Disilane-glycidyl azide polymer coated aluminum-lithium alloy powder as well as preparation method and application of disilane-glycidyl azide polymer coated aluminum-lithium alloy powder

By forming a double-layer coating on the surface of aluminum-lithium alloy powder, the problem of poor stability and compatibility of aluminum-lithium alloy powder is solved, and its combustion efficiency and energy performance in solid propellant are improved.

CN118808635APending Publication Date: 2024-10-22BEIJING INST OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410839906.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Aluminum-lithium alloy has problems of poor stability and poor compatibility with other components in solid propellants, which affects its combustion efficiency and storage stability.

Method used

By using epoxy silanes and fluorosilanes with epoxy groups to react with the surface of aluminum-lithium alloy powder to form Al-O-Si bonds, and performing a ring-opening addition reaction with glycidyl azide (GAP), the structure Double-layer coating improves the stability and energy performance of aluminum-lithium alloy powder.

Benefits of technology

The storage stability and energy performance of aluminum-lithium alloy powder are significantly improved, the compatibility with other propellant components is enhanced, and the combustion calorific value and combustion efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808635A_ABST
    Figure CN118808635A_ABST
Patent Text Reader

Abstract

The invention relates to disilane-glycidyl azide polymer coated aluminum-lithium alloy powder as well as a preparation method and application thereof, and belongs to the technical field of energetic materials. Epoxy silane with epoxy groups and fluorosilane with the fluorine atom number larger than or equal to 9 are subjected to dehydration condensation with the surface of the alloy powder to form Al-O-Si bonds, the Si-O-Si bonds are formed through condensation polymerization between the two kinds of silane, a layer of compact coating film can be formed on the surface of the alloy powder, the storage stability of the alloy powder is improved, and meanwhile the service life of the alloy powder is prolonged. According to the present invention, the polyazide glycidyl ether and the epoxy silane are subjected to the ring-opening addition reaction so as to construct the second coating film structure, such that the energy performance of the alloy powder is significantly improved. And the coated aluminum-lithium alloy powder has good stability, hydrophobicity and relatively high energy level, and can be used as a metal fuel in a solid propellant, so that the energy release performance and the combustion performance of the propellant are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder, a preparation method and application thereof, and belongs to the technical field of energetic materials. Background Art

[0002] As an important component of solid propellant, metal fuel can play a role in improving energy levels. Compared with the widely used metal fuel aluminum powder, aluminum-lithium alloy has higher combustion calorific value and energy level while maintaining the advantages of pure aluminum powder such as low toxicity, low oxygen consumption, and low price. Its "micro-explosion effect" during the combustion process can effectively inhibit the combustion and agglomeration of aluminum powder. At the same time, aluminum-lithium alloy can effectively reduce the release of HCl gas during the combustion of solid propellant. However, due to the presence of active metallic lithium, aluminum-lithium alloy has disadvantages such as poor stability and poor compatibility with other components of the propellant.

[0003] In order to improve the storage stability and combustion efficiency of aluminum-lithium alloys and solve the problem of poor compatibility with other components of propellants, researchers usually use surface coating to modify aluminum-lithium alloy powders. The thermal decomposition products of the fluoride coating can undergo a pre-ignition reaction with the aluminum oxide on the surface of the aluminum-lithium alloy powder, which is beneficial to reduce agglomeration and improve combustion efficiency; the thermite coating relies on the replacement reaction with aluminum, which is beneficial to reduce ignition delay and increase heat release; the organic coating can greatly improve storage stability by chemically bonding with the surface of the aluminum-lithium alloy. Since the coating itself does not contain energy, coating the aluminum-lithium alloy powder alone will reduce the energy of the entire system to a certain extent, so the design of the coating component still needs to be further improved. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder, a preparation method and its application. Through the dehydration condensation of epoxysilane with epoxy groups and fluorosilane with fluorine atoms ≥ 9 with the surface of the alloy powder to form Al-O-Si bonds, and the Si-O-Si bonds formed by the polycondensation reaction between the two silanes, a dense coating film can be formed on the surface of the alloy powder, while improving the storage stability of the alloy powder, it also gives it a certain modifiable function, and then through the ring-opening addition reaction between polyazide glycidyl ether and epoxysilane, a second layer of coating film structure is constructed, which significantly improves the energy performance of the alloy powder. The coated aluminum-lithium alloy powder has good stability, hydrophobicity and high energy level, and can be used as a metal fuel in solid propellants to improve the energy release performance and combustion performance of the propellant.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows.

[0006] A disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder, wherein the coating on the surface of the aluminum-lithium alloy powder is fluorosilane with fluorine atoms ≥9, epoxysilane and polyazide glycidyl ether (GAP), hydroxyl groups formed after hydrolysis of fluorosilane and free hydroxyl groups on the surface of the aluminum-lithium alloy powder undergo dehydration condensation to form Al-O-Si bonds, and van der Waals forces are formed between F atoms and Al, so that the fluorosilane is coated on the surface of the aluminum-lithium alloy powder; epoxysilane is connected to the aluminum-lithium alloy powder through Al-O-Si bonds, and fluorosilane and epoxysilane are polycondensed to form Si-O-Si bonds to tightly coat the surface of the aluminum-lithium alloy powder; GAP is grafted on the outermost layer through ring-opening addition of terminal hydroxyl groups and epoxy groups on epoxysilane, and finally an aluminum-lithium alloy powder with a double coating layer is formed.

[0007] Preferably, the fluorosilane is one or more of perfluorodecyltrimethoxysilane, perfluorooctyltrichlorosilane, perfluorohexyltrichlorosilane, perfluorooctylmethyldimethoxysilane and nonafluorohexyltrimethoxysilane.

[0008] Preferably, the epoxysilane is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0009] Preferably, the molecular weight of the GAP is 800-1400.

[0010] Preferably, the mass fraction of aluminum in the aluminum-lithium alloy powder is 90% to 98%.

[0011] Preferably, the particle size of the aluminum-lithium alloy powder is 5 μm to 50 μm.

[0012] A method for preparing the disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder according to the present invention comprises the following steps:

[0013] (1) dissolving a fluorosilane having a fluorine atom number of ≥9 in a second organic solvent to obtain a solution A, and dissolving an epoxysilane in a first organic solvent to obtain a solution B;

[0014] (2) adding the aluminum-lithium alloy powder to the third organic solvent, stirring and dispersing the powder evenly, adding solution A, stirring and reacting for 10 to 30 minutes, adding solution B, continuing to stir and react for 1 to 1.5 hours, and after the stirring is completed, filtering, washing, and drying to obtain a disilane-coated alloy powder;

[0015] (3) adding the alloy powder coated with disilane into a fourth organic solvent, then adding GAP and a catalyst, stirring the reaction for 2 to 3 hours, separating the solid and liquid after the stirring, and drying to obtain an aluminum-lithium alloy powder coated with disilane-polyazide glycidyl ether.

[0016] Preferably, the first organic solvent, the second organic solvent and the third organic solvent are ethyl acetate, n-hexane, acetone or dichloromethane respectively.

[0017] Preferably, the third organic solvent is ethyl acetate, dichloromethane, tetrahydrofuran or N,N-dimethylformamide.

[0018] Preferably, the catalyst is boron trifluoride etherate, triethylamine or bismuth trichloride.

[0019] Preferably, the amount of fluorosilane is 10% to 15% of the mass of the aluminum-lithium alloy powder, the amount of epoxysilane is 15% to 20% of the mass of the aluminum-lithium alloy powder, and the amount of GAP is 10% to 15% of the mass of the aluminum-lithium alloy powder.

[0020] Preferably, the usage ratio of the aluminum-lithium alloy powder, the fourth organic solvent and the catalyst is 1 g: 20-30 mL: 0.2-0.5 mL.

[0021] An application of the disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder described in the present invention, which is used as a metal fuel for solid propellant.

[0022] Preferably, the binder of the solid propellant is hydroxyl-terminated polybutadiene.

[0023] Beneficial Effects

[0024] (1) The present invention provides a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder, wherein fluorosilane and epoxysilane with a specific number of fluorine atoms are introduced into the aluminum-lithium alloy powder system, forming a dense coating film on the surface of the alloy powder, thereby improving the storage stability of the alloy powder; fluorosilane can react with aluminum lithium and aluminum oxide to cause a pre-ignition reaction in the alloy powder, thereby reducing the ignition temperature of the alloy powder and the agglomeration between particles, thereby increasing the combustion efficiency; the introduction of epoxy groups in epoxysilane also gives it a certain modifiable function; GAP compensates for the effect of the first coating layer itself containing no energy on the system energy reduction, thereby giving the alloy powder a higher energy level.

[0025] (2) The present invention provides a method for preparing aluminum-lithium alloy powder coated with disilane-polyazide glycidyl ether, wherein two silanes are coated on the surface of the alloy powder through chemical reaction with the alloy powder and polymerization reaction between the silanes to form a first coating film, and GAP is chemically grafted with a silane auxiliary agent to construct a second coating film structure. The order of addition, dosage ratio and reaction time of the two silanes have a great influence on the formation of the first coating layer.

[0026] (3) The present invention provides an application of aluminum-lithium alloy powder coated with disilane-polyazide glycidyl ether. The combustion heat of the alloy powder after two coating treatments is significantly increased compared with the original powder. At the same time, the formation of a dense coating layer not only improves the stability of the alloy powder, but also increases the compatibility between the alloy powder and other components in the propellant. In addition, the introduction of GAP also improves the energy level and combustion performance of the propellant. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 1 and 2. The X-ray photoelectron spectroscopy (XPS) curves of the coated aluminum-lithium alloy powder (Al-4.7Li@FSG) and the original aluminum-lithium alloy powder (Al-4.7Li) in Example 1.

[0028] Figure 2 This is a comparison of scanning electron microscope photos of the coated aluminum-lithium alloy powder (right) and the original aluminum-lithium alloy powder (left) in Example 1.

[0029] Figure 3 This is a comparison chart of the stability of the coated aluminum-lithium alloy powder (right) and the original aluminum-lithium alloy powder (left) in the liquid phase in Example 1.

[0030] Figure 4 This is the EDS nitrogen element distribution diagram of the coated aluminum-lithium alloy powder in Example 1. DETAILED DESCRIPTION

[0031] The present invention will be further described in detail below in conjunction with specific embodiments.

[0032] Example 1

[0033] Dissolve 0.15g 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 0.15g perfluorodecyltrimethoxysilane in 5mL ethyl acetate, stir for 5min to make them uniformly dispersed, and obtain epoxysilane solution and fluorosilane solution respectively; add 1g aluminum-lithium alloy powder Al-4.7Li (lithium content is 4.7%, particle size is 50μm) into 20mL ethyl acetate to prepare alloy powder suspension. First add fluorosilane solution to the obtained suspension and stir for 15min; then add epoxysilane solution to the system and stir for 1h; after the reaction is completed, separate the solid and liquid, dry the solid at 70℃ with forced air for 8h, and store it under vacuum for use, and obtain aluminum-lithium alloy powder Al-4.7Li@FS coated with double silane. The powder obtained above was added into ethyl acetate and stirred for 10 min to make it evenly dispersed. 0.1 g GAP and 0.2 mL boron trifluoride ether were added in sequence and stirred for 3 h. After the reaction, the mixture was centrifuged, washed and dried to obtain aluminum-lithium alloy powder Al-4.7Li@FSG coated with polysilane-polyazide glycidyl ether.

[0034] XPS test was performed on the aluminum-lithium alloy powder Al-4.7Li and the aluminum-lithium alloy powder Al-4.7Li@FSG coated in Example 1. The results are as follows: Figure 1 As shown, compared with the original alloy powder, the coated aluminum-lithium alloy powder has new peaks at 400eV, 689eV and 833eV, which belong to N1s, F 1s and F Auger, respectively, proving the presence of nitrogen and fluorine in the coating layer. This shows that this embodiment successfully achieves the coating of aluminum-lithium alloy powder with perfluorodecyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane and GAP.

[0035] Scanning electron microscope-energy spectrum test was performed on the aluminum-lithium alloy original powder Al-4.7Li and the aluminum-lithium alloy powder Al-4.7Li@FSG coated in Example 1, and it was found that Si, F, and N elements were distributed on the surface of the alloy powder; Figure 2 The scanning electron microscope results show that the original powder surface is rough and has many granular protrusions, while after coating, the alloy powder surface is relatively smooth, the granular protrusions disappear, and the coating layer is relatively dense. This also shows that the alloy powder has been successfully coated and the passivation of the powder has been effectively achieved, making the alloy powder have a certain stability.

[0036] In order to verify that the coated aluminum-lithium alloy powder Al-4.7Li@FSG prepared in this example has good stability, the aluminum-lithium original powder Al-4.7Li and the coated aluminum-lithium alloy powder Al-4.7Li@FSG in Example 1 were placed in water for comparison. Figure 3 As shown, the aluminum-lithium raw powder reacts violently in 25°C water (left picture), and the coated alloy powder can stably exist in 25°C water (right picture) and float on the water surface. This shows that the stability of the alloy powder prepared in this embodiment has been greatly improved and has a certain hydrophobicity.

[0037] In order to confirm that the aluminum-lithium alloy powder coated with disilane-polyazide glycidyl ether prepared in this embodiment has a high heat of combustion, oxygen bomb calorimetry tests were performed on Al-4.7Li, Al-4.7Li@FS and Al-4.7Li@FSG, and the heat of combustion results are shown in Table 1. The heat of combustion value of Al-4.7Li@FS is reduced because the first layer of silane structure coated is energy-free, and its addition will inevitably lead to a decrease in the heat of combustion value of the entire system. For Al-4.7Li@FS, compared with Al-4.7Li and Al-4.7Li@FS, its heat of combustion increased by 3.1% and 4.8%, respectively, which shows that the introduction of GAP increases the energy of the system and enables the alloy powder to have an excellent energy release level.

[0038] Table 1

[0039]

[0040] Example 2

[0041] 0.2g 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 0.1g perfluorodecyltrimethoxysilane were dissolved in 5mL ethyl acetate, stirred for 5min to make them uniformly dispersed, and epoxysilane solution and fluorosilane solution were obtained respectively; 1g aluminum-lithium alloy powder (lithium content of 4.7%, particle size of 50μm) was added to 20mL ethyl acetate to prepare alloy powder suspension. First, fluorosilane solution was added to the obtained suspension and stirred for 15min; then epoxysilane solution was added to the system and stirred for 1h; after the reaction, solid-liquid separation was performed, and the solid was dried at 70℃ for 8h, and stored under vacuum conditions for standby use to obtain aluminum-lithium alloy powder coated with silane. The above-obtained powder was added to ethyl acetate, stirred for 10min to make it uniformly dispersed, 0.1g GAP and 0.2mL boron trifluoride ether were added in sequence, and the reaction was stirred for 3h. After the reaction, it was centrifuged, washed and dried to obtain aluminum-lithium alloy powder coated with silane-polyazide glycidyl ether.

[0042] The aluminum-lithium alloy powder coated in this embodiment was subjected to XPS testing. The results showed that the coated aluminum-lithium alloy powder had N1s, F 1s and F Auger peaks at 400eV, 689eV and 833eV, respectively, indicating that this embodiment successfully achieved the coating of aluminum-lithium alloy powder with perfluorodecyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane and GAP.

[0043] The aluminum-lithium alloy powder after coating in this embodiment was subjected to scanning electron microscopy-energy spectrum test, and it was found that Si, F, and N elements were distributed on the surface of the alloy powder; and the scanning electron microscopy results showed that after coating, the surface of the alloy powder was relatively smooth, and the coating layer was relatively dense, which effectively achieved the passivation of the powder and made the alloy powder have a certain stability.

[0044] The disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder prepared in this embodiment has good stability, can stably exist in water at 25°C, float on the water surface, and has a certain hydrophobicity.

[0045] Comparative Example 1

[0046] Dissolve 0.15g 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 0.15g perfluorodecyltrimethoxysilane in 5mL ethyl acetate, stir for 5min to make them uniformly dispersed, and obtain epoxysilane solution and fluorosilane solution respectively; add 1g aluminum-lithium alloy powder (lithium content is 4.7%, particle size is 50μm) into 20mL ethyl acetate to prepare alloy powder suspension. First add epoxysilane solution to the obtained suspension and stir for 15min; then add fluorosilane solution to the system and stir for 1h; after the reaction is completed, separate the solid and liquid, dry the solid at 70℃ with air blast for 8h, and store it under vacuum conditions for standby use to obtain aluminum-lithium alloy powder coated with double silane. Add the above-obtained powder to ethyl acetate, stir for 10min to make it uniformly dispersed, add 0.1g GAP and 0.2mL boron trifluoride etherate in turn, continue stirring and reacting for 3h, centrifuge, wash and dry after completion to obtain coated aluminum-lithium alloy powder.

[0047] The XPS test was performed on the coated aluminum-lithium alloy powder of this comparative example. The results showed that the coated aluminum-lithium alloy powder had F1s and F Auger peaks, but the N1s peak was not obvious, indicating that the order of silane addition has a certain influence on the formation of the coating layer. The first addition of fluorosilane can more effectively coat the epoxy silane on the surface of the alloy powder.

[0048] The aluminum-lithium alloy powder after coating in this comparative example was subjected to scanning electron microscopy-energy spectrum testing, and it was found that Si and F elements were distributed on the surface of the alloy powder, but N element was less and unevenly distributed; and the scanning electron microscopy results showed that after coating, the coating layer was not as dense as Examples 1 and 2.

[0049] Comparative Example 2

[0050] 0.1g 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 0.2g perfluorodecyltrimethoxysilane were dissolved in 5mL ethyl acetate, stirred for 5min to make them uniformly dispersed, and epoxysilane solution and fluorosilane solution were obtained respectively; 1g aluminum-lithium alloy powder (lithium content of 4.7%, particle size of 50μm) was added to 20mL ethyl acetate to prepare alloy powder suspension. First, add fluorosilane solution to the obtained suspension and stir for 15min; then add epoxysilane solution to the system and stir for 1h; after the reaction, separate the solid and liquid, dry the solid at 70℃ with air blast for 8h, and store it under vacuum conditions for standby use to obtain silane-coated aluminum-lithium alloy powder. The above-obtained powder was added to ethyl acetate, stirred for 10min to make it uniformly dispersed, and 0.1g GAP and 0.2mL boron trifluoride ether were added in sequence, and the reaction was stirred for 3h. After the reaction, centrifugation, washing and drying were performed to obtain the coated aluminum-lithium alloy powder.

[0051] XPS test was performed on the aluminum-lithium alloy powder coated in this comparative example. The results showed that the aluminum-lithium alloy powder after coating had F1s and F Auger peaks at 689eV and 833eV, but no N1s peak was found, indicating that this comparative example only achieved the coating of aluminum-lithium alloy powder with perfluorodecyltrimethoxysilane. This indicates that when too much fluorosilane is added, since fluorosilane is easier to combine with alloy powder than epoxy silane, it will compete with epoxy silane to a certain extent, making it impossible for epoxy silane to be coated on the surface of the alloy powder.

[0052] The coated aluminum-lithium alloy powder of this comparative example was subjected to a scanning electron microscope-energy spectrum test, and it was found that Si and F elements were evenly distributed on the surface of the alloy powder, and the distribution of N element was not obvious.

[0053] Comparative Example 3

[0054] Dissolve 0.15g 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 0.15g perfluorodecyltrimethoxysilane in 5mL ethyl acetate, stir for 5min to make them uniformly dispersed, and obtain epoxysilane solution and fluorosilane solution respectively; add 1g aluminum-lithium alloy powder (lithium content is 4.7%, particle size is 50μm) to 20mL ethyl acetate to prepare alloy powder suspension. First add fluorosilane solution to the obtained suspension and stir for 2h; then add epoxysilane solution to the system and stir for 1h; after the reaction is completed, separate the solid and liquid, dry the solid at 70℃ with air blast for 8h, and store it under vacuum conditions for standby use to obtain silane-coated aluminum-lithium alloy powder. Add the above-obtained powder to ethyl acetate, stir for 10min to make it uniformly dispersed, add 0.1g GAP and 0.2mL boron trifluoride ether in turn, continue stirring and react for 3h, and after the end, centrifuge, wash and dry to obtain the coated aluminum-lithium alloy powder.

[0055] The coated aluminum-lithium alloy powder of this comparative example was subjected to XPS testing. The results showed that only F1s and F Auger peaks appeared in the coated aluminum-lithium alloy powder, and no N1s peak was detected. This was because the fluorosilane was added too long, resulting in the formation of a dense fluorosilane coating layer on the surface of the alloy powder before the epoxy silane was added, making it impossible for the epoxy silane to be successfully coated.

[0056] The coated aluminum-lithium alloy powder of this comparative example was subjected to a scanning electron microscope-energy spectrum test, and it was found that Si and F elements were evenly distributed on the surface of the alloy powder, and no N element was present.

[0057] Comparative Example 4

[0058] Dissolve 0.3g perfluorodecyltrimethoxysilane in 5mL ethyl acetate, stir for 5min to make it uniformly dispersed, and obtain fluorosilane solution; add 1g aluminum-lithium alloy powder (lithium content is 4.7%, particle size is 50μm) to 20mL ethyl acetate to prepare alloy powder suspension. Add fluorosilane solution to the obtained suspension and stir for 1.25h; after the reaction, separate the solid and liquid, dry the solid at 70℃ with air blast for 8h, and store it under vacuum conditions for use. Add the above-obtained powder to ethyl acetate, stir for 10min to make it uniformly dispersed, add 0.1g GAP and 0.2mL boron trifluoride etherate in turn, continue stirring and react for 3h, and after the reaction, centrifuge, wash and dry to obtain the coated aluminum-lithium alloy powder.

[0059] XPS test was performed on the aluminum-lithium alloy powder coated in this comparative example. The results showed that the aluminum-lithium alloy powder after coating had F1s and F Auger peaks at 689eV and 833eV, and no N1s peak at 400eV was detected. This comparative example achieved the coating of aluminum-lithium alloy powder with perfluorodecyltrimethoxysilane. This shows that the presence of 3-(2,3-epoxypropyloxy)propyltrimethoxysilane plays a key role in whether the alloy powder can be successfully coated with GAP.

[0060] The final product of this comparative example was subjected to a scanning electron microscope-energy spectrum test, and it was found that Si and F elements were evenly distributed on the surface of the alloy powder, and no N element was present.

[0061] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.

Claims

1. A disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder, characterized in that: The coating on the surface of the aluminum-lithium alloy powder is fluorosilane, epoxysilane and GAP with fluorine atoms ≥9. The hydroxyl groups formed after the hydrolysis of fluorosilane and the free hydroxyl groups on the surface of the aluminum-lithium alloy powder undergo dehydration condensation to form Al-O-Si bonds, and van der Waals forces are formed between the F atoms and Al, so that the fluorosilane is coated on the surface of the aluminum-lithium alloy powder; the epoxysilane is connected to the aluminum-lithium alloy powder through the Al-O-Si bond, and at the same time, the fluorosilane and the epoxysilane are condensed to form Si-O-Si bonds to tightly coat the surface of the aluminum-lithium alloy powder; GAP is grafted on the outermost layer through the ring-opening addition of the terminal hydroxyl group and the epoxy group on the epoxysilane, and finally an aluminum-lithium alloy powder with a double coating layer is formed.

2. The aluminum-lithium alloy powder coated with bissilane-polyazide glycidyl ether according to claim 1, characterized in that: The fluorosilane is one or more of perfluorodecyltrimethoxysilane, perfluorooctyltrichlorosilane, perfluorohexyltrichlorosilane, perfluorooctylmethyldimethoxysilane and nonafluorohexyltrimethoxysilane; The epoxysilane is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

3. The aluminum-lithium alloy powder coated with bissilane-polyazide glycidyl ether according to claim 1, characterized in that: The molecular weight of the GAP is 800-1400.

4. A disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder according to any one of claims 1 to 3, characterized in that: The mass fraction of aluminum in the aluminum-lithium alloy powder is 90% to 98%; the particle size of the aluminum-lithium alloy powder is 5 μm to 50 μm.

5. A method for preparing a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder according to any one of claims 1 to 4, characterized in that: The method steps include: (1) dissolving a fluorosilane having a fluorine atom number of ≥9 in a second organic solvent to obtain a solution A, and dissolving an epoxysilane in a first organic solvent to obtain a solution B; (2) adding the aluminum-lithium alloy powder to the third organic solvent, stirring and dispersing the powder evenly, adding solution A, stirring and reacting for 10 to 30 minutes, adding solution B, continuing to stir and react for 1 to 1.5 hours, and after the stirring is completed, filtering, washing, and drying to obtain a disilane-coated alloy powder; (3) adding the alloy powder coated with disilane into a fourth organic solvent, then adding GAP and a catalyst, stirring the reaction for 2 to 3 hours, separating the solid and liquid after the stirring, and drying to obtain an aluminum-lithium alloy powder coated with disilane-polyazide glycidyl ether.

6. The method for preparing a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder according to claim 5, characterized in that: The first organic solvent, the second organic solvent and the third organic solvent are ethyl acetate, n-hexane, acetone or dichloromethane respectively; The third organic solvent is ethyl acetate, dichloromethane, tetrahydrofuran or N,N-dimethylformamide; The catalyst is boron trifluoride etherate, triethylamine or bismuth trichloride.

7. The method for preparing a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder according to claim 5, characterized in that: The amount of fluorosilane used is 10% to 15% of the mass of the aluminum-lithium alloy powder, the amount of epoxysilane used is 15% to 20% of the mass of the aluminum-lithium alloy powder, and the amount of GAP used is 10% to 15% of the mass of the aluminum-lithium alloy powder.

8. The method for preparing a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder according to claim 5, characterized in that: The usage ratio of the aluminum-lithium alloy powder, the fourth organic solvent and the catalyst is 1 g: 20-30 mL: 0.2-0.5 mL.

9. An application of the disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder as claimed in any one of claims 1 to 4, characterized in that: The metal fuel is used as a solid propellant.

10. The use of a disilane-polyazide glycidyl ether coated aluminum-lithium alloy powder as claimed in claim 9, characterized in that: The binder of the solid propellant is hydroxyl-terminated polybutadiene.

Citation Information

Cited By

  • High-performance HTPB propellant and preparation method thereof

    CN121974769A