Metal surface treatment method based on nano injection molding and application
By surface treatment of the metal substrate, micron-scale stripes and nano-scale holes are formed, which improves the bonding strength between metal and plastic, solves the problem of insufficient bonding force in nano-injection molding technology, and improves the stability and fatigue resistance of the product.
Patent Information
- Application Number
- CN202411240256.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In nano injection molding technology, due to process limitations, it is difficult for plastic to completely enter the nanopores on the metal surface, resulting in a decrease in the bonding force between the resin and the metal, affecting the fatigue strength and service life of the product.
By performing surface treatment on the metal substrate, including polishing, removing the metal oxide layer, using photoresist to form a micron-scale stripe structure, electrochemical etching to form a concave structure, ultrasonic vibration treatment and immersion in different solutions, nano-scale holes and active groups are generated. Improve the bonding performance of metal and plastic.
It significantly improves the bonding strength between plastic and metal, improves the nano-injection molding effect, improves the stability and bonding ability of the product, and extends the service life.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, in particular to a metal surface treatment method based on nano injection molding and application thereof. Background Art
[0002] Nano injection molding technology is a molding technology that integrates metal and plastic. It can anchor metal and plastic together through the nanopores on the metal surface, thereby tightly combining metal and plastic together. However, in the existing nano injection molding technology, due to process limitations, the nanopores prepared on the metal surface are relatively small. During the injection molding process, it is difficult for the plastic to completely enter the nanopores due to temperature, viscosity and other issues, resulting in a decrease in the bonding force between the resin and the metal, which becomes a defect of the product after nano injection molding, easily causing a decrease in fatigue resistance in the later stage and affecting the product's service life. Summary of the invention
[0003] The purpose of the present invention is to provide a metal surface treatment method based on nano injection molding and its application to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a metal surface treatment method based on nano injection molding, comprising the following steps:
[0005] S1. The surface of the metal substrate is polished to remove the metal oxide layer on the surface, and then it is immersed in an alkali solution to remove the oil stains on the surface, and then it is taken out, washed with deionized water and anhydrous ethanol three times, and then dried to obtain a metal substrate;
[0006] S2. After the photoresist is coated on the surface of the metal substrate, the photoresist layer in the exposed area of the metal substrate is removed by exposure and development, and a bare metal area and a protected photoresist area are formed on the surface of the metal substrate;
[0007] S3. Electrochemically corrode the metal substrate in step S2. After electrochemically corroding, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a rough-pore treated metal plate;
[0008] S4. The rough-pore treated metal plate is placed in a mixed etching solution, the etching time is 60-250s, the etching temperature is 35-60°C, after the etching is completed, the metal plate is removed, the surface is washed, and then placed in a nitrogen atmosphere and dried at 90-100°C for 10-15min;
[0009] S5. Immerse the metal plate treated in step S4 in γ-aminopropyltriethoxysilane, and ultrasonically vibrate for 10-15 minutes, then add distilled water (20% by volume of γ-aminopropyltriethoxysilane), and continue ultrasonically vibrating for 2-4 minutes. Then, take out the metal plate, raise the temperature to 105-110° C. and dry it for 0.5-1 hour under a nitrogen atmosphere;
[0010] S6. Immerse the metal plate treated in step S5 in a terephthalic acid solution, heat it to 80-120°C, and ultrasonically vibrate it. After immersing it for 0.5-1h, take it out and place the metal plate in pure DMF again, and ultrasonically vibrate it for 5-10min;
[0011] S7. After nitrogen is passed through ethylene glycol for 1-2 hours, an ethylene glycol impregnation solution is obtained; benzoic acid is dispersed in distilled water, the temperature is raised to 75-85° C., and nitrogen is passed through for 2-5 hours to obtain a benzoic acid impregnation solution;
[0012] The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 85-90°C, and ultrasonically shaken for 15-30 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 75-85°C, and ultrasonically shaken for 15-30 minutes. Then, the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0013] Furthermore, in step S1, the alkali solution is a mixture of 5-15 g / L sodium hydroxide and 5-10 g / L sodium phosphate, and the treatment temperature is 25-30°C.
[0014] Furthermore, in step S2, during exposure and development, the exposure shape is a plurality of parallel stripes, each stripe width is 5-15 microns, and the total area of the stripes accounts for 30-60% of the area of the exposure and development region.
[0015] Furthermore, in step S3, during electrochemical corrosion, the metal plate is placed in an electrochemical corrosion solution and electrochemically corroded. During electrochemical corrosion, the metal substrate in step S2 is used as an anode, graphite is used as a cathode, and the current density is 80-200 mA / cm 2 , the power-on time is 4-8min;
[0016] The electrochemical etching solution is a mixed solution of 1.5-3wt% hydrochloric acid, 0.5-1wt% sulfuric acid, and 0.5-0.8wt% acetic acid.
[0017] Furthermore, in step S4, the mixed etching solution is a mixture of 2.5-5wt% hydrochloric acid and 0.5-2wt% sodium acetate.
[0018] Furthermore, in step S6, the terephthalic acid solution is a mixed solution of terephthalic acid and DMF, wherein the concentration of terephthalic acid is 0.5-3wt%.
[0019] Furthermore, in step S7, the concentration of benzoic acid in the benzoic acid impregnation solution is 0.5-2wt%.
[0020] Furthermore, the metal surface treatment method is applied to nano-injection molding of PBT material on the metal surface.
[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0022] In order to improve the bonding strength between plastic and metal during nano injection molding, the present invention performs a surface treatment process on the metal plate; the present invention first uses an alkali solution to treat the oil stains on the surface of the polished metal plate, and after cleaning the surface of the metal plate with the alkali solution, a photoresist is used to coat the surface and expose and develop the surface. Currently, the photoresist can achieve micron-level development processing capabilities, and can form micron-level striped patterns on the metal surface. The metal plate is further immersed in an electrochemical etching solution. After electrochemical corrosion, micron-level striped grooves are formed on the surface of the metal plate, thereby increasing the surface area of the metal plate and forming a micron-level concave structure on the surface of the metal plate. When the plastic is injected, an anchoring effect can be achieved, thereby increasing the bonding performance of the plastic and the metal.
[0023] Afterwards, the present invention further removes the photoresist and uses a corrosive liquid to perform a corrosive treatment on the metal plate, thereby further preparing nanoscale holes on the surface of the metal plate and in its recessed structure, so that when the plastic is nano-injected on the metal surface, the plastic will preferentially combine with the micron-scale recessed structure under high temperature and pressure, and further combine with the nanoscale hole structure, thereby improving the defect of poor injection molding effect of a single nanoscale hole and improving the stability and bonding ability of the product;
[0024] Moreover, the concave structure of the corroded metal sheet also contains a large number of active groups, which can be grafted after the hydrolysis of γ-aminopropyltriethoxysilane, thereby realizing the amino treatment of the concave structure; on this basis, the present invention further uses terephthalic acid, ethylene glycol and benzoic acid, and after they are respectively configured into solutions, the metal sheet is immersed in them and heat-treated, thereby generating a PBT-like structure in the concave structure and in the nano-scale pores, improving the bonding performance between the metal sheet and the PBT plastic, thereby improving the bonding performance between the resin and the metal sheet, and further improving the bonding strength between the metal and the plastic. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The aluminum alloy plates used in the embodiments of the present invention and the comparative examples are 6061 aluminum-magnesium-silicon aluminum alloys;
[0027] Embodiment 1. A metal surface treatment method based on nano injection molding comprises the following steps:
[0028] S1. The surface of the aluminum alloy plate was polished to remove the metal oxide layer on the surface, and then the plate was placed in an alkali solution composed of 10 g / L sodium hydroxide and 8 g / L sodium phosphate, heated to 25°C, and soaked for 90 seconds to remove the surface oil stains. The plate was taken out and washed with deionized water and anhydrous ethanol for 3 times, respectively, and then dried to obtain a metal substrate;
[0029] S2. After the metal substrate surface is coated with photoresist, it is exposed and developed, and the exposure shape is a plurality of parallel stripes, each stripe is 8 microns wide, and the total area of the stripes accounts for 40% of the area of the exposure and development area. After the exposure is completed, the photoresist layer of the metal substrate exposure area is removed to form a bare metal area and a protected photoresist area on the metal substrate surface;
[0030] S3. Place the metal substrate in step S2 in an electrochemical etching solution composed of 2wt% hydrochloric acid, 1wt% sulfuric acid, and 0.8wt% acetic acid, and perform electrochemical etching on it. During the electrochemical etching, the metal substrate in step S2 is used as the anode, graphite is used as the cathode, the current density is 100mA / cm2, and the power-on time is 5min. After the electrochemical etching is completed, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a coarse-pore treated metal plate;
[0031] S4. The rough-pore treated metal plate is placed in a mixed etching solution of 3wt% hydrochloric acid and 1wt% sodium acetate, the etching time is 100s, the etching temperature is 45°C, after the etching is completed, the metal plate is taken out, washed with deionized water, immersed in anhydrous ethanol, ultrasonically shaken for 2min, taken out, placed in a nitrogen atmosphere, and dried at 100°C for 15min;
[0032] S5. The metal plate treated in step S4 is immersed in γ-aminopropyltriethoxysilane, and after ultrasonic oscillation for 10 minutes, 20% of the volume of γ-aminopropyltriethoxysilane in distilled water is added thereto, and the ultrasonic oscillation is continued for 2 minutes, and the metal plate is taken out and dried at 110° C. for 1 hour under a nitrogen atmosphere;
[0033] S6. Dissolve terephthalic acid in DMF, raise the temperature to 45-60°C, and prepare a terephthalic acid solution with a concentration of 0.5wt%. Immerse the metal plate treated in step S5 in the terephthalic acid solution, raise the temperature to 85°C, and ultrasonically vibrate. After immersion for 01h, take out the metal plate, place it in pure DMF again, and ultrasonically vibrate it for 10min;
[0034] S7. After nitrogen was passed through ethylene glycol for 1 hour, an ethylene glycol impregnation solution was obtained; benzoic acid was dispersed in distilled water, the temperature was raised to 75°C, and nitrogen was passed through for 2 hours to obtain a benzoic acid impregnation solution with a concentration of 0.5wt%;
[0035] The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 90°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 85°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0036] Embodiment 2. A metal surface treatment method based on nano injection molding, comprising the following steps:
[0037] Compared with Example 1, this embodiment increases the total area of the stripes in step S2 to the total area of the exposure and development area;
[0038] S1. The surface of the aluminum alloy plate was polished to remove the metal oxide layer on the surface, and then the plate was placed in an alkali solution composed of 10 g / L sodium hydroxide and 8 g / L sodium phosphate, heated to 25°C, and soaked for 90 seconds to remove the surface oil stains. The plate was taken out and washed with deionized water and anhydrous ethanol for 3 times, respectively, and then dried to obtain a metal substrate;
[0039] S2. After the metal substrate surface is coated with photoresist, it is exposed and developed, and the exposure shape is a plurality of parallel stripes, each stripe is 8 microns wide, and the total area of the stripes accounts for 60% of the area of the exposure and development area. After the exposure is completed, the photoresist layer of the metal substrate exposure area is removed to form a bare metal area and a protected photoresist area on the metal substrate surface;
[0040] S3. Place the metal substrate in step S2 in an electrochemical etching solution composed of 2wt% hydrochloric acid, 1wt% sulfuric acid, and 0.8wt% acetic acid, and perform electrochemical etching on it. During the electrochemical etching, the metal substrate in step S2 is used as the anode, graphite is used as the cathode, the current density is 100mA / cm2, and the power-on time is 5min. After the electrochemical etching is completed, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a coarse-pore treated metal plate;
[0041] S4. The rough-pore treated metal plate is placed in a mixed etching solution of 3wt% hydrochloric acid and 1wt% sodium acetate, the etching time is 100s, the etching temperature is 45°C, after the etching is completed, the metal plate is taken out, washed with deionized water, immersed in anhydrous ethanol, ultrasonically shaken for 2min, taken out, placed in a nitrogen atmosphere, and dried at 100°C for 15min;
[0042] S5. The metal plate treated in step S4 is immersed in γ-aminopropyltriethoxysilane, and after ultrasonic oscillation for 10 minutes, 20% of the volume of γ-aminopropyltriethoxysilane in distilled water is added thereto, and the ultrasonic oscillation is continued for 2 minutes, and the metal plate is taken out and dried at 110° C. for 1 hour under a nitrogen atmosphere;
[0043] S6. Dissolve terephthalic acid in DMF, raise the temperature to 45-60°C, and prepare a terephthalic acid solution with a concentration of 0.5wt%. Immerse the metal plate treated in step S5 in the terephthalic acid solution, raise the temperature to 85°C, and ultrasonically vibrate. After immersion for 01h, take out the metal plate, place it in pure DMF again, and ultrasonically vibrate it for 10min;
[0044] S7. After nitrogen was passed through ethylene glycol for 1 hour, an ethylene glycol impregnation solution was obtained; benzoic acid was dispersed in distilled water, the temperature was raised to 75°C, and nitrogen was passed through for 2 hours to obtain a benzoic acid impregnation solution with a concentration of 0.5wt%;
[0045] The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 90°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 85°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0046] Embodiment 3. A metal surface treatment method based on nano injection molding, comprising the following steps:
[0047] Compared with Example 1, this example increases the concentration of terephthalic acid in step S6;
[0048] S1. The surface of the aluminum alloy plate was polished to remove the metal oxide layer on the surface, and then the plate was placed in an alkali solution composed of 10 g / L sodium hydroxide and 8 g / L sodium phosphate, heated to 25°C, and soaked for 90 seconds to remove the surface oil stains. The plate was taken out and washed with deionized water and anhydrous ethanol for 3 times, respectively, and then dried to obtain a metal substrate;
[0049] S2. After the metal substrate surface is coated with photoresist, it is exposed and developed, and the exposure shape is a plurality of parallel stripes, each stripe is 8 microns wide, and the total area of the stripes accounts for 40% of the area of the exposure and development area. After the exposure is completed, the photoresist layer of the metal substrate exposure area is removed to form a bare metal area and a protected photoresist area on the metal substrate surface;
[0050] S3. Place the metal substrate in step S2 in an electrochemical etching solution composed of 2wt% hydrochloric acid, 1wt% sulfuric acid, and 0.8wt% acetic acid, and perform electrochemical etching on it. During the electrochemical etching, the metal substrate in step S2 is used as the anode, graphite is used as the cathode, the current density is 100mA / cm2, and the power-on time is 5min. After the electrochemical etching is completed, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a coarse-pore treated metal plate;
[0051] S4. The rough-pore treated metal plate is placed in a mixed etching solution of 3wt% hydrochloric acid and 1wt% sodium acetate, the etching time is 100s, the etching temperature is 45°C, after the etching is completed, the metal plate is taken out, washed with deionized water, immersed in anhydrous ethanol, ultrasonically shaken for 2min, taken out, placed in a nitrogen atmosphere, and dried at 100°C for 15min;
[0052] S5. The metal plate treated in step S4 is immersed in γ-aminopropyltriethoxysilane, and after ultrasonic oscillation for 10 minutes, 20% of the volume of γ-aminopropyltriethoxysilane in distilled water is added thereto, and the ultrasonic oscillation is continued for 2 minutes, and the metal plate is taken out and dried at 110° C. for 1 hour under a nitrogen atmosphere;
[0053] S6. Dissolve terephthalic acid in DMF, raise the temperature to 45-60°C, and prepare a terephthalic acid solution with a concentration of 3 wt%. Immerse the metal plate treated in step S5 in the terephthalic acid solution, raise the temperature to 85°C, and ultrasonically vibrate. After immersion for 01h, take out the metal plate, place it in pure DMF again, and ultrasonically vibrate it for 10min;
[0054] S7. After nitrogen was passed through ethylene glycol for 1 hour, an ethylene glycol impregnation solution was obtained; benzoic acid was dispersed in distilled water, the temperature was raised to 75°C, and nitrogen was passed through for 2 hours to obtain a benzoic acid impregnation solution with a concentration of 0.5wt%;
[0055] The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 90°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 85°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0056] Embodiment 4. A metal surface treatment method based on nano injection molding, comprising the following steps:
[0057] Compared with Example 1, this embodiment increases the concentration of benzoic acid in step S7;
[0058] S1. The surface of the aluminum alloy plate was polished to remove the metal oxide layer on the surface, and then the plate was placed in an alkali solution composed of 10 g / L sodium hydroxide and 8 g / L sodium phosphate, heated to 25°C, and soaked for 90 seconds to remove the surface oil stains. The plate was taken out and washed with deionized water and anhydrous ethanol for 3 times, respectively, and then dried to obtain a metal substrate;
[0059] S2. After the metal substrate surface is coated with photoresist, it is exposed and developed, and the exposure shape is a plurality of parallel stripes, each stripe is 8 microns wide, and the total area of the stripes accounts for 40% of the area of the exposure and development area. After the exposure is completed, the photoresist layer of the metal substrate exposure area is removed to form a bare metal area and a protected photoresist area on the metal substrate surface;
[0060] S3. Place the metal substrate in step S2 in an electrochemical etching solution composed of 2wt% hydrochloric acid, 1wt% sulfuric acid, and 0.8wt% acetic acid, and perform electrochemical etching on it. During the electrochemical etching, the metal substrate in step S2 is used as the anode, graphite is used as the cathode, the current density is 100mA / cm2, and the power-on time is 5min. After the electrochemical etching is completed, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a coarse-pore treated metal plate;
[0061] S4. The rough-pore treated metal plate is placed in a mixed etching solution of 3wt% hydrochloric acid and 1wt% sodium acetate, the etching time is 100s, the etching temperature is 45°C, after the etching is completed, the metal plate is taken out, washed with deionized water, immersed in anhydrous ethanol, ultrasonically shaken for 2min, taken out, placed in a nitrogen atmosphere, and dried at 100°C for 15min;
[0062] S5. The metal plate treated in step S4 is immersed in γ-aminopropyltriethoxysilane, and after ultrasonic oscillation for 10 minutes, 20% of the volume of γ-aminopropyltriethoxysilane in distilled water is added thereto, and the ultrasonic oscillation is continued for 2 minutes, and the metal plate is taken out and dried at 110° C. for 1 hour under a nitrogen atmosphere;
[0063] S6. Dissolve terephthalic acid in DMF, raise the temperature to 45-60°C, and prepare a terephthalic acid solution with a concentration of 0.5wt%. Immerse the metal plate treated in step S5 in the terephthalic acid solution, raise the temperature to 85°C, and ultrasonically vibrate. After immersion for 01h, take out the metal plate, place it in pure DMF again, and ultrasonically vibrate it for 10min;
[0064] S7. After nitrogen was passed through ethylene glycol for 1 hour, an ethylene glycol impregnation solution was obtained; benzoic acid was dispersed in distilled water, the temperature was raised to 75° C., and nitrogen was passed through for 2 hours to obtain a benzoic acid impregnation solution with a concentration of 2 wt%;
[0065] The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 90°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 85°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0066] Embodiment 5. A metal surface treatment method based on nano injection molding, comprising the following steps:
[0067] S1. The surface of the aluminum alloy plate was polished to remove the metal oxide layer on the surface, and then the plate was placed in an alkali solution composed of 10 g / L sodium hydroxide and 8 g / L sodium phosphate, heated to 25°C, and soaked for 90 seconds to remove the surface oil stains. The plate was taken out and washed with deionized water and anhydrous ethanol for 3 times, respectively, and then dried to obtain a metal substrate;
[0068] S2. After the metal substrate surface is coated with photoresist, it is exposed and developed, and the exposure shape is a plurality of parallel stripes, each stripe is 8 microns wide, and the total area of the stripes accounts for 60% of the area of the exposure and development area. After the exposure is completed, the photoresist layer of the metal substrate exposure area is removed to form a bare metal area and a protected photoresist area on the metal substrate surface;
[0069] S3. Place the metal substrate in step S2 in an electrochemical etching solution composed of 2wt% hydrochloric acid, 1wt% sulfuric acid, and 0.8wt% acetic acid, and perform electrochemical etching on it. During the electrochemical etching, the metal substrate in step S2 is used as the anode, graphite is used as the cathode, the current density is 100mA / cm2, and the power-on time is 5min. After the electrochemical etching is completed, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a coarse-pore treated metal plate;
[0070] S4. The rough-pore treated metal plate is placed in a mixed etching solution of 3wt% hydrochloric acid and 1wt% sodium acetate, the etching time is 100s, the etching temperature is 45°C, after the etching is completed, the metal plate is taken out, washed with deionized water, immersed in anhydrous ethanol, ultrasonically shaken for 2min, taken out, placed in a nitrogen atmosphere, and dried at 100°C for 15min;
[0071] S5. The metal plate treated in step S4 is immersed in γ-aminopropyltriethoxysilane, and after ultrasonic oscillation for 10 minutes, 20% of the volume of γ-aminopropyltriethoxysilane in distilled water is added thereto, and the ultrasonic oscillation is continued for 2 minutes, and the metal plate is taken out and dried at 110° C. for 1 hour under a nitrogen atmosphere;
[0072] S6. Dissolve terephthalic acid in DMF, raise the temperature to 45-60°C, and prepare a terephthalic acid solution with a concentration of 3 wt%. Immerse the metal plate treated in step S5 in the terephthalic acid solution, raise the temperature to 85°C, and ultrasonically vibrate. After immersion for 01h, take out the metal plate, place it in pure DMF again, and ultrasonically vibrate it for 10min;
[0073] S7. After nitrogen was passed through ethylene glycol for 1 hour, an ethylene glycol impregnation solution was obtained; benzoic acid was dispersed in distilled water, the temperature was raised to 75° C., and nitrogen was passed through for 2 hours to obtain a benzoic acid impregnation solution with a concentration of 2 wt%;
[0074] The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 90°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 85°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0075] Comparative Example 1. A metal surface treatment method based on nano injection molding, comprising the following steps:
[0076] Compared with Example 1, the metal plate was not treated in step S2 in this comparative example;
[0077] S1. The surface of the aluminum alloy plate was polished to remove the metal oxide layer on the surface, and then the plate was placed in an alkali solution composed of 10 g / L sodium hydroxide and 8 g / L sodium phosphate, heated to 25°C, and soaked for 90 seconds to remove the surface oil stains. The plate was taken out and washed with deionized water and anhydrous ethanol for 3 times, respectively, and then dried to obtain a metal substrate;
[0078] S2. Place the metal substrate in step S1 in an electrochemical etching solution composed of 2wt% hydrochloric acid, 1wt% sulfuric acid, and 0.8wt% acetic acid, and perform electrochemical etching on the metal substrate. During the electrochemical etching, the metal substrate in step S2 is used as the anode, graphite is used as the cathode, the current density is 100mA / cm2, and the power-on time is 5min. After the electrochemical etching is completed, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a coarse-pore treated metal plate;
[0079] S3. The rough-pore treated metal plate is placed in a mixed etching solution of 3wt% hydrochloric acid and 1wt% sodium acetate, the etching time is 100s, the etching temperature is 45°C, after the etching is completed, the metal plate is taken out, washed with deionized water, immersed in anhydrous ethanol, ultrasonically shaken for 2min, taken out, placed in a nitrogen atmosphere, and dried at 100°C for 15min;
[0080] S4. Immerse the metal plate treated in step S3 in γ-aminopropyltriethoxysilane, and ultrasonically vibrate for 10 minutes, then add distilled water (20% by volume of γ-aminopropyltriethoxysilane), and continue ultrasonically vibrating for 2 minutes, then take out the metal plate, and heat it to 110° C. and dry it for 1 hour under a nitrogen atmosphere;
[0081] S5. Dissolve terephthalic acid in DMF, raise the temperature to 45-60°C, and prepare a terephthalic acid solution with a concentration of 0.5wt%. Immerse the metal plate treated in step S5 in the terephthalic acid solution, raise the temperature to 85°C, and ultrasonically vibrate. After immersion for 01h, take out the metal plate, place it in pure DMF again, and ultrasonically vibrate it for 10min;
[0082] S6. After nitrogen was passed through ethylene glycol for 1 hour, an ethylene glycol impregnation solution was obtained; benzoic acid was dispersed in distilled water, the temperature was raised to 75°C, and nitrogen was passed through for 2 hours to obtain a benzoic acid impregnation solution with a concentration of 0.5wt%;
[0083] The metal plate treated in step S5 is immersed in ethylene glycol impregnation solution, heated to 90°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 85°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0084] Comparative Example 2. A metal surface treatment method based on nano injection molding, comprising the following steps:
[0085] Compared with Example 1, this comparative example does not perform steps S5-S7 on the metal plate;
[0086] S1. The surface of the aluminum alloy plate was polished to remove the metal oxide layer on the surface, and then the plate was placed in an alkali solution composed of 10 g / L sodium hydroxide and 8 g / L sodium phosphate, heated to 25°C, and soaked for 90 seconds to remove the surface oil stains. The plate was taken out and washed with deionized water and anhydrous ethanol for 3 times, respectively, and then dried to obtain a metal substrate;
[0087] S2. After the metal substrate surface is coated with photoresist, it is exposed and developed, and the exposure shape is a plurality of parallel stripes, each stripe is 8 microns wide, and the total area of the stripes accounts for 40% of the area of the exposure and development area. After the exposure is completed, the photoresist layer of the metal substrate exposure area is removed to form a bare metal area and a protected photoresist area on the metal substrate surface;
[0088] S3. Place the metal substrate in step S2 in an electrochemical etching solution composed of 2wt% hydrochloric acid, 1wt% sulfuric acid, and 0.8wt% acetic acid, and perform electrochemical etching on it. During the electrochemical etching, the metal substrate in step S2 is used as the anode, graphite is used as the cathode, the current density is 100mA / cm2, and the power-on time is 5min. After the electrochemical etching is completed, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a coarse-pore treated metal plate;
[0089] S4. The rough-pore treated metal plate is placed in a mixed etching solution of 3wt% hydrochloric acid and 1wt% sodium acetate, the etching time is 100s, the etching temperature is 45°C, after the etching is completed, the metal plate is taken out, washed with deionized water, immersed in anhydrous ethanol, ultrasonically shaken for 2min, taken out, placed in a nitrogen atmosphere, and dried at 100°C for 15min;
[0090] S5. The metal plate treated in step S4 is immersed in γ-aminopropyltriethoxysilane, and after ultrasonic oscillation for 10 minutes, 20% of the volume of γ-aminopropyltriethoxysilane in distilled water is added thereto, and the ultrasonic oscillation is continued for 2 minutes, and the metal plate is taken out and dried at 110° C. for 1 hour under a nitrogen atmosphere;
[0091] S6. Dissolve terephthalic acid in DMF, raise the temperature to 45-60°C, and prepare a terephthalic acid solution with a concentration of 0.5wt%. Immerse the metal plate treated in step S5 in the terephthalic acid solution, raise the temperature to 85°C, and ultrasonically vibrate. After immersion for 01h, take out the metal plate, place it in pure DMF again, and ultrasonically vibrate it for 10min;
[0092] S7. After nitrogen was passed through ethylene glycol for 1 hour, an ethylene glycol impregnation solution was obtained; benzoic acid was dispersed in distilled water, the temperature was raised to 75°C, and nitrogen was passed through for 2 hours to obtain a benzoic acid impregnation solution with a concentration of 0.5wt%;
[0093] The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 90°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 85°C, and ultrasonically shaken for 20 minutes, then the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
[0094] Nano injection molding was performed on the surface of the metal plate treated by the surface treatment methods of Examples 1-5 and Comparative Examples 1-2, respectively. The thickness of the metal plate was 3 mm, the nano injection molding material was PBT (Polyplastic PBT 2000 of Japan), the injection molding pressure was 120 MPa, the holding pressure was 100 MPa, and the holding time was 3 s.
[0095] Another pair of comparison 3 is set up, in which the metal plate is treated by the treatment method of Example 1, the nano injection molding material is changed to PPA, and the rest remains unchanged;
[0096] The nano injection molding samples of Examples 1-5 and Comparative Examples 1-3 were subjected to tensile tests using a CMT2203 push-pull testing machine. The test results are shown in the following table;
[0097] The nano injection molded samples of Examples 1-5 and Comparative Examples 1-3 were tested for impact strength according to ASTM D256; the test results are shown in the table below;
[0098] <![CDATA[Tensile force (kgf / 0.5 cm 2 )]]> Impact strength (J / m) Example 1 139.25 28.6 Example 2 146.73 28.9 Example 3 139.82 28.6 Example 4 139.78 28.6 Example 5 147.91 29.0 Comparative Example 1 131.67 28.1 Comparative Example 2 132.15 28.4 Comparative Example 3 128.74 27.5
[0099] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A metal surface treatment method based on nano injection molding, It is characterized in that The following steps are involved: S1. The surface of the metal substrate is polished to remove the metal oxide layer on the surface, and then it is immersed in an alkali solution to remove the oil stains on the surface, and then it is taken out, washed with deionized water and anhydrous ethanol three times, and then dried to obtain a metal substrate; S2. After the photoresist is coated on the surface of the metal substrate, the photoresist layer in the exposed area of the metal substrate is removed by exposure and development, and a bare metal area and a protected photoresist area are formed on the surface of the metal substrate; S3. Electrochemically corrode the metal substrate in step S2. After electrochemically corroding, take out the metal plate, wash it with distilled water, expose the surface of the metal plate again, remove the remaining photoresist, wash the surface of the metal plate with anhydrous ethanol, and dry it to obtain a rough-pore treated metal plate; S4. The rough-pore treated metal plate is placed in a mixed etching solution, the etching time is 60-250s, the etching temperature is 35-60°C, after the etching is completed, the metal plate is removed, the surface is washed, and then placed in a nitrogen atmosphere and dried at 90-100°C for 10-15min; S5. Immerse the metal plate treated in step S4 in γ-aminopropyltriethoxysilane, and ultrasonically vibrate for 10-15 minutes, then add distilled water (20% by volume of γ-aminopropyltriethoxysilane), and continue ultrasonically vibrating for 2-4 minutes. Then, take out the metal plate, raise the temperature to 105-110° C. and dry it for 0.5-1 hour under a nitrogen atmosphere; S6. Immerse the metal plate treated in step S5 in a terephthalic acid solution, heat it to 80-120°C, and ultrasonically vibrate it. After immersing it for 0.5-1h, take it out and place the metal plate in pure DMF again, and ultrasonically vibrate it for 5-10min; S7. After nitrogen is passed through ethylene glycol for 1-2 hours, an ethylene glycol impregnation solution is obtained; benzoic acid is dispersed in distilled water, the temperature is raised to 75-85° C., and nitrogen is passed through for 2-5 hours to obtain a benzoic acid impregnation solution; The metal plate treated in step S6 is immersed in ethylene glycol impregnation solution, heated to 85-90°C, and ultrasonically shaken for 15-30 minutes, then the metal plate is taken out, and the surface of the metal plate is rinsed with distilled water. The metal plate is immersed in benzoic acid impregnation solution again, heated to 75-85°C, and ultrasonically shaken for 15-30 minutes. Then, the metal plate is taken out, and it is rinsed with distilled water again and dried to complete the surface treatment of the metal.
2. A metal surface treatment method based on nano injection molding according to claim 1, Features: In step S1, the alkali solution is a mixture of 5-15 g / L sodium hydroxide and 5-10 g / L sodium phosphate, and the treatment temperature is 25-30°C.
3. A metal surface treatment method based on nano injection molding according to claim 1, Features: In step S2, during exposure and development, the exposure shape is a plurality of parallel stripes, each stripe width is 5-15 microns, and the total area of the stripes accounts for 30-60% of the area of the exposure and development region.
4. A metal surface treatment method based on nano injection molding according to claim 1, Features: In step S3, during electrochemical corrosion, the metal plate is placed in an electrochemical corrosion solution and electrochemically corroded. During electrochemical corrosion, the metal substrate in step S2 is used as an anode, graphite is used as a cathode, and the current density is 80-200 mA / cm 2 , the power-on time is 4-8min; The electrochemical etching solution is a mixed solution of 1.5-3wt% hydrochloric acid, 0.5-1wt% sulfuric acid, and 0.5-0.8wt% acetic acid.
5. A metal surface treatment method based on nano injection molding according to claim 1, Features: In step S4, the mixed etching solution is a mixture of 2.5-5wt% hydrochloric acid and 0.5-2wt% sodium acetate.
6. A metal surface treatment method based on nano injection molding according to claim 1, Features: In step S6, the terephthalic acid solution is a mixed solution of terephthalic acid and DMF, wherein the concentration of terephthalic acid is 0.5-3wt%.
7. A metal surface treatment method based on nano injection molding according to claim 1, Features: In step S7, the concentration of benzoic acid in the benzoic acid impregnation solution is 0.5-2wt%.
8. An application of the metal surface treatment method according to any one of claims 1 to 7, Features: The metal surface treatment method is applied to nano injection molding of PBT material on the metal surface.
Citation Information
Patent Citations
Aluminum or aluminum alloy metal nanometer injection molding method
CN108943565A
Metal-plastic composite, preparation method and preparation device
CN112318814A
Injection-molded ultrahigh-strength metal-polymer joint and preparation method thereof
CN117774218A
Cited By
Metal and nylon heterogeneous connection material with high interface bonding strength and preparation method of metal and nylon heterogeneous connection material
CN119704528A
Metal and nylon heterogeneous connecting material with strong interface bonding strength and preparation method thereof
CN119704528B