Method for producing a molded part and molded part
By preparing nonwoven fabrics from a mixture of continuous filaments and short fibers, and applying heat and pressure in a pressing mold, the problems of sustainability and insufficient mechanical properties of molded parts are solved, and efficient and economical preparation of molded parts is achieved. Suitable for many applications.
Patent Information
- Application Number
- CN202410460797.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-22
AI Technical Summary
There are shortcomings in the sustainability and mechanical properties of existing molded parts. In particular, molded parts based on plastics and petroleum raw materials have low sustainability and poor mechanical properties, and moldings based on cellulose have complex and costly preparation methods. , and the mechanical properties cannot meet all requirements.
Non-woven fabrics are prepared from a mixture of continuous filaments and short fibers. The filament-air flow and short fiber-air flow are produced through a spinning nozzle and a short fiber production device. After being combined, they are fully mixed on the laying conveyor to form a non-woven fabric. material, and heat and apply deformation pressure in a pressing mold to prepare molded parts.
This enables the use of sustainable raw materials to produce molded parts that meet all requirements for mechanical properties, while reducing the proportion of continuous filaments, improving the mechanical properties and economy of the molded parts, and is suitable for applications such as food containers and automotive structural components. .
Smart Images

Figure CN118814366A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing a molded part and to a molded part. The molded part according to the invention can be, in particular, a container for holding and / or packaging food, such as dishes. According to a preferred embodiment, the molded part according to the invention is a food bowl or other disposable tableware. Furthermore, the molded part according to the invention is a structural component for the interior of a vehicle, such as a lining element. In principle, however, other possible applications of the molded part according to the invention also lie within the scope of the invention. Background Art
[0002] Methods for producing molded parts and molded parts are known in principle from practice in various embodiments. Many of the molded parts known from practice consist of plastic materials. For example, plastic bowls and plates for dishes produced by deep drawing are known. Structural components for automobiles also generally consist of plastic. Such plastic molded parts and the corresponding production methods are less sustainable. The molded parts are mostly composed completely or to a large extent of plastic or petroleum-based raw materials.
[0003] In addition, molded parts made of cellulose and sometimes of renewable raw materials are known. However, the production methods for such cellulose-based molded parts are generally highly complex and cost-intensive and therefore less economical. It has also been shown that the molded parts obtained do not meet all requirements with regard to their mechanical properties (for example with regard to their mechanical strength and / or their flexibility). In this regard, the measures known from practice need to be improved on the one hand with regard to the sustainability of the molded parts (for example the raw materials used) and on the other hand with regard to the mechanical properties of the molded parts. The present invention is proposed here. Summary of the invention
[0004] In contrast to the prior art, the invention is based on the technical problem of providing a method of the type mentioned in the introduction, with which a molded part can be produced which is distinguished by its sustainability or by the use of sustainable, in particular renewable raw materials and which nevertheless meets all requirements with regard to its mechanical properties. In addition, the invention is based on the technical problem of providing a corresponding molded part.
[0005] In order to solve the technical problem, the present invention discloses a method for producing a molded part from at least one nonwoven fabric, wherein the at least one nonwoven fabric has at least one layer, in particular one layer, formed from a continuous filament-staple fiber mixture, wherein at least one filament-air stream comprising continuous filaments is generated by at least one spinning nozzle, and wherein at least one staple fiber-air stream comprising staple fibers is produced by at least one staple fiber generating device.
[0006] wherein the at least one filament-air stream and the at least one staple-air stream are combined in a contact zone and subsequently laid down as a continuous filament-staple fiber mixture on at least one laying conveyor, in particular at least one laying screen belt, to form a nonwoven fabric or a fibrous web, wherein the continuous filaments of the continuous filament-staple fiber mixture laid down on the laying conveyor form a matrix in which the staple fibers are embedded,
[0007] wherein the at least one nonwoven fabric is arranged in a pressing mold, wherein the nonwoven fabric is heated—in particular by temperature control of the pressing mold—to a temperature in the range of 30° C. to 275° C., preferably 60° C. to 260° C., preferably 100° C. to 250° C., and wherein the nonwoven fabric—preferably the heated nonwoven fabric—is subjected to a deformation pressure of at least 1 MPa, preferably 2 MPa to 40 MPa, preferably 3 MPa to 30 MPa, further preferably 4 MPa to 25 MPa, very preferably 5 MPa to 23 MPa, particularly preferably 6 MPa to 22 MPa, very particularly preferably 7 MPa to 21 MPa, for example 15 MPa to 20 MPa, and is molded into a molded part. According to a further preferred embodiment of the invention, the at least one nonwoven fabric is heated to a temperature in the range of 100° C. to 200° C.
[0008] In the context of the present invention, “the at least one nonwoven fabric is subjected to a deformation pressure in a pressing mold” means in particular that at least one element of the pressing mold, preferably a punch, acts on or presses the at least one nonwoven fabric with a corresponding deformation pressure. It is possible that the at least one nonwoven fabric is subjected to an isostatic deformation pressure within the specified range in the pressing mold. The pressing mold or the pressing device is then suitably designed accordingly, for example, a closed pressure chamber can be provided.
[0009] Within the scope of the present invention, the expression "filament-air stream" refers in particular to a stream of continuous filaments and air generated by a spinning nozzle. Within the scope of the method according to the invention, the filament-air stream comprising continuous filaments preferably flows in the direction of the at least one short fiber-air stream and / or in the direction of the web laying conveyor. Within the scope of the present invention, the expression "short fiber-air stream" refers in particular to a stream of short fibers and air generated by a short fiber generating device, wherein the short fiber-air stream flows appropriately in the direction of the web laying conveyor and / or in the direction of the at least one filament-air stream. Within the scope of the present invention, in other cases, the term "fiber" refers to both continuous filaments and short fibers. Continuous filaments are distinguished from short fibers by their almost unlimited length, which have a much smaller length of, for example, 0.1 mm to 60 mm.
[0010] According to the invention, the at least one filament-air stream is combined with the at least one, in particular one, short fiber-air stream in a contact zone. Within the scope of the invention, the contact zone is particularly arranged above the web-laying conveyor, preferably above the web-laying screen belt, so that the at least one filament-air stream and the at least one short fiber-air stream are combined in the contact zone above the web-laying conveyor. In the contact zone, the at least one filament-air stream and the short fiber-air stream are fully mixed. According to a preferred embodiment of the method of the invention, the continuous filament-short fiber mixture produced in this way flows from the contact zone to the web-laying conveyor as a uniform or substantially uniform mixture. By fully mixing and distributing the short fibers with the continuous filaments in the continuous filament-short fiber mixture according to the invention, particularly advantageous properties of the nonwoven fabric and the corresponding molded part laid are obtained. For example, a relatively low continuous filament ratio in the at least one nonwoven fabric or in the molded part is sufficient, so that the continuous filaments can form a matrix in which the short fibers are embedded in a more functionally reliable manner, thereby ensuring the advantageous mechanical properties of the molded part.
[0011] According to a preferred embodiment, the laying mesh conveyor is a laying mesh belt, particularly preferably an air-permeable laying mesh belt. According to a very particularly preferred embodiment, the laying mesh belt or the air-permeable laying mesh belt is a continuously movable, particularly endless, laying mesh belt.
[0012] According to the present invention, the at least one nonwoven fabric is arranged in a pressing mold and heated to a temperature in the range of 30°C to 275°C, preferably 60°C to 260°C, preferably 100°C to 250°C. This heating of the nonwoven fabric is preferably carried out by temperature control of the pressing mold. In this connection, temperature control of the pressing mold refers in particular to heating or warming the pressing mold. However, in principle, it is also possible that the nonwoven fabric has been heated to a corresponding temperature or at least partially heated or preheated before being arranged in the pressing mold. This can be done, for example, by a heating device arranged upstream of the pressing mold. In addition, according to the present invention, the nonwoven fabric is applied with a deformation pressure of at least 1MPa, preferably 2MPa to 40MPa, preferably 3MPa to 30MPa, further preferably 4MPa to 25MPa, very preferably 5MPa to 23MPa, particularly preferably 6MPa to 22MPa, very particularly preferably 7MPa to 21MPa, for example 15MPa to 20MPa and is molded into a molded part. Expediently, the nonwoven is already heated to a temperature in the range of 30° C. to 275° C., preferably 60° C. to 260° C., preferably 100° C. to 250° C. before the deformation pressure is applied. However, it is also possible in principle that the nonwoven is already subjected to the deformation pressure in the pressing mold before it is (completely) heated to this temperature and is only (completely) heated to this temperature, in particular by tempering the pressing mold, so that the nonwoven is preferably heated or further heated during the application of pressure.
[0013] According to a very particularly preferred embodiment of the method according to the invention, the at least one non-woven fabric is first arranged in the pressing mold, then heated to a temperature in the range of 30°C to 275°C, preferably 60°C to 260°C, preferably 100°C to 250°C by temperature control of the pressing mold, and subsequently a deforming pressure is applied to the heated non-woven fabric in the pressing mold and molded into a molded part.
[0014] It has proven useful if the at least one nonwoven arranged in the pressing tool is subjected to the shaping pressure for a period of time of 0.01 to 25 seconds, preferably 0.05 to 20 seconds, preferably 0.1 to 15 seconds, particularly preferably 0.2 to 10 seconds.
[0015] A particularly preferred embodiment according to aspects of the present invention is characterized in that the pressing mold has an upper mold part and a lower mold part and wherein the upper mold part and / or the lower mold part are preferably formed as a punch. Preferably, the upper mold part is formed as a punch. Further preferably, the lower mold part is formed as a receiving element complementary to the punch. The deformation pressure for pressurizing the at least one nonwoven fabric in the pressing mold is suitably the pressure of the punch acting on or pressing the nonwoven fabric arranged in the pressing mold. When the pressing mold is temperature-controlled according to a preferred embodiment, the upper mold part and / or the lower mold part, preferably the upper mold part and the lower mold part, are preferably temperature-controlled.
[0016] It is particularly preferred within the scope of the present invention that the at least one spinning nozzle is a meltblown spinning nozzle, wherein preferably there are at least two, especially two spinning nozzles or meltblown spinning nozzles, so that it is particularly preferred to produce at least two, especially two filament-air streams containing continuous filaments and merge with the at least one short fiber-air stream in the contact zone. When the one or more spinning nozzles are formed as meltblown spinning nozzles according to a preferred embodiment, molten plastic filaments (meltblown continuous filaments) are produced by these meltblown spinning nozzles and extruded into a fast blowing airflow. Blowing air also suitably leaves from the corresponding meltblown spinning nozzle and is preferably warm or hot blowing air at this. Then the filament-air stream formed by the continuous filaments produced and the blowing air preferably flows from the at least one meltblown spinning nozzle or these meltblown spinning nozzles in the direction of the short fiber-air stream and / or in the direction of the web laying conveyor.
[0017] A preferred embodiment of the present invention is characterized in that the at least one meltblown spinning nozzle is formed as a single-row nozzle, the single-row nozzle having a plurality of nozzle openings arranged in a single row and preferably having two air inflow gaps extending on both sides parallel to the nozzle opening row and particularly inclined in the direction of the nozzle opening, from which the blow leaves. Suitably, the at least two, particularly the two meltblown spinning nozzles are formed in this way. It is also possible that at least one, preferably at least two, particularly the two meltblown spinning nozzles of the meltblown spinning nozzles are formed as a multi-row nozzle, wherein there are a plurality of nozzle openings arranged in a plurality of rows, wherein preferably each nozzle opening is assigned an (own) air inflow opening, from which the blow leaves.
[0018] According to a preferred embodiment of the present invention, the continuous filaments produced flow as a (first) filament-air stream with an initial volume flow rate V2 from the at least one spinning nozzle or meltblown spinning nozzle in the direction of the short fiber-air stream and / or in the direction of the web laying conveyor. When at least two spinning nozzles or meltblown spinning nozzles are provided according to a preferred embodiment, a second filament-air stream with an initial volume flow rate V3 particularly preferably flows from the second spinning nozzle or meltblown spinning nozzle in the direction of the short fiber-air stream and / or in the direction of the web laying conveyor. The initial volume flow rate V2 or V3 here refers in particular to the volume flow rate of the filament-air stream directly or immediately below the corresponding spinning nozzle or meltblown spinning nozzle after air, in particular blowing, is applied to the continuous filaments.
[0019] The at least one staple fiber air flow expediently flows with an initial volume flow rate V1 in the direction of the web laying conveyor device and / or in the direction of the at least one filament air flow. The initial volume flow rate V1 then refers in particular to the volume flow that is present directly or immediately after leaving the staple fiber generating device. It has proven to be useful that in the web laying area of the continuous filament-staple fiber mixture, air or process air is sucked through the web laying conveyor device, in particular through the web laying screen belt, preferably through a breathable web laying screen belt, with a volume flow rate V4. For this purpose, at least one suction device, in particular an exhaust fan, is expediently arranged below the web laying conveyor device, in particular below the web laying area. A preferred embodiment of the method according to the invention is characterized in that the volume flow rate V4 sucked through the web laying conveyor device is greater than the sum of the volume flows V1 and V2, so that the following formula holds: V4>(V1+V2). When there are at least two spinning nozzles or melt-blown spinning nozzles, it is particularly preferred that the volume flow rate V4 is greater than the sum of the volume flows V1, V2 and V3, so that the following formula is preferably established: V4>(V1+V2+V3). A particularly preferred embodiment of the method according to the present invention corresponds to a volume flow rate V4 between 1.05 and 30 times, preferably between 5 and 25 times, preferably between 10 and 20 times, of the sum V1+V2 and / or the sum V1+V2+V3. Within the scope of the method according to the present invention, by this special flow ratio, a particularly good thorough mixing of staple fibers and continuous filaments and a favorable uniformity of the distribution of continuous filaments and staple fibers in the laid nonwoven fabric and in the molded part can be achieved. Thus, the proportion of required continuous filaments can be further reduced and the molded part still meets all requirements.
[0020] In other cases, it has proven useful if, in the case of two spinning nozzles, in particular meltblowing spinning nozzles, a first filament-air stream flows in the conveying direction F of the laying conveyor before the short fiber-air stream and a second filament-air stream expediently flows after the short fiber-air stream in the conveying direction F of the laying conveyor. The short fiber-air stream is then arranged in particular centrally between the two filament-air streams.
[0021] According to a preferred embodiment of the method according to the invention, the filament-air stream hits the at least one short fiber-air stream in the contact zone at an acute angle α1, preferably at an angle α1 of 10° to 80°, preferably 20° to 75°, particularly preferably 30° to 65° and / or the second filament-air stream hits the at least one short fiber-air stream in the contact zone at an acute angle α2, preferably at an angle α2 of 10° to 80°, preferably 20° to 75°, particularly preferably 30° to 65°. Angles α1 and α2 here refer in particular to the angle formed by the flow direction or flow vector of the short fiber-air stream (S1) and the corresponding filament-air stream (S2 or S3) in or shortly before the contact zone, and also represent the angle of inclination of the filament-air stream hitting the short fiber-air stream in the contact zone.
[0022] According to a preferred embodiment of the present invention, the at least one filament-air stream, in particular the two filament-air streams, in their flow direction S2 or S3 along the entire flow path - in particular linearly or substantially linearly - flows from the corresponding spinning nozzle, in particular the meltblowing spinning nozzle, at an angle α1 or α2 relative to the flow direction S1 of the short fiber-air stream to the contact zone. Within the scope of the present invention, the one or more filament-air streams flow at an angle α1 or α2 relative to the flow direction S1 of the short fiber-air stream in their flow direction S2 or S3, in particular, means that the flow vector of the filament-air stream extends at least partially or segmentally at an angle α1 or α2 relative to the flow vector of the short fiber-air stream. Within the scope of the present invention, the terms "flow direction" and "flow vector" refer in particular to the average flow direction or average flow vector of the corresponding material flow.
[0023] It has proven to be useful that the angles α1 and α2 have the same value, so that the two filament-air streams hit the short fiber-air stream, which is arranged in the center, preferably symmetrically on both sides in the contact zone. The short fiber-air stream preferably flows perpendicularly or substantially perpendicularly to the surface of the laying conveyor in terms of its flow direction S1. Within the scope of the present invention, this means in particular that the flow vector of the short fiber-air stream extends perpendicularly or substantially perpendicularly to the planar extension of the surface of the laying conveyor. The basis for the embodiment in which the filament-air stream hits the short fiber-air stream at the angles α1 and α2 in the contact zone is the following recognition: with these angles, a particularly optimized and thorough mixing of continuous filaments and short fibers in the contact zone can be achieved, and particularly preferably, a uniform or substantially uniform continuous filament-short fiber mixture can be laid on the laying screen belt as a nonwoven fabric or a fiber web. This thorough mixing of continuous filaments and short fibers is further improved when, according to a very particularly preferred embodiment, the angles α1 and α2 have the same value. Advantageously, the continuous filament-staple fiber mixture flows in its flow direction from the contact zone to the laying wire belt perpendicularly or essentially perpendicularly to the laying wire conveyor surface.
[0024] Within the scope of the present invention, the at least one spinning nozzle or meltblown spinning nozzle, preferably the at least two, especially the two meltblown spinning nozzles, are arranged at an inclined angle relative to the short fiber generating device, especially relative to the outlet channel of the short fiber generating device. The inclination angle between the spinning nozzle, especially the meltblown spinning nozzle and the short fiber generating device or the outlet channel of the short fiber generating device is suitably (respectively) 10° to 80°, preferably 20° to 75°, particularly preferably 30° to 65°. In this way, the filament-air flow can flow from the spinning nozzle, especially from the meltblown spinning nozzle, in the direction of the short fiber-air flow at an angle α1 or α2 relative to the flow direction S1 of the short fiber-air flow. It is recommended that the inclination angle between the spinning nozzle and the outlet channel is respectively adjustable.
[0025] According to a preferred embodiment of the present invention, continuous filaments are produced from at least one thermoplastic polymer. Preferably, continuous filaments are produced from at least one polyolefin, preferably from polypropylene and / or polyethylene, particularly preferably from polypropylene. According to another preferred embodiment, continuous filaments are produced from at least one polyester, preferably from polylactic acid and / or polyethylene terephthalate, particularly preferably from polylactic acid. According to another preferred embodiment of the present invention, continuous filaments are produced from polyvinyl alcohol. In principle, continuous filaments can also be produced from other thermoplastic polymers, for example from polyamides and from mixtures of the above-mentioned thermoplastic polymers. According to a preferred embodiment of the present invention, within the scope of the method according to the present invention, the at least one nonwoven fabric is heated to a temperature lower than the melting temperature of the at least one thermoplastic polymer of the continuous filaments. It is recommended that the continuous filaments have an average filament diameter of 0.2 to 15 μm, preferably 0.5 to 12 μm and preferably 0.5 to 10 μm. The continuous filaments are very particularly preferably melt-blown continuous filaments.
[0026] According to a preferred embodiment of the present invention, continuous filaments are produced by at least one biodegradable thermoplastic polymer, preferably by polylactic acid and / or polyvinyl alcohol. In other cases, it has been proven useful that the continuous filaments are composed of the aforementioned and above-mentioned thermoplastic polymers or mixtures thereof or are essentially composed of them.
[0027] According to the invention, at least one short fiber generating device is used to produce at least one short fiber-air stream comprising short fibers. Preferably, the at least one short fiber generating device is formed in the form of a fiberizing device, wherein the short fibers of the at least one short fiber-air stream are generated in the short fiber generating device or in the fiberizing device, wherein the short fiber-air stream is preferably guided through an outlet channel and leaves the outlet channel, and wherein the short fiber-air stream particularly preferably flows perpendicularly or substantially perpendicularly to the surface of the web laying conveyor from the outlet channel or from the end of the outlet channel. According to a particularly preferred embodiment, the short fiber-air stream leaves the outlet channel with an initial volume flow rate V1 and flows in the direction of the web laying conveyor with a flow direction S1. The outlet channel is preferably part of the short fiber generating device, in particular the fiberizing device. The initial volume flow rate V1 then preferably refers to the volume flow rate of the short fiber-air stream directly or immediately after leaving the outlet channel. Preferably, the fiberizing device is a saw blade grinder.
[0028] It has proven useful that the produced short fiber air flow is accelerated in the outlet channel, in particular by a fan of the short fiber generating device or the fiberizing device. Therefore, according to a preferred embodiment, the short fiber generating device has a fan for feeding air into the device. Within the scope of the invention, the air flow for generating the short fiber air flow in the short fiber generating device or the fiberizing device is generated by a fiberizing process and / or by a fan. The short fiber air flow accelerated in the outlet channel then preferably leaves the outlet channel with an initial volume flow rate V1.
[0029] Preferably, the staple fiber air stream leaves the staple fiber generating device, in particular the outlet channel, at a ratio of 0.0138 kg to 0.0833 kg, preferably 0.0222 kg to 0.0694 kg, preferably 0.0277 kg to 0.05 kg of staple fibers per kg of air. It is also preferred that the at least one filament air stream or the plurality of filament air streams (respectively) leave the spinning nozzle, in particular the meltblown spinning nozzle, at a ratio of 0.002 kg to 0.5 kg, preferably 0.01 kg to 0.25 kg, preferably 0.015 kg to 0.12 kg, particularly preferably 0.018 kg to 0.1 kg of continuous filaments per kg of air.
[0030] According to a preferred embodiment of the method of the present invention, the staple fibers of at least one nonwoven fabric or at least one layer of the nonwoven fabric are produced from natural fibers. Then, the staple fibers are natural staple fibers. Within the scope of the present invention, natural fibers or natural staple fibers refer in particular to fibers or staple fibers formed from renewable raw materials. Preferably, the staple fibers of at least one nonwoven fabric or at least one layer of the nonwoven fabric are produced from cellulose. Very particularly preferably, the staple fibers of at least one nonwoven fabric or at least one layer of the nonwoven fabric are produced from at least one material selected from the following group: "pulp, bagasse, cellulose, bamboo, cotton, agricultural waste" and preferably from pulp. When the staple fibers are produced from pulp, the staple fibers are pulp staple fibers. Within the scope of the present invention, the term "pulp" refers in particular to a cellulose-based fibrous material. Preferably, solid pulp is used within the scope of the method according to the present invention. The expression "solid pulp" here refers in particular to a dry material based on cellulose. It is particularly preferred within the scope of the present invention to use a web formed from solid pulp and to be fiberized into pulp staple fibers by the at least one fiberizing device. The pulp used within the scope of the method according to the present invention is preferably conditioned. The short fibers, in particular pulp short fibers, produced in the at least one short fiber generating device expediently have a length or average length of 0.05 to 5 mm, preferably 0.1 to 4 mm, particularly preferably 0.1 to 3 mm.
[0031] In the scope of the present invention, the proportion of the continuous filaments in the at least one nonwoven fabric placed and / or in the molded part is 0.5% by weight to 35% by weight, preferably 1% by weight to 25% by weight, preferably 1% by weight to 15% by weight, particularly preferably 1% by weight to 10% by weight, very particularly preferably 1% by weight to 8% by weight, for example 1% by weight to 5% by weight. The basis of this embodiment is the following recognition: the molded part obtained is outstanding in that the mechanical properties and sustainability are particularly satisfactory compromises, especially in that sustainable or renewable raw materials are used. This is also particularly applicable to the situation in which the proportion of the continuous filaments in the at least one nonwoven fabric placed and / or in the molded part is in the range of 1% by weight to 10% by weight, preferably 1% by weight to 8% by weight, preferably 1% by weight to 5% by weight. Then, the molded part obtained is mainly composed of staple fibers, especially natural staple fibers, especially pulp staple fibers and is therefore similar to paper, wherein the continuous filaments still form a functionally reliable matrix for the staple fibers.
[0032] It is further preferred that the proportion of the staple fibers in the applied nonwoven and / or in the molded part is 65% to 97% by weight, preferably 70% to 95% by weight, preferably 75% to 95% by weight.
[0033] Another embodiment of the method according to the present invention is characterized in that the nonwoven fabric has at least two layers formed by a continuous filament-short fiber mixture, the layers are preferably produced simultaneously and / or successively and laid on the at least one laying conveyor device overlapping each other, wherein the continuous filament-short fiber mixture or the continuous filaments of the layer respectively form a matrix, and the short fibers are embedded in the matrix. Preferably, two fiber web production devices arranged front and back on the conveying direction F of the laying conveyor device are used to produce the two layers formed by a continuous filament-short fiber mixture from at least one spinning nozzle, preferably at least two spinning nozzles and at least one short fiber generating device. The above description is particularly similarly applicable in terms of the preferred properties of the continuous filament-short fiber mixture of the second layer. It is possible that the continuous filament-short fiber mixture of the at least two layers is different in its composition. According to another embodiment, the continuous filament-short fiber mixture of the at least two layers has the same or substantially the same composition. According to a preferred embodiment, the fiber web production device for producing the corresponding continuous filament-staple fiber mixture is arranged above the same laying conveyor device so that the at least two layers of the nonwoven fabric are laid one on top of the other on the same laying conveyor device.
[0034] It is possible that the nonwoven fabric has at least three, especially at least four layers formed by a continuous filament-staple fiber mixture, respectively, and there is a corresponding fiber web production device for producing a continuous filament-staple fiber mixture. It is also possible that the nonwoven fabric has another layer, such as a spunbond layer or a meltblown layer, produced with a corresponding spinning nozzle. Such spunbond layers and / or meltblown layers can be arranged as the last layer or as an intermediate layer between layers formed by a continuous filament-staple fiber mixture. According to one embodiment of the present invention, the nonwoven fabric only has the at least one layer, especially this layer formed by a continuous filament-staple fiber mixture, and the nonwoven fabric is therefore preferably composed of at least one continuous filament-staple fiber mixture or substantially composed of at least one continuous filament-staple fiber mixture.
[0035] Within the scope of the method according to the invention, according to a preferred embodiment, the at least one nonwoven fabric is arranged in the pressing mold so that the at least one nonwoven fabric is arranged in the pressing mold as a fiber web. Then, during or after the molding process or the pressing process, the nonwoven fabric or the molded part is suitably punched and / or cut, so that in particular a single molded part is obtained. However, according to another preferred embodiment, it is also possible to first cut the at least one nonwoven fabric from the fiber web and then arrange the at least one cut nonwoven fabric in the pressing mold. Within the scope of the present invention, arranging the at least one nonwoven fabric in the pressing mold preferably means placing the at least one nonwoven fabric or the cut nonwoven fabric in the pressing mold.
[0036] According to the preferred embodiment of the method of the present invention, in the method step separated from the production of nonwoven fabrics in place and / or time, the at least one nonwoven fabric is arranged in the pressing mold and molded into the molded part. It has been proved to be particularly useful that after being laid on the at least one web laying conveyor, the at least one nonwoven fabric is taken off from the web laying conveyor, wound into a roll and preferably in the method step separated in place and / or time, the nonwoven fabric or the roll is unwound again so as to be arranged and molded in the pressing mold. In this respect, "the method step separated in place" especially refers to that the at least one nonwoven fabric is molded into the molded part in the device separated from the fiber web production device for producing the at least one nonwoven fabric in place. This particularly preferably refers to that it does not involve the continuous method consisting of the production of nonwoven fabrics and the molding of nonwoven fabrics into the molded part immediately thereafter. However, such continuous operating mode is also within the scope of the present invention in principle. In this context, "time-separated method steps" means in particular that there is a time interval between the production of the nonwoven fabric and the molding of the at least one nonwoven fabric into the molded part, wherein this time interval can be, for example, a few minutes, such as more than 2 minutes, preferably more than 5 minutes, preferably more than 10 minutes, particularly preferably more than 15 minutes or also a few hours or days. Very particularly preferably, after laying the web on the at least one laying web conveyor device, the at least one nonwoven fabric is removed from the laying web conveyor device and wound into a roll, and if necessary, the nonwoven fabric or the roll is unwound and the nonwoven fabric is molded into a molded part.
[0037] In other cases, it is possible to further process, for example, reinforce, and / or admix at least one additive on the at least one web laying conveyor. It is also possible to further process, for example, reinforce the nonwoven fabric and / or admix at least one additive in a separate step after being removed from the at least one web laying conveyor. Within the scope of the method according to the invention, the reinforcement of the nonwoven fabric is carried out by at least one calender. The at least one calender preferably has at least one calender roller pair, through which the nonwoven fabric is guided under a pressing force. According to a particularly preferred embodiment of the method according to the invention, further processing can be carried out before the nonwoven fabric is preferably wound into a roll and / or after the nonwoven fabric or roll is unwound and preferably before the nonwoven fabric is arranged in the pressing mold, particularly preferably in the form of spraying, coating, gluing, etc., admixing the nonwoven fabric with an additive and / or preferably using a calender to reinforce the nonwoven fabric.
[0038] Preferably, at least one barrier layer in the form of a covering layer (Abschlusslage) is applied to at least one outer side of the nonwoven fabric, preferably to the two outer sides of the nonwoven fabric, wherein the covering layer is preferably a meltblown fiber web layer and / or a membrane. Therefore, when the nonwoven fabric has only one layer formed by a continuous filament-short fiber mixture, the covering layer or barrier layer can be applied to one or two outer sides of this layer of the nonwoven fabric. Therefore, when the nonwoven fabric has two layers formed by a continuous filament-short fiber mixture according to an embodiment, a barrier layer in the form of a covering layer can be applied to the outer side of one or two layers located outside the nonwoven fabric. The outer side of the nonwoven fabric particularly refers to the outer surface of the nonwoven fabric here. The nonwoven fabric obtained therefore preferably has a barrier layer in the form of a covering layer on one or two outer sides thereof. Within the scope of the present invention, the at least one barrier layer can, for example, serve as a barrier for grease and / or liquid (especially water). If the molded part according to a preferred embodiment is a food packaging, such as a food bowl for a dish, the covering layer or barrier layer can, for example, prevent grease from penetrating into the molded part when the covering layer or barrier layer faces the dish. Thus, if such a food packaging or food bowl has a covering layer or barrier layer on the side facing away from the dish, it can be avoided that grease completely penetrates the molded part, so that, for example, the user can hold the bowl in his hand without grease escaping in an undesirable manner.
[0039] Within the scope of the method according to the invention, according to one embodiment, the at least one barrier layer can be applied to the nonwoven fabric in the form of a covering layer on the at least one web laying conveyor in the fiber web production device. Then, in particular, at least one spinning nozzle, in particular at least one melt-blown spinning nozzle can be connected to the upstream and / or downstream of the at least one fiber web production device for producing a continuous filament-short fiber mixture. It is also possible that only after the nonwoven fabric is removed from the web laying conveyor, the at least one barrier layer is applied to the nonwoven fabric in the form of a covering layer. This can also be done, for example, in the pressing die. For this reason, it is preferred that a covering layer, for example in the form of a diaphragm, can be placed in the pressing die and / or placed on the nonwoven fabric arranged in the pressing die and then suitably engaged with the remaining nonwoven fabric layers during the pressing process. Therefore, the at least one nonwoven fabric preferably has a barrier layer in the form of a covering layer on one or both outer sides.
[0040] According to another preferred embodiment of the method of the present invention, at least one external boundary layer of the nonwoven fabric and / or the molded part is mixed with at least one additive for adjusting the mechanical properties and / or hydrophobic properties and / or oleophobic properties of the molded part, thereby preferably producing at least one barrier layer of the molded part. According to one embodiment of the present invention, the at least one additive can be applied to the nonwoven fabric in a fiber web production device for producing the at least one nonwoven fabric. The additive can be a finishing agent (Avivage). The external boundary layer of the nonwoven fabric and / or the molded part refers in particular to the outer part of the nonwoven fabric of the outer nonwoven fabric layer infiltrated by the additive. The at least one external boundary layer is suitably mixed with the additive on one or both outer sides of the nonwoven fabric or the molded part.
[0041] It is also possible that the nonwoven fabric is admixed with the at least one additive only after removal from the at least one laying conveyor, preferably before the nonwoven fabric is preferably wound into a roll or after the nonwoven fabric or roll is unwound. Within the scope of the method according to the invention, the at least one additive is applied, for example, by spraying the nonwoven fabric with the at least one additive, in particular in the form of a finishing agent.
[0042] It is also possible that the at least one additive is applied to at least one outer boundary layer of the molded part only after the nonwoven fabric is molded into a molded part. In this case, the additive is also applied to an outer side of the molded part or to both outer sides of the molded part. According to a preferred embodiment, at least one barrier layer of the molded part is produced by mixing at least one additive into at least one outer boundary layer of the nonwoven fabric and / or the molded part. This can be done, for example, by adjusting the hydrophobic and / or oleophobic properties of the molded part with the aid of the at least one additive, so that at least one outer boundary layer of the nonwoven fabric and / or the molded part mixed with the at least one additive has hydrophobic and / or oleophobic properties and thus also acts as a barrier for liquids (especially water) and / or grease. It is also possible within the scope of the present invention that the at least one cover layer of the nonwoven fabric forms the outer boundary layer of the nonwoven fabric or a part of this outer boundary layer, which is preferably mixed with the at least one additive.
[0043] A particularly preferred embodiment of the method according to the invention is characterized in that at least two non-woven fabrics, preferably at least three non-woven fabrics, are arranged as a non-woven fabric stack in the pressing mold, and wherein the non-woven fabric stack is heated - in particular by temperature control of the pressing mold - to a temperature in the range of 30°C to 275°C, preferably 60°C to 260°C, preferably 100°C to 250°C, and wherein the non-woven fabric stack - preferably the heated non-woven fabric stack - is subjected to a deformation pressure of at least 1 MPa, preferably 2 MPa to 40 MPa, preferably 3 MPa to 30 MPa, further preferably 4 MPa to 25 MPa, very preferably 5 MPa to 23 MPa, particularly preferably 6 MPa to 22 MPa, very particularly preferably 7 MPa to 21 MPa, for example 15 MPa to 20 MPa and is molded into a molded part. In this regard, it has proven useful to first produce the at least two non-woven fabrics separately from one another and, preferably after being laid down on a laying conveyor respectively, remove them from the laying conveyor and respectively wind them into rolls, and then - very preferably in method steps separated in place and / or time - very particularly preferably unwind the corresponding non-woven fabrics or the corresponding rolls again in order to arrange and mold them in the pressing mold and arrange the non-woven fabrics as a non-woven fabric stack in the pressing mold so as to overlap one another.
[0044] In the context of the present invention, the at least one nonwoven fabric has in particular a thickness of 0.1 to 3 mm, preferably 0.2 to 2 mm and preferably 0.3 to 1.5 mm. The thickness of the nonwoven fabric here refers in particular to the maximum thickness of the nonwoven fabric transversely, in particular perpendicularly or substantially perpendicularly to its planar extension. The thickness here particularly relates to the nonwoven fabric before the molding process to form a molding, optionally reinforced. It is further preferred that the nonwoven fabric has a thickness of 10 g / m 2 Up to 1000g / m 2 , preferably 100g / m 2 Up to 300g / m 2 Weight per unit area within the range.
[0045] In order to solve the technical problem, the present invention also teaches a molded part, in particular a molded part prepared using the above method, wherein the molded part has at least one non-woven fabric, wherein the non-woven fabric has at least one layer, in particular one layer, formed by a continuous filament-staple fiber mixture and preferably consists of or essentially consists of the continuous filament-staple fiber mixture, wherein the continuous filament-staple fiber mixture has continuous filaments and staple fibers and wherein the continuous filaments form a matrix for the staple fibers.
[0046] According to a particularly preferred embodiment, the molded part has a two-dimensional or three-dimensional structure. The molded part is preferably a container for holding and / or packaging food, for example a food bowl for a dish. According to one embodiment, the molded part according to the invention can also be a disposable tableware or a structural component for a car.
[0047] According to a preferred embodiment of the invention, at least one outer boundary layer of the molded part forms a barrier layer having a water absorption capacity of less than 300% of the mass of the at least one nonwoven, in particular the total mass of the molded part, preferably less than 30% of the mass, preferably less than 15% of the mass, very preferably less than 5% of the mass, particularly preferably less than 2.5% of the mass, very particularly preferably less than 1% of the mass and / or a grease absorption capacity of less than 300% of the mass of the at least one nonwoven, in particular the total mass of the molded part, preferably less than 30% of the mass, preferably less than 15% of the mass, very preferably less than 5% of the mass, particularly preferably less than 2.5% of the mass, very particularly preferably less than 1% of the mass, and wherein the outer boundary layer or the barrier layer is preferably biodegradable. If the molded part according to one embodiment has more than one nonwoven, for example two nonwovens, the masses relate in particular to these (the two) nonwovens. In other cases, it is also possible that the at least one covering layer forms or is part of the outer boundary layer or barrier layer, which has the water and / or grease absorption capacity given above.
[0048] According to one embodiment of the present invention, the at least one nonwoven fabric is biodegradable. According to a particularly preferred embodiment, the molded part is biodegradable. Within the scope of the present invention, "biodegradable" especially refers to that the corresponding sublayer or layer or nonwoven fabric or the entire molded part is composed of biodegradable materials. This can be achieved, for example, in the following manner: use a biodegradable thermoplastic polymer, for example polyester, especially polylactic acid and / or polyvinyl alcohol as the thermoplastic polymer for continuous filaments. In this respect, within the scope of the present invention, continuous filaments are produced by at least one biodegradable thermoplastic polymer, preferably by polylactic acid and / or polyvinyl alcohol.
[0049] The present invention is based on the following recognition: a molded part can be provided with the method according to the invention, which is distinguished by the best compromise between sustainability, especially by the use of materials based on renewable raw materials, and satisfactory mechanical properties. The molded part can be prepared by the best thorough mixing of continuous filaments and staple fibers in the continuous filament-short fiber mixture achieved within the scope of the method according to the invention, which is distinguished by an advantageously low proportion of continuous filaments and, according to a particularly preferred embodiment, by natural staple fibers, especially pulp staple fibers, in a major proportion. The continuous filaments still form a functionally reliable matrix for the staple fibers, so that the molded part also meets all requirements in terms of its mechanical properties. Nevertheless, within the scope of the method according to the invention, an unexpectedly low proportion of continuous filaments can be achieved in the molded part. When continuous filaments based on biodegradable thermoplastic polymers are used according to a preferred embodiment, it is also possible to provide a molded part that is completely or substantially completely biodegradable. It should also be emphasized that within the scope of the method according to the invention, the above advantages are achieved by less expensive measures, and in this regard, the method according to the invention is also distinguished by high economy. This is to be emphasized in particular against the background that the corresponding molded parts—for example when they are used as containers for holding and / or packaging food—are mass-produced products.
[0050] The invention will be explained in more detail below with reference to the drawing, which shows only one exemplary embodiment. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] The accompanying drawings show schematically:
[0052] Figure 1 A vertical section through a fiber web production plant for producing a nonwoven fabric within the scope of the method according to the invention is shown.
[0053] Figure 2a It is shown that according to the present invention, Figure 1 Molding process of nonwoven fabric prepared by fiber web production equipment into molded parts
[0054] Figure 2b 1. A molding process of molding a nonwoven fabric stack into a molded article according to the present invention is shown.
[0055] FIG. 2c shows a diagram of a method for using a Figure 1 A molding process in which a nonwoven fabric prepared by a fiber web production device and then cut is molded into a molded part
[0056] Figure 3a -d shows a cross section through a section of a nonwoven fabric in various embodiments before molding into a molded part.
[0057] Figure 1 A fiber web production device for preparing a nonwoven fabric 2 within the scope of the method according to the invention is shown, the nonwoven fabric having a layer 18 formed by a continuous filament-short fiber mixture 3. Suitably and in the embodiment, the continuous filaments 5 are produced by two spinning nozzles formed as melt-blown spinning nozzles 12, 13, respectively. Within the scope of the invention and in this embodiment, the continuous filaments 5 can be produced from at least one thermoplastic polymer, for example from polypropylene and / or polylactic acid. Preferably and in this embodiment, the short fibers 7 are produced with at least one short fiber production device, which is preferably and in the embodiment formed as a fiberizing device 15. The fiberizing device 15 can be a saw blade grinder in this embodiment. Suitably and in this embodiment, the short fibers 7 are natural short fibers, in particular pulp short fibers. In the short fiber production device or fiberizing device 15, preferably and in this embodiment, the short fiber-air flow 6 including the short fibers 7 is produced from pulp short fibers. The fiberizing device 15 preferably and in this embodiment has an outlet channel 16, which has an outlet channel end 17. The short fiber air flow 6 leaves the outlet channel 16 or the outlet channel end 17 of the fiberizing device 15 with an initial volume flow rate V1. In the context of the present invention, the initial volume flow rate V1 refers in particular to the volume flow rate of the short fiber air flow 6 directly or immediately after leaving the fiberizing device 15 or the outlet channel 16. The short fiber air flow 6 flows in the direction of the laid mesh belt 9 with a flow direction S1 which is preferably and in this embodiment directed perpendicularly or substantially perpendicularly to the mesh belt surface of the air-permeable laid mesh belt 9. Preferably and in this embodiment, the air-permeable laid mesh belt 9 is formed as an endless ring-shaped laid mesh belt 9.
[0058] The continuous filaments 5 produced by the meltblowing nozzles 12, 13 flow expediently and in the embodiment as filament-air streams 4, 14 with an initial volume flow rate V2 or V3 from the meltblowing nozzles 12, 13 in the direction of the staple air stream 6. The initial volume flow rate V2 or V3 here refers in particular to the volume flow rate of the filament-air streams 4, 14 directly or immediately below the meltblowing nozzles 12, 13 after the continuous filaments 5 are applied with air or blown.
[0059] Within the scope of the invention and in this embodiment, the first filament-air stream 4 flows in the conveying direction F of the laid mesh belt 9 before the short fiber-air stream 6. The filament-air stream 4 preferably and in this embodiment flows at an angle α1 with respect to the flow direction S1 of the short fiber air stream 6 in its flow direction S2. Preferably and in this embodiment, the second filament-air stream 14 flows in the conveying direction F of the laid mesh belt 9 after the short fiber-air stream 6. This second filament-air stream 14 further preferably and according to Figure 1In its flow direction S3, it flows at an angle α2 relative to the flow direction S1 of the staple air flow 6. Thus, the filament air flows 4, 14 flow into the staple air flow 6 preferably and in this embodiment from both sides of the centrally arranged staple air flow 6 at an angle α1 or α2.
[0060] Expediently and in the embodiment, the filament-air stream 4, 14 and the short fiber-air stream 6 merge in the contact zone 8 above the laying wire belt 9 and are laid as a continuous filament-short fiber mixture 3 in the laying area 24 on the laying wire belt 9 to form a nonwoven fabric 2 or a fibrous web. The continuous filaments 5 of the laid continuous filament-short fiber mixture 3 form a matrix 10 according to the invention, in which the short fibers 7 are embedded. Preferably and in this embodiment, the filament-air streams 4, 14 hit the short fiber-air stream 6 in the contact zone 8 at an acute angle α1 or α2, respectively. Very preferably and in this embodiment, the angles α1 and α2 have the same value, so that the two filament-air streams 4, 14 hit the centrally arranged short fiber-air stream 6 symmetrically on both sides in the contact zone 8. In the embodiment according to the drawings, the angles α1 and α2 can each be about 30°. The angles α1 and α2 refer here in particular to the angle formed by the flow directions or flow vectors of the staple fiber air stream (S1) and the corresponding filament air stream (S2 or S3) in or shortly before the contact zone, and therefore also represent the angle of inclination at which the filament air streams 4, 14 strike the staple fiber air stream 6 in the contact zone 8. Within the scope of the invention and in this exemplary embodiment, in the remaining cases, the two filament air streams 4, 14 flow at an angle α1 or α2 with respect to the flow direction S1 of the staple fiber air stream 6 along their entire flow path from the corresponding meltblown spinning nozzle 12, 13 to the contact zone 8 in terms of their flow direction S2 or S3.
[0061] Preferably and in accordance with Figure 1 In the embodiment of the present invention, in the laying area 24 of the continuous filament-short fiber mixture 3 on the laying screen belt 9, air or process air is sucked from below through the laying screen belt 9 with a volume flow rate V4. For this purpose, preferably and in this embodiment, a suction device 25 is arranged below the laying screen belt 9, in particular below the laying area 24. The volume flow rate V4 is preferably greater than the sum of the volume flows V1, V2 and V3 (V4>(V1+V2+V3)).
[0062] Preferably, the continuous filament-short fiber mixture 3 flows as a homogeneous or substantially homogeneous mixture from the contact zone 8 to the laying screen belt 9. The homogeneous continuous filament-short fiber mixture 3 is subsequently laid down to form a nonwoven fabric 2 or a fiber web in the laying area 24. Further preferably and in this embodiment, the continuous filament-short fiber mixture 3 flows from the contact zone 8 to the laying screen belt 9 or the laying area 24 perpendicularly or substantially perpendicularly to the screen belt surface in terms of its flow direction.
[0063] Figure 2a and Figure 2b It is shown that according to the present invention, the nonwoven fabric 2 ( Figure 2a ) or a nonwoven fabric stack 22 formed of two nonwoven fabrics 2 ( Figure 2b ) is molded into a molding process of the molded part 1. Then Figure 1 After the fiber web is produced in the fiber web production device shown in FIG, according to a preferred embodiment of the present invention, the at least one nonwoven fabric 2 is removed from the laying screen belt 9 and wound into a roll 21. The nonwoven fabric 2 or roll 21 is then suitably unwound again in order to be arranged and molded in the pressing mold 11. This can be done in Figure 2a and Figure 2b Appropriately and according to Figure 2a and Figure 2b The nonwoven fabric 2 or the nonwoven fabric stack 22 is arranged in the form of a web or in the form of a plurality of webs in a pressing mold 11. Then, preferably and according to Figure 2a and Figure 2b In the embodiment of the present invention, the nonwoven fabric 2 / nonwoven fabric stack 22 or the molded part 1 is punched and / or cut during or after the molding process or the pressing process, so that in particular individual molded parts 1 are produced. In FIG. 2 c , the molding process of the nonwoven fabric 2 according to the invention is shown, preferably and according to FIG. 2 c , the nonwoven fabric is first cut from the fiber web and then arranged in the pressing mold 11 as a cut nonwoven fabric 2.
[0064] Preferably and in accordance with Figure 2a In the embodiment of FIG. 2c , the nonwoven fabric 2 is arranged in a pressing mold 11 and heated to a temperature in the range of 30°C to 275°C, preferably 100°C to 250°C, by temperature control or heating of the pressing mold 11. The pressing mold is preferably and in this embodiment composed of an upper mold part 11a formed as a punch and a lower mold part 11b preferably and in this embodiment formed as a receiving element complementary to the punch. Then, preferably and in this embodiment, a deformation pressure of at least 1MPa, preferably 2MPa to 40MPa, is applied to the heated nonwoven fabric 2 and molded into a molded part 1. Here, “the nonwoven fabric 2 is subjected to a deformation pressure in the pressing mold 11” refers in particular to the upper mold part 11a formed as a punch acting on or pressing on the at least one nonwoven fabric 2 with a corresponding deformation pressure. This is in Figure 2a , Figure 2b and represented by arrows in Figure 2c.
[0065] In other cases, Figure 2b In the present invention, two nonwoven fabrics 2 are arranged overlapping each other as a nonwoven fabric stack 22 in a pressing mold 11. Figure 2a The heating of the nonwoven fabric stack 22 and the molding of the molded part 1 with the deformation pressure are carried out similarly to the above-mentioned method flow for a single nonwoven fabric 2 in FIG. 2c. It is possible within the scope of the present invention that the nonwoven fabric stack 22 is a stack of cut nonwoven fabrics 2. In other cases, preferably and according to Figure 2a In the embodiment of FIG. 2 c , the molded part 1 is formed as a food bowl for a dish.
[0066] Figures 3a to 3d In each case, a cross section of a section of a nonwoven fabric 2 is shown in different embodiments before being molded into a molded part 1. Figure 3a In a preferred design, the nonwoven fabric 2 is shown to have a single layer 18 formed by a continuous filament-short fiber mixture 3. The continuous filament-short fiber mixture 3 has continuous filaments 5 and short fibers 7, wherein the continuous filaments 5 form a matrix 10 for the short fibers 7. The short fibers 7 are embedded in the matrix 10.
[0067] exist Figure 3b , another preferred embodiment of the nonwoven fabric 2 is shown in which the outer boundary layer 23 is admixed with at least one additive in order to adjust the mechanical properties and / or the hydrophobicity and / or oleophobicity of the molded part. The outer boundary layer 23 of the nonwoven fabric 2 is in this case in particular the nonwoven outer part of the nonwoven fabric layer 18. Figure 3b Indicated by dotted line. Figure 3b In a preferred embodiment, the outer boundary layer 23 on the outer side of the nonwoven fabric 2 is admixed with an additive. Within the scope of the invention, after the subsequent molding step, due to the admixture of the outer boundary layer 23, a barrier layer of the molded part 1 is preferably obtained, which acts, for example, as a barrier against liquids (especially water) and / or grease.
[0068] exist Figure 3c , another preferred embodiment of a nonwoven fabric 2 is shown, which has a layer 18 formed by a continuous filament-staple fiber mixture 3. A barrier layer in the form of a cover layer 20 is applied to the outer side of the nonwoven fabric 2, wherein the cover layer 20 is preferably and in this embodiment a meltblown fiber web layer. The barrier layer in the form of a cover layer 20 can, for example, act as a barrier against liquids (especially water) and / or grease.
[0069] exist Figure 3d In FIG. 1 , another embodiment of a nonwoven fabric 2 is shown, which is formed by two layers 18, 19 each formed from a continuous filament-staple fiber mixture 3. The continuous filaments 5 of the continuous filament-staple fiber mixture 3 or layers 18, 19 respectively form a matrix 10, in which the staple fibers 7 are embedded.
[0070] appropriately and in accordance with Figures 3a to 3d In the embodiment of the present invention, the continuous filaments can be formed based on at least one thermoplastic polymer. Recommendedly and in this embodiment, the staple fibers 7 can be produced from natural fibers and preferably from pulp, so that the staple fibers are pulp staple fibers 7. The proportion of continuous filaments 5 in the at least one laid nonwoven fabric 2 is preferably 1% by weight to 8% by weight and in this embodiment can be 5% by weight, for example.
Claims
1. A method for producing a molded part (1) from at least one nonwoven fabric (2), wherein the at least one nonwoven fabric (2) has at least one, in particular one, layer (18) of a continuous filament-staple fiber mixture (3), wherein at least one filament-air stream (4) comprising continuous filaments (5) is generated by at least one spinning nozzle and at least one staple fiber-air stream (6) comprising staple fibers (7) is generated by at least one staple fiber generating device, wherein the at least one filament-air stream (4) and the at least one staple-air stream (6) are combined in a contact zone (8) and subsequently laid as a continuous filament-staple fiber mixture (3) on at least one laying conveyor, in particular at least one laying screen belt (9) to form a nonwoven fabric (2) or a fiber web, wherein the continuous filaments (5) of the continuous filament-staple fiber mixture (3) laid on the laying conveyor form a matrix (10) in which the staple fibers (7) are embedded, The at least one nonwoven fabric (2) is arranged in a pressing mold (11), the nonwoven fabric (2) being heated—in particular by temperature control of the pressing mold (11)—to a temperature in the range of 30° C. to 275° C., preferably 60° C. to 260° C., preferably 100° C. to 250° C., and the nonwoven fabric (2)—preferably the heated nonwoven fabric (2)—being subjected to a deformation pressure of at least 1 MPa, preferably 2 MPa to 40 MPa, preferably 3 MPa to 30 MPa, further preferably 4 MPa to 25 MPa, very preferably 5 MPa to 23 MPa, particularly preferably 6 MPa to 22 MPa, very particularly preferably 7 MPa to 21 MPa, for example 15 MPa to 20 MPa, and being molded into a molded part (1).
2. The method according to claim 1, wherein the pressing tool (11) has an upper tool part (11a) and a lower tool part (11b) and wherein the upper tool part (11a) and / or the lower tool part (11b) are preferably formed as a punch.
3. A method according to one of claims 1 or 2, wherein the at least one spinning nozzle is a meltblowing spinning nozzle (12), wherein preferably there are at least two, in particular two spinning nozzles or meltblowing spinning nozzles (12, 13), so that at least two, in particular two filament-air streams (4, 14) containing continuous filaments (5) are particularly preferably generated and merged with the at least one short fiber-air stream (6) in the contact zone (8).
4. A method according to any one of claims 1 to 3, wherein the filament-air flow (4) hits the at least one short fiber-air flow (6) in the contact zone (8) at an acute angle α1, preferably at an angle α1 of 10° to 80°, preferably 20° to 75°, and particularly preferably 30° to 65° and / or wherein the second filament-air flow (14) hits the at least one short fiber-air flow (6) in the contact zone (8) at an acute angle α2, preferably at an angle α2 of 10° to 80°, preferably 20° to 75°, and particularly preferably 30° to 65°.
5. The method according to claim 4, wherein the angles α1 and α2 have the same value so that the two filament air flows (4, 14) in the contact zone (8) preferably hit the short fiber air flow (6) arranged in the center symmetrically on both sides.
6. The method according to any one of claims 1 to 5, wherein the continuous filaments (5) are produced from at least one thermoplastic polymer, preferably from at least one polyolefin, preferably from polypropylene and / or polyethylene, particularly preferably from polypropylene.
7. The method according to any one of claims 1 to 6, wherein the continuous filaments (5) are produced from at least one thermoplastic polymer, preferably from at least one polyester, preferably from polylactic acid and / or polyethylene terephthalate, particularly preferably from polylactic acid and / or wherein the continuous filaments are produced from polyvinyl alcohol.
8. A method according to any one of claims 1 to 7, wherein the at least one short fiber generating device is formed in the form of a fiberizing device (15), wherein the short fibers (7) of the at least one short fiber-air flow (6) are generated in the short fiber generating device or in the fiberizing device (15), wherein the short fiber-air flow (6) is preferably guided through an outlet channel (16) and leaves the outlet channel, and wherein the short fiber-air flow (6) particularly preferably flows from the outlet channel (16) or from the outlet channel end (17) perpendicularly or substantially perpendicularly to the surface of the laying conveying device.
9. The method according to any one of claims 1 to 8, wherein the staple fibers (7) of the at least one nonwoven fabric (2) or at least one layer (18) of the nonwoven fabric (2) are produced from natural fibers, preferably from at least one material selected from the group consisting of "pulp, bagasse, cellulose, bamboo, cotton, agricultural waste", and preferably from pulp.
10. The method according to any one of claims 1 to 9, wherein the proportion of the continuous filaments (5) in at least one laid nonwoven fabric (2) and / or in the molded part (1) is 0.5% to 35% by weight, preferably 1% to 25% by weight, preferably 1% to 15% by weight, particularly preferably 1% to 10% by weight, very particularly preferably 1% to 8% by weight, for example 1% to 5% by weight.
11. The method according to any one of claims 1 to 10, wherein the proportion of the short fibers (7) in the deposited nonwoven fabric (2) and / or in the molded part (1) is 65% to 97% by weight, preferably 70% to 95% by weight, preferably 75% to 95% by weight.
12. A method according to any one of claims 1 to 11, wherein the nonwoven fabric (2) has at least two layers (18, 19) each formed by a continuous filament-staple fiber mixture (3), the layers being preferably produced simultaneously and / or successively and laid overlapping each other on the at least one laying conveyor device, wherein the continuous filament-staple fiber mixture (3) or the continuous filaments (5) of the layers (18, 19) respectively form a matrix (10), and the staple fibers (7) are embedded in the matrix.
13. A method according to any one of claims 1 to 12, wherein after laying the web on at least the web laying conveyor, the at least one non-woven fabric (2) is removed from the web laying conveyor, wound into a roll (21) and the non-woven fabric (2) or the roll (21) is unwound again in a method step preferably separated in place and / or time in order to be arranged and molded in a pressing mold (11).
14. The method according to any one of claims 1 to 13, wherein at least one barrier layer in the form of a covering layer (20) is applied to at least one outer side of the non-woven fabric (2), preferably to both outer sides of the non-woven fabric (2), wherein the covering layer (20) is preferably a meltblown non-woven fabric fiber web layer and / or a membrane sheet.
15. A method according to any one of claims 1 to 14, wherein at least one additive for adjusting the mechanical properties and / or hydrophobic properties and / or oleophobic properties of the molded part (1) is admixed into at least one outer boundary layer (23) of the nonwoven fabric (2) and / or the molded part (1), thereby preferably producing at least one barrier layer of the molded part (1).
16. A method according to any one of claims 1 to 15, wherein at least two non-woven fabrics (2), preferably at least three non-woven fabrics (2) are arranged as a non-woven fabric stack in the pressing mold (11), and wherein the non-woven fabric stack (22) - in particular by temperature control of the pressing mold (11) - is heated to a temperature in the range of 30°C to 275°C, preferably 60°C to 260°C, preferably 100°C to 250°C, and wherein the non-woven fabric stack (22) - preferably the heated non-woven fabric stack (22) - is applied with a deformation pressure of at least 1 MPa, preferably 2 MPa to 40 MPa, preferably 3 MPa to 30 MPa, further preferably 4 MPa to 25 MPa, very preferably 5 MPa to 23 MPa, particularly preferably 6 MPa to 22 MPa, very particularly preferably 7 MPa to 21 MPa, for example 15 MPa to 20 MPa and is molded into a molded part (1).
17. A molded part, in particular a molded part prepared according to the method according to any one of claims 1 to 16, wherein the molded part (1) has at least one non-woven fabric (2), wherein the non-woven fabric (2) has at least one, in particular one, layer (18) formed by a continuous filament-staple fiber mixture (3) and preferably consists of or essentially consists of the continuous filament-staple fiber mixture (3), wherein the continuous filament-staple fiber mixture (3) has continuous filaments (5) and staple fibers (7) and wherein the continuous filaments (5) form a matrix (10) for the staple fibers (7).
18. The molded part according to claim 17, wherein the molded part (1) has a two-dimensional or three-dimensional structure.
19. A moulding according to any one of claims 17 or 18, wherein at least one outer boundary layer (23) of the moulding (1) forms a barrier layer, the barrier layer having a water absorption capacity of less than 300%, preferably less than 30%, preferably less than 15%, very preferably less than 5%, particularly preferably less than 2.5%, very particularly preferably less than 1% of the mass of the at least one non-woven fabric (2), in particular the total mass of the moulding (1) and / or having a grease absorption capacity of less than 300%, preferably less than 30%, preferably less than 15%, very preferably less than 5%, particularly preferably less than 2.5%, very particularly preferably less than 1% of the mass of the at least one non-woven fabric (2), in particular the total mass of the moulding (1), and wherein the outer boundary layer (23) or the barrier layer is preferably biodegradable.
20. The molded part according to any one of claims 17 to 19, wherein the molded part (1) is biodegradable.