa . s、2600mPa . s, 2700mPa . s、2800mPa . s, 2900mPa . s、3000mPa . s. The present application controls the viscosity of the release agent for liquid die forging within the above range, which can further promote its subsequent coating in the forging die and effectively improve the bonding force between the release agent coating and the die, facilitate the subsequent demolding of the casting and improve the surface quality of the casting.

[0081] The liquid die forging release agent provided in the present application has good thermal insulation performance, high temperature stability and stress absorption capacity, which can effectively ensure the fluidity of liquid metal in the liquid die forging process, thereby ensuring the dimensional accuracy and mechanical properties of liquid die forged alloy products. In addition, the liquid die forging release agent is green and environmentally friendly, low in cost, and simple in preparation method.

[0082] The present application also provides a method for preparing the release agent for liquid die forging provided above, comprising:

[0083] The liquid die forging release agent is obtained by mixing the various components of the liquid die forging release agent.

[0084] In some embodiments of the present application, the auxiliary agent includes a suspending agent, a binder, a rust inhibitor, a dispersant and a wetting agent, and the raw material mixing process includes: first adding the suspending agent, the rust inhibitor, the dispersant and the wetting agent to deionized water for a first stirring treatment, adding an organosilicon defoamer to eliminate the foam in the mixed slurry, and then adding an inorganic powder, an organic lubricant and a binder for a second stirring treatment and then grinding and dispersing treatment to obtain a liquid die forging release agent with a D50 particle size of 1.5μm-2.5μm (the particle size is tested using an OMEC TOPsizer Plus laser particle size analyzer). In some other embodiments of the present application, the suspending agent is added to deionized water and finally added to the mixed slurry of the liquid die forging release agent to play the role of a thickener, further enhancing the viscosity of the liquid die forging release agent.

[0085] In some embodiments of the present application, the first stirring process and the second stirring process adopt a high-speed disperser. In some embodiments of the present application, the speed of the first stirring process is 600r / min-800r / min, and the time is 30min-40min. In some specific embodiments, the speed of the first stirring process can be, for example, 600r / min, 650r / min, 700r / min, 750r / min, 800r / min, and the time can be, for example, 30min, 32min, 34min, 35min, 36min, 38min, 40min. In some embodiments of the present application, the speed of the second stirring process is 2500r / min-4000r / min, and the time is 40min-50min. In some specific embodiments, the speed of the second stirring process can be, for example, 2500r / min, 2800r / min, 3000r / min, 3200r / min, 3500r / min, 3600r / min, 3800r / min, 4000r / min, and the time can be, for example, 40min, 42min, 44min, 45min, 46min, 48min, 50min. In some embodiments of the present application, the flow rate of the grinding and dispersing process is 6L / min-8L / min. In some specific embodiments, the flow rate of the grinding and dispersing process can be 6L / min, 6.5L / min, 7L / min, 7.5L / min, 8L / min.

[0086] The present application also provides an automobile structural part, the preparation of which adopts the liquid die forging release agent provided in the foregoing text. In the embodiment of the present application, the automobile structural part is made by liquid die forging, and the liquid die forging release agent provided in the foregoing text of the present application is used in the liquid die forging process. In the embodiment of the present application, the automobile structural part is a common structural part and functional part in the automobile, including but not limited to a steering knuckle, a compressor bracket, an engine bracket, a suspension bracket, an airbag support arm, a battery compartment end plate, etc. In some specific embodiments, the material of the automobile structural part can be, for example, an aluminum alloy, and the aluminum alloy can be, for example, an Al-Si series aluminum alloy, an Al-Mg series aluminum alloy, an Al-Zn series aluminum alloy, etc., wherein the Al-Si series aluminum alloy includes, but is not limited to, an Al-Si aluminum alloy, an Al-Si-Cu aluminum alloy, an Al-Si-Mg aluminum alloy, an Al-Mg series aluminum alloy includes an Al-Mg aluminum alloy, an Al-Mg-Cu aluminum alloy, and an Al-Zn series includes an Al-Zn-Si aluminum alloy, an Al-Zn-Mg aluminum alloy, etc.

[0087] The present application is further described below in multiple embodiments:

[0088] Example 1

[0089] A release agent for liquid die forging is prepared from the following components in percentage by weight: 6% talc, 4% calcined kaolin, 2% diatomaceous earth, 1% alkylaryl modified polysiloxane emulsion, 4% carnauba wax emulsion, 0.5% hydrophilic modified fumed silica, 0.5% xanthan gum, 2% styrene acrylic resin emulsion, 1% triethanolamine, 0.5% n-octanoic acid, 0.5% neodecanoic acid, 0.5% acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer, 0.5% naphthalenesulfonate formic acid condensate sodium salt, 0.05% sulfonated dioctyl succinate sodium salt, 0.3% organic silicon leveling agent, 0.3% organic silicon defoaming agent, and the remaining components are deionized water. The corresponding preparation method is described in the following steps:

[0090] (1) adding triethanolamine, n-octanoic acid and neodecanoic acid to water in sequence, and then stirring for 0.5 hours to obtain a mixed solution;

[0091] (2) adding naphthalenesulfonate formic acid condensate sodium salt, silicone leveling agent, acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer, dioctyl sulfonated succinate sodium salt, and hydrophilic modified fumed silica to the mixed solution obtained in step (1), and dispersing the mixture uniformly by using a high-speed disperser for 15 minutes at a speed of 800 r / min. After the dispersion is completed, adding silicone defoamer;

[0092] (3) adding calcined kaolin, talc, diatomaceous earth, carnauba wax emulsion, alkylaryl modified polysiloxane emulsion, and styrene acrylic resin emulsion to the mixed solution treated in step (2) in sequence, and then stirring the mixture evenly in a high-speed disperser for 30 minutes at a speed of 4000 r / min;

[0093] (4) grinding and dispersing the material obtained in step (3) at a flow rate of 8 L / min until the particle size D50 is 1.5 μm to obtain a release agent slurry;

[0094] (5) Add the pre-dissolved xanthan gum solution to the slurry obtained in step (4), and then stir at a low speed to obtain a liquid die forging release agent.

[0095] Example 2

[0096] The difference from Example 1 is that the mass percentage of talc is 8% and the mass percentage of calcined kaolin is 4%.

[0097] Example 3

[0098] The difference from Example 1 is that the mass percentage of talc is 9% and the mass percentage of calcined kaolin is 3%.

[0099] Example 4

[0100] The difference from Example 1 is that the mass percentage of talc is 3.2% and the mass percentage of calcined kaolin is 3.2%.

[0101] Example 5

[0102] The difference from Example 1 is that it is made of the following components in weight percentage: 10% talc, 7.7% calcined kaolin, 2% diatomaceous earth, 1% alkylaryl modified polysiloxane emulsion, 1% carnauba wax emulsion, 0.5% hydrophilic modified fumed silica, 2% styrene acrylic resin emulsion, 0.5% triethanolamine, 0.25% n-octanoic acid, 0.25% neodecanoic acid, 0.5% acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer, 0.4% naphthalenesulfonate formic acid condensate sodium salt, 0.1% dioctyl sulfonated succinate sodium salt, 0.1% organosilicon leveling agent, 0.1% organosilicon defoaming agent, and the remaining components are deionized water.

[0103] Example 6

[0104] The difference from Example 1 is that the mass percentage content of the carnauba wax emulsion is 0.7%.

[0105] Example 7

[0106] The difference from Example 1 is that the mass percentage of the carnauba wax emulsion is 5.7%.

[0107] Example 8

[0108] The difference from Example 1 is that 6% of talc is replaced by 5% of talc and 1% of hexagonal boron nitride.

[0109] Example 9

[0110] The difference from Example 1 is that 6% of talc is replaced by 3% of talc and 3% of hexagonal boron nitride.

[0111] Example 10

[0112] The difference from Example 1 is that 1% of the alkylaryl-modified polysiloxane emulsion and 4% of the carnauba wax emulsion are replaced by 4% of the high-density oxidized polyethylene wax emulsion and 1% of the carnauba wax emulsion.

[0113] Embodiment 11

[0114] The difference from Example 1 is that 1% of the alkylaryl-modified polysiloxane emulsion and 4% of the carnauba wax emulsion are replaced by 1% of the high-density oxidized polyethylene wax emulsion and 4% of the polypropylene wax emulsion.

[0115] Comparative Example 1

[0116] The difference from Example 1 is that the mass percentage of the alkyl aryl modified polysiloxane emulsion is 10%.

[0117] Comparative Example 2

[0118] The difference from Example 1 is that there is no carnauba wax emulsion.

[0119] Comparative Example 3

[0120] The difference from Example 1 is that the mass percentage of talc is 1%, the mass percentage of calcined kaolin is 1%, and the mass percentage of diatomaceous earth is 1%.

[0121] Comparative Example 4

[0122] The difference from Example 1 is that the mass percentage of talc is 10%, the mass percentage of calcined kaolin is 10%, and the mass percentage of diatomaceous earth is 10%.

[0123] Comparative Example 5

[0124] A release agent for liquid die forging is prepared from the following components in percentage by weight: 65% of trimethylolpropane oleate, 15% of epoxy soybean oil, 18.0% of graphite, and 2% of alkylaryl modified polysiloxane. The corresponding preparation method is as follows:

[0125] Trimethylolpropane oleate, epoxy soybean oil, graphite, and alkyl aryl modified polysiloxane were added into a high-speed disperser and stirred evenly, wherein the speed of the high-speed disperser was 3000 r / min and the dispersion time was 30 minutes, to obtain a release agent for liquid die forging.

[0126] The liquid die forging release agents prepared in Examples 1 to 11 and Comparative Examples 1 to 5 were used in the liquid die forging process of castings. The materials and processes used in the castings were all the same. Then 60 pieces were randomly selected. Then, they were manually observed for sticking, cold shut, pores, water marks, and carbon deposition. Among them:

[0127] Sticking is when the liquid metal adheres to the mold surface, causing the metal to form an adherent layer on the mold wall instead of flowing and filling the mold shape securely.

[0128] Cold shut refers to the situation when liquid metal flows in the mold and fills the cavity. Due to the excessive cooling speed of the metal at the flow front, the metal front solidifies prematurely, forming a thin solid or semi-solid layer. When the subsequent liquid metal continues to flow and tries to fill the cavity, this solidified or semi-solidified metal layer will hinder the flow of the metal, thus forming a cold shut in the final product.

[0129] Porosity refers to the formation of cavities or gaps due to the retention of gas or the release of gas inside the metal during the solidification process of the metal;

[0130] Watermarks refer to the wavy texture that appears on the metal surface, similar to ripples on the water;

[0131] Carbon deposits refer to the formation of carbon deposits on the metal surface or inside. These deposits are usually formed by the reaction of hydrocarbons and lubricating grease at high temperatures.

[0132] The specific results are shown in Table 1:

[0133] Table 1

[0134] Performance Testing Mucous membranes Cold insulation Pores Water Ripple Carbon deposits Example 1 0 0 0 0 0 Example 2 0 3 0 0 0 Example 3 0 5 0 0 0 Example 4 3 4 1 0 0 Example 5 5 0 3 0 0 Example 6 9 0 0 0 0 Example 7 0 0 0 5 2 Example 8 0 4 0 0 0 Example 9 1 7 0 0 0 Example 10 5 0 0 2 1 Embodiment 11 4 0 0 2 1 Comparative Example 1 2 1 1 17 0 Comparative Example 2 28 1 0 0 0 Comparative Example 3 4 30 0 0 0 Comparative Example 4 20 0 15 0 0 Comparative Example 5 0 60 40 60 60

[0135] It can be seen from the data in Table 1 that, compared with the release agents for liquid die forging of Examples 1 to 11 of the present application, in Example 1, too much organic lubricant easily causes water marks and other phenomena to occur in the prepared castings; in Example 2, too little organic lubricant results in insufficient lubrication and is prone to problems with sticking films; in Example 3, the content of inorganic powder is too little, causing cold shut of the castings and easily leading to insufficient filling of the castings; in Example 4, the content of inorganic powder is too much, making it difficult for the release agent to form a continuous coating, and the castings are prone to problems such as sticking films and pores; the release agent of Example 5 adopts an oily system, and the castings produce a large number of defects such as cold shuts, pores, water marks, and carbon deposits.

[0136] The preferred embodiments are described in detail above, but the present invention is not limited to the above-mentioned specific implementation modes. Under the guidance of the present application, technicians in this field can also make various specific changes without departing from the scope of protection of the present application, which all fall within the scope of protection of the present invention.

Claims

1. A release agent for liquid die forging, characterized in that: The following components are included in the mass percentage: Inorganic powder: 6.4%-19.7%; Organic lubricant: 1.7%-6.7%; Water: 73.6%-90%.

2. The release agent for liquid die forging according to claim 1, characterized in that: The inorganic powder includes a first inorganic powder and a second inorganic powder; the first inorganic powder includes one or more of talc and boron nitride; the second inorganic powder includes one or more of diatomaceous earth, calcined kaolin, dolomite powder, alumina-rich rustite powder, mullite powder and bauxite.

3. The release agent for liquid die forging according to claim 2, characterized in that: The mass ratio of the first inorganic powder to the second inorganic powder in the liquid die forging release agent is (1-3):

1.

4. The liquid die forging release agent according to any one of claims 1 to 3, characterized in that: The organic lubricant includes one or more of alkylaryl modified polysiloxane, carnauba wax, polypropylene wax, high density oxidized polyethylene wax, epoxy soybean oil and trimethylolpropane oleate.

5. The release agent for liquid die forging according to claim 4, characterized in that: The chemical structure of the alkylaryl modified polysiloxane is shown in formula (I): Wherein, 120≤m≤150, 25≤n≤30, and m and n are integers; R1 is a C12-C18 alkyl group; R2 is an aromatic group.

6. The liquid die forging release agent according to any one of claims 1 to 5, characterized in that: The thermal conductivity of the inorganic powder is 0.1500 (m0°C)-3.800 (m0°C).

7. The liquid die forging release agent according to any one of claims 1 to 6, characterized in that: The D50 particle size of the inorganic powder is 1.5 μm-2.5 μm.

8. The release agent for liquid die forging according to any one of claims 1 to 7, characterized in that: The liquid die forging release agent further comprises an auxiliary agent, and the mass percentage of the auxiliary agent in the liquid die forging release agent is 1.5%-10%.

9. The release agent for liquid die forging according to claim 8, characterized in that: The auxiliary agent includes at least one component having the following mass percentage in the liquid die forging release agent: Suspension: 0.5%-1.0%; Binder: 0.01%-2.0%; Rust inhibitor: 0.4%-2.0%; Dispersant: 0.5%-1.5%; Wetting agent: 0.01%-0.1%; Silicone defoamer: 0.1%-0.3%; Silicone leveling agent: 0.1%-0.3%.

10. The release agent for liquid die forging according to claim 9, characterized in that: The suspending agent includes one or more of bentonite, attapulgite, rectorite clay, hydrophilic modified fumed silica and xanthan gum; The binder includes one or more of styrene acrylic resin emulsion, phenolic resin, syrup, water glass, dextrin and polysaccharide compound; The rust inhibitor comprises triethanolamine and an organic acid, wherein the organic acid comprises one or more of n-octanoic acid, neodecanoic acid and isononanoic acid; The dispersant includes one or more of sodium hexametaphosphate, acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer and naphthalenesulfonate formic acid condensate sodium salt; The wetting agent includes one or more of isomeric decanol polyoxyethylene ether, dioctyl sulfonate succinate sodium salt, and isomeric decanol polyoxyethylene ether.

11. The release agent for liquid die forging according to any one of claims 1 to 10, characterized in that: The liquid die forging release agent has a rotational viscosity of 2000 mPa at 25°C. . s-3000mPa . s.

12. A method for preparing a release agent for liquid die forging according to any one of claims 1 to 11, characterized in that: include: The liquid die forging release agent is obtained by mixing the various components of the liquid die forging release agent.

13. An automobile structural part, characterized in that: The automobile structural part is prepared by using the liquid die forging release agent as described in any one of claims 1 to 11.

Citation Information

Patent Citations

  • Non-graphite type lubricant for hot die forging of metal and preparation method of non-graphite type lubricant

    CN102533423A

  • Alloy material liquid forging release agent and preparing method thereof

    CN104226897A

  • High-property water-based metal die-casting releasing agent, preparation method and application of high-property water-based metal die-casting releasing agent

    CN107876692A

  • Copper alloy die-casting die lubricant as well as preparation and use methods thereof

    CN116496830A

  • Powdery lubricant for aluminum alloy forging

    GB9202254D0