Foam metal welding method using anisotropic heat-conducting filler under assistance of magnetic field

By using a combination of magnetic hexagonal boron nitride and iron particles as a filler under a magnetic field, the problem of large contact thermal resistance between foam metal and the thermally conductive substrate is solved, and high thermal conductivity and strength improvement after welding are achieved.

CN118808808APending Publication Date: 2024-10-22CHINA NORTH VEHICLE RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410703219.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

It is difficult for foam metal to form good contact with the thermally conductive substrate during the traditional welding process, resulting in a large contact thermal resistance. The existing technology lacks a welding process that can effectively reduce the contact thermal resistance.

Method used

Magnetic hexagonal boron nitride is used as a thermally conductive filler, and foam metal welding is performed with the assistance of a magnetic field. The flux is melted by heating and arranged in a directional magnetic field. Combined with the stirring effect of iron particles, the thermal conductivity and strength after welding are improved.

Benefits of technology

It effectively reduces the contact thermal resistance between the foam metal and the thermally conductive substrate, improves the thermal conductivity and strength after welding, and forms a more complete weld structure with higher mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808808A_ABST
    Figure CN118808808A_ABST
Patent Text Reader

Abstract

The invention discloses a foam metal welding method using anisotropic heat-conducting filler under the assistance of a magnetic field, and belongs to the technical field of metal interface welding processes. The method is implemented by the following steps of: 1, filling a welding flux added with magnetic hexagonal boron nitride as a filler between foam metal and a heat-conducting substrate; step 2, heating to melt the welding flux and brazing; 3, electrifying the electromagnet to enable the magnetic field direction to be consistent with the heat conduction direction; 4, keeping the combined action of high temperature and the magnetic field for 1.5-3 hours; and 5, stopping high-temperature heating, and cooling and curing according to natural aging. After the welding flux is melted, the magnetic boron nitride heat conduction particles are arranged according to the heat conduction direction under the action of a directional magnetic field, and the heat conduction strengthening effect is achieved. And the stirring effect of iron particles in the welding flux under the magnetic field effect further improves the post-welding strength effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal interface welding technology, and in particular to a foam metal welding method using anisotropic thermal conductive fillers under the assistance of a magnetic field. Background Art

[0002] Since open-cell metal foam has the characteristics of high specific surface area, high porosity, high thermal conductivity, high strength, high toughness and light weight, it can be used as a heat exchange medium to replace the compact heat exchanger of traditional military vehicles. However, as the wind-side fin of the radiator, metal foam is prone to fail to form good contact with the thermally conductive substrate during the traditional welding process due to its apparent geometric characteristics of a needle-like fiber skeleton, thus failing to dissipate the heat on the water side in time. On the other hand, the interface thermal conductivity formed by traditional aluminum solder is low. Based on the above two points, the contact thermal resistance formed between the metal foam and the thermally conductive substrate is relatively large. At present, the heat dissipation structure of metal foam mainly focuses on strengthening heat exchange and reducing resistance, processing technology, etc. In view of the above situation, there are few public reports on the welding process of metal foam to reduce the contact thermal resistance. Summary of the invention

[0003] In view of this, the present invention provides a foam metal welding method using anisotropic thermal conductive filler under the assistance of a magnetic field. The welding process method targets the unique geometric characteristics of foam metal and is beneficial to the forming of interface metal materials and the improvement of interface thermal conductivity under magnetic field-assisted welding.

[0004] A foam metal welding method using anisotropic thermal conductive filler under the assistance of a magnetic field, the implementation of the method comprises the following steps:

[0005] Step 1: Fill the space between the foam metal and the thermal conductive substrate with flux containing magnetic hexagonal boron nitride as filler;

[0006] Step 2: Heat to melt the flux and perform brazing;

[0007] Step 3: Power on the electromagnet to make the direction of the magnetic field consistent with the direction of heat conduction;

[0008] Step 4: Maintain high temperature and magnetic field for 1.5-3 hours;

[0009] Step 5: Turn off high temperature heating and allow to cool and solidify naturally.

[0010] Furthermore, the directional magnetic field is formed by an electromagnet, and the electromagnet is not energized during the solder heating process.

[0011] Furthermore, the magnetic hexagonal boron nitride is prepared by a method of mixing deionized water, nano iron oxide aqueous solution, and boron nitride particles and then drying them.

[0012] Furthermore, a certain amount of iron particles is added to the solder.

[0013] Furthermore, the magnetic hexagonal boron nitride particles are nanoparticles.

[0014] Beneficial effects:

[0015] 1. The present invention adds magnetic hexagonal boron nitride as a filler in the flux, so that the magnetic boron nitride thermal conductive particles in the solder are arranged in the thermal conductive direction under the action of the directional magnetic field after the solder is melted, thereby enhancing the thermal conductivity. The stirring effect of the iron particles in the solder under the action of the magnetic field further improves the effect of the strength after welding.

[0016] 2. The directional magnetic field of the present invention is generated by an electromagnet, which is not powered during the solder heating process. When the solder is completely melted and the heating is stopped, the electromagnet is powered to form a directional magnetic field to complete the directional arrangement of the magnetic boron nitride.

[0017] 3. The present invention adds a certain amount of iron particles to the solder. The ferromagnetic particles should have a higher melting point than the base material and the core material. Their main function is to act as a stirrer when the solder melts, so that the weld is fully uniform and has a complete morphology, further improving the structural integrity and mechanical strength of the weld. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a diagram showing the positional relationship between the foam metal and the thermally conductive substrate.

[0019] Among them, 1- foam metal, 2- thermally conductive substrate. DETAILED DESCRIPTION

[0020] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0021] The present invention provides a foam metal welding method using anisotropic thermal conductive filler under the assistance of a magnetic field, comprising the following steps:

[0022] Step 1: Fill the space between the foam metal 1 and the thermal conductive substrate 2 with flux containing magnetic hexagonal boron nitride as filler, as shown in the attached Figure 1 As shown, two thermally conductive substrates 2 sandwich the foam metal 1 to form a sandwich structure;

[0023] Step 2: Heat to melt the flux and perform brazing;

[0024] Step 3: Power on the electromagnet to make the direction of the magnetic field consistent with the direction of heat conduction;

[0025] Step 4: Maintain high temperature and magnetic field for 2 hours;

[0026] Step 5: Turn off high temperature heating and allow to cool and solidify naturally.

[0027] Preferably, the directional magnetic field is formed by an electromagnet which is not energized during the solder heating process.

[0028] Preferably, a dose of iron particles is added to the solder.

[0029] The preparation of magnetic hexagonal boron nitride particles is carried out according to the following process:

[0030] 1. Use an ultrasonic cleaner to ultrasonically clean the volumetric flask and use a drying oven to dry it;

[0031] 2. Use an electronic balance to weigh 4g of h-BN, weigh 1g at a time, and add it into the volumetric flask in four times;

[0032] 3. Add 200 ml of ultrapure water to the volumetric flask and shake the volumetric flask to initially dilute the h-BN;

[0033] 4. Clean the magnet with an ultrasonic cleaner, dry it and place it in a volumetric flask;

[0034] 5. Place the volumetric flask on a magnetic stirrer, set the speed to 900, and stir for 30 minutes to obtain a suspension of h-BN;

[0035] 6. Use a 200 ml range pipette to take 400 ml of EMG 605 magnetic fluid in two times;

[0036] 7. Use a 5 ml range pipette to extract ultrapure water to dilute the ferrofluid and shake it to disperse the diluted ferrofluid;

[0037] 8. Use drip irrigation to add ferrofluid into the h-BN aqueous solution at a uniform speed and continue stirring for 1 hour;

[0038] 9. After stirring, let it stand for 15 minutes until the liquid sinks to the bottom, and then discard 20 ml of the supernatant.

[0039] 10. Shake the remaining 180 ml suspension evenly and add it to 50 ml centrifuge bottles, 30 ml per bottle, divided into six bottles;

[0040] 11. Weigh the six bottles of dispersion separately on an electronic balance and add ultrapure water to make the mass of each bottle the same;

[0041] 12. Place six bottles of dispersion of the same mass in a centrifuge and centrifuge at 2000 rpm for 10 min.

[0042] 13. Repeat steps 11 and 12, and gradually increase the centrifugal speed to 300 rpm and 4000 rpm respectively;

[0043] 14. Place the mh-BN that has been repeatedly washed three times in a vacuum drying oven and dry it continuously at 90°C for 12 hours.

[0044] Since the in-plane and out-of-plane thermal conductivity of hexagonal boron nitride are quite different, and its out-of-plane thermal conductivity is higher than that of aluminum and aluminum alloys, it is used as a welding filler and heated and melted together with aluminum flux. During welding, the direction of the auxiliary magnetic field is kept consistent with the direction of thermal conduction. Under the action of the magnetic field, the magnetic hexagonal boron nitride is arranged in an orderly manner along the directional magnetic field. After welding, the boron nitride is fixedly arranged in the direction of thermal conduction.

[0045] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A foam metal welding method using anisotropic thermal conductive filler assisted by a magnetic field, characterized in that: The implementation of this method includes the following steps: Step 1: Fill the space between the foam metal and the thermal conductive substrate with flux containing magnetic hexagonal boron nitride as filler; Step 2: Heat to melt the flux and perform brazing; Step 3: Power on the electromagnet to make the direction of the magnetic field consistent with the direction of heat conduction; Step 4: Maintain high temperature and magnetic field for 1.5-3 hours; Step 5: Turn off high temperature heating and allow to cool and solidify naturally.

2. The foam metal welding method using anisotropic thermal conductive filler under the assistance of a magnetic field as claimed in claim 1, characterized in that: The directional magnetic field is formed by an electromagnet which is not energized during the solder heating process.

3. The foam metal welding method using anisotropic thermal conductive filler under the assistance of a magnetic field as claimed in claim 1, characterized in that: The magnetic hexagonal boron nitride is prepared by a method of mixing deionized water, nano iron oxide aqueous solution and boron nitride particles and then drying them.

4. The foam metal welding method using anisotropic thermal conductive filler under the assistance of a magnetic field as claimed in claim 3, characterized in that: Add iron particles to the solder.

5. The foam metal welding method using anisotropic thermal conductive filler under the assistance of a magnetic field as claimed in claim 3 or 4, characterized in that: The magnetic hexagonal boron nitride particles are nanoparticles.