Thin-wall and thick-wall small-deformation laser welding method for heavy gas turbine end cover assembly
Through the combined use of laser welding methods and tube expanders, the problems of large deformation and unstable welding quality when welding thin-walled and thick-walled heavy-duty gas turbine end cover components are solved, achieving efficient and precise welding effects and improving the quality of the components. Assembly accuracy and service life.
Patent Information
- Application Number
- CN202411158548.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-10-22
AI Technical Summary
When welding thin-walled and thick-walled heavy-duty gas turbine end cover components, there are problems such as large deformation, unstable welding quality, and large heat-affected zones, which affect the accuracy and service life of the components.
The laser welding method is used to fix the expansion connection through the pipe expander, and the laser welding is performed under the manual teaching pendant programming to ensure high-precision welding between the pipeline and the sealed connection plug-in, including protection, cleaning, pipe threading, pipe expansion, Pipe milling, turning and welding steps.
It achieves small deformation after welding, small heat-affected zone, fast welding speed, high precision, high flexibility and high degree of automation, meets the requirements of product assembly accuracy, and improves welding quality and production efficiency.
Abstract
Description
Technical Field
[0001] The invention relates to a laser welding method for thin-wall and thick-wall heavy-duty combustion engine end cover components with small deformation. Background Art
[0002] As a highly efficient energy conversion device, heavy-duty gas turbines use continuous flow of gas as the working fluid to drive the impeller to rotate at high speed. They are internal combustion power machinery that can convert the energy of fuel into kinetic energy and play an important role in the energy field. The end cover assembly is one of the key components of heavy-duty gas turbines. Its quality and performance directly affect the operating reliability and efficiency of the gas turbine. In the manufacture of heavy-duty gas turbine end cover assemblies, the connection between thin-walled and thick-walled components is often involved. Traditional welding methods, such as arc welding and gas shielded welding, often have many problems when welding such structures.
[0003] Since thin-walled structures have small heat capacity and poor rigidity, they are easily affected by heat input during welding and produce large deformation. Thick-walled parts are thicker, and heat transfer is uneven during welding, which can easily lead to unstable weld quality, and defects such as incomplete penetration and pores may appear inside. In addition, the heat-affected zone of traditional welding methods is large, which will change the material properties near the weld joint and reduce the overall performance and service life of the component.
[0004] In order to meet the requirements of high precision, high quality and low deformation of heavy-duty gas turbine end cover assemblies, a new welding method is urgently needed to solve the welding problem when connecting thin walls and thick walls, improve welding quality and production efficiency, and reduce deformation, thereby ensuring the stable operation and performance improvement of heavy-duty gas turbines. Summary of the invention
[0005] The present invention aims to solve the problem that the existing heavy-duty gas engine end cover assembly has large deformation after welding with thick walls and cannot ensure the subsequent assembly accuracy of the welding, and provides a laser welding method for heavy-duty gas engine end cover assembly with thin walls and thick walls and small deformation.
[0006] A laser welding method for thin-walled and thick-walled heavy-duty gas engine end cover components with small deformation in the present invention comprises:
[0007] 1. Protection: Use tape to protect the sealed chamber;
[0008] 2. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening to remove surface impurities;
[0009] 3. Pipe penetration: Pipe the stainless steel pipe and make sure the inner pipe opening is not lower than the outer end surface of the stainless steel pipe opening;
[0010] 4. Tube expansion: Use a tube expander to expand and fix the stainless steel tube;
[0011] 5. Milling pipe: Use a pipe milling cutter to remove the excess head of the pipe end in multiple times to ensure that the stainless steel pipe is aligned with the inner pipe mouth;
[0012] 6. Cleaning: Use a file to grind and clean the burrs on the milling tube side;
[0013] 7. Turn over: turn over the end face, repeat the above operation to expand and mill the tube on the reverse side;
[0014] 8. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening again to remove surface impurities;
[0015] 9. Welding: After aligning each expansion-fixed pipe opening, laser welding is performed between the pipeline and the sealing connection plug-in according to the welding parameters.
[0016] Beneficial effects of the present invention:
[0017] The present invention utilizes a tube expander for expansion and fixing, and adopts a laser welding method under the programming of a manual teaching device to weld the end cover assembly to a 16mm*0.5 stainless steel tube, thereby obtaining the NB / T47013 level 1 qualification of the penetration testing standard. Compared with common welding methods such as argon arc welding and sealing welding, the present invention adopts a laser welding method for welding, which has a small heat-affected zone, a fast welding speed, small welding deformation, high efficiency and energy saving, high precision, high flexibility, and a high degree of automation, thereby meeting the requirements for high precision in product assembly. DETAILED DESCRIPTION
[0018] Specific implementation method 1: A laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation in this implementation method includes:
[0019] 1. Protection: Use tape to protect the sealed chamber;
[0020] 2. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening to remove surface impurities;
[0021] 3. Pipe penetration: Pipe the stainless steel pipe and make sure the inner pipe opening is not lower than the outer end surface of the stainless steel pipe opening;
[0022] 4. Tube expansion: Use a tube expander to expand and fix the stainless steel tube;
[0023] 5. Milling pipe: Use a pipe milling cutter to remove the excess head of the pipe end in multiple times to ensure that the stainless steel pipe is aligned with the inner pipe mouth;
[0024] 6. Cleaning: Use a file to grind and clean the burrs on the milling tube side;
[0025] 7. Turn over: turn over the end face, repeat the above operation to expand and mill the tube on the reverse side;
[0026] 8. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening again to remove surface impurities;
[0027] 9. Welding: After aligning each expansion-fixed pipe opening, laser welding is performed between the pipeline and the sealing connection plug-in according to the welding parameters.
[0028] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the outer diameter of the stainless steel pipe in step 2 is 16 mm and the wall thickness is 0.5 mm. The other steps and parameters are the same as those in specific implementation method 1.
[0029] Specific implementation method 3: This implementation method is different from the specific implementation method 1 in that the model of the tube expander in step 4 is 6981-4141. The other steps and parameters are the same as those in the specific implementation method 1.
[0030] Specific implementation method 4: This implementation method is different from specific implementation method 1 in that: in step 4, the expansion and fixation process adopts the method of manually rotating the tube expander to perform expansion and fixation; the tube expansion rate is 0.6-1.0%. Other steps and parameters are the same as those of specific implementation method 1.
[0031] Specific implementation method 5: This implementation method is different from specific implementation method 1 in that: in the milling process of step 5, the pipe mouth is prevented from being scratched, and the amount of pipe mouth removal is ≤0.30mm. Other steps and parameters are the same as those of specific implementation method 1.
[0032] Specific implementation method 6: This implementation method is different from specific implementation method 6 in that: the welding parameters in step 9 are: the welding speed is 0.025 m / s, the power is 800w, and the laser defocus is controlled to be 0.333-0.5 mm away from the outer diameter of the tube. Other steps and parameters are the same as those in specific implementation method 6.
[0033] Specific implementation method 7: This implementation method is different from the specific implementation method 1 in that: after the welding is completed in step 9, the weld is subjected to penetrant flaw detection. The other steps and parameters are the same as those in the specific implementation method 1.
[0034] The beneficial effects of the present invention are verified by the following examples:
[0035] Embodiment 1: A laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation includes:
[0036] 1. Protection: Use tape to protect the sealed chamber;
[0037] 2. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening to remove surface impurities;
[0038] 3. Pipe penetration: Pipe the stainless steel pipe and make sure the inner pipe opening is not lower than the outer end surface of the stainless steel pipe opening;
[0039] 4. Tube expansion: Use a tube expander to expand and fix the stainless steel tube;
[0040] 5. Milling pipe: Use a pipe milling cutter to remove the excess head of the pipe end in multiple times to ensure that the stainless steel pipe is aligned with the inner pipe mouth;
[0041] 6. Cleaning: Use a file to grind and clean the burrs on the milling tube side;
[0042] 7. Turn over: turn over the end face, repeat the above operation to expand and mill the tube on the reverse side;
[0043] 8. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening again to remove surface impurities;
[0044] 9. Welding: After aligning each expansion-fixed pipe opening, laser weld the pipeline and the sealing connection plug-in according to the welding parameters;
[0045] First, use the KUKA teaching pendant to program, select the SCIRC program in the teaching pendant, use the three-point positioning method to keep the red light on the weld (0.333-0.5mm away from the outer diameter of the pipe mouth), and program the welding speed to 0.025m / s before selecting the external program; select high-purity argon gas with a purity of ≥99.99% and adjust the gas output to 20L; select the laser program pulse type in the external computer, adjust it to continuous wave and set the power to 800W; adjust the laser parameters to robot mode in the computer work interface; click on the keyboard in sequence: dust removal - gas supply - laser enable - KUKA enable - remote start - program execution, and then start welding.
[0046] This embodiment uses a tube expander for expansion and fixation, and adopts a laser welding method under the programming of a manual teach pendant to weld the end cover assembly to a 16mm*0.5 stainless steel tube, and obtains the NB / T47013 level 1 qualification of the penetration testing standard. Compared with common welding methods such as argon arc welding and sealing welding, the present invention adopts a laser welding method, which has a small heat-affected zone, a fast welding speed, small welding deformation, high efficiency and energy saving, high precision, high flexibility, and a high degree of automation, and meets the requirements of high product assembly precision.
Claims
1. A laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation, characterized in that The welding method includes:
1. Protection: Use tape to protect the sealed chamber; 2. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening to remove surface impurities; 3. Pipe penetration: Pipe the stainless steel pipe and make sure the inner pipe opening is not lower than the outer end surface of the stainless steel pipe opening; 4. Tube expansion: Use a tube expander to expand and fix the stainless steel tube; 5. Milling pipe: Use a pipe milling cutter to remove the excess head of the pipe end in multiple times to ensure that the stainless steel pipe is aligned with the inner pipe mouth; 6. Cleaning: Use a file to grind and clean the burrs on the milling tube side; 7. Turn over: turn over the end face, repeat the above operation to expand and mill the tube on the reverse side; 8. Cleaning: Use alcohol to wipe the stainless steel pipe and the inner pipe opening again to remove surface impurities; 9. Welding: After aligning each expansion-fixed pipe opening, laser welding is performed between the pipeline and the sealing connection plug-in according to the welding parameters.
2. A laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation according to claim 1, characterized in that The outer diameter of the stainless steel tube in step 2 is 16 mm and the wall thickness is 0.5 mm.
3. A laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation according to claim 2, characterized in that The model of the tube expander described in step 4 is 6981-4141.
4. A laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation according to claim 1, characterized in that In the expansion and fixing process described in step 4, the expansion and fixing is performed by manually rotating the tube expander; the tube expansion rate is 0.6-1.0%.
5. The laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation according to claim 1 is characterized in that In the milling process of step 5, the pipe mouth should be prevented from being scratched, and the removal amount of the pipe mouth should be ≤0.30mm.
6. The laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation according to claim 1 is characterized in that The welding parameters described in step nine are: welding speed is 0.025 m / s, power is 800 w, and the laser defocus is controlled to be 0.333 to 0.5 mm away from the outer diameter of the tube mouth.
7. The laser welding method for thin-walled and thick-walled heavy-duty gas turbine end cover components with small deformation according to claim 1 is characterized in that Step 9: After welding is completed, perform penetrant testing on the weld.
Citation Information
Patent Citations
Novel manufacturing technique for double-tubesheet heat exchanger
CN105014336A
Connecting method for corrosion-resistant high-temperature alloy pipe and corrosion-resistant high-temperature pipe plate and heat exchanger
CN106001825A
Method for manufacturing efficient heat exchange pipe of high-pressure boiler
CN112045379A
Tube-plate laser welding process suitable for flush type strength welding
CN112643204A
Lining tube for leaking stoppage of finned tube type heat exchanger and leaking stoppage method of lining tube
CN117288025A