A silicon carbide power device and its preparation method and application
By combining semi-insulated silicon carbide single crystal substrate and laser scanning technology in silicon carbide power devices, the reuse of substrates is achieved, solving the problems of high manufacturing cost and on-resistance of silicon carbide power devices, and improving the device performance and application potential.
Patent Information
- Application Number
- CN202411296352.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-18
AI Technical Summary
The high manufacturing costs and on-resistance of existing silicon carbide power devices limit their large-scale applications, and traditional thinning processes have problems with wear, lattice damage and process complexity.
The semi-insulated silicon carbide single crystal substrate is used for homoequitaxial and device preparation, and the substrate is stripped by laser scanning technology to achieve reuse of the semi-insulated silicon carbide substrate, reducing the on-resistance and manufacturing cost of the device.
Through the reuse of semi-insulated silicon carbide substrates, the on-resistance and manufacturing cost of silicon carbide power devices are reduced, the current density is improved, and the large-scale application of silicon carbide power electronic devices is promoted.
Smart Images

Figure CN118824845B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a silicon carbide power device and a preparation method and application thereof. Background Art
[0002] As a wide bandgap semiconductor material, silicon carbide has the advantages of high critical breakdown electric field strength, high saturated electron mobility, and high thermal conductivity, and has great material advantages in the field of power electronic devices. There are already mature products of 650 V~1200 V silicon carbide Schottky diodes and metal oxide field effect transistors, but the main factor limiting the large-scale application of silicon carbide power electronic devices is the high manufacturing cost. Silicon carbide power devices are usually vertical structures, in which the n-type doped silicon carbide single crystal substrate is the device carrier, with a thickness of 350 μm~500 μm and a resistivity of about 20 mcm. On the one hand, the substrate resistance accounts for half of the device on-resistance, limiting the forward current conduction capability of the device; on the other hand, the n-type doped silicon carbide single crystal substrate accounts for 60% of the manufacturing cost of silicon carbide power devices, limiting the cost reduction of silicon carbide power devices.
[0003] Existing silicon carbide power devices all use a vertical structure with n-type silicon carbide single crystal as the substrate. The substrate resistance is an important component of the device on-resistance. Therefore, in order to reduce the device on-resistance, the silicon carbide device substrate needs to be thinned. The substrate thinning processes include back grinding thinning, ion implantation stripping, and laser thinning, but these processes have the following disadvantages:
[0004] The use of a grinding device to thin the n-type silicon carbide single crystal substrate results in high wear and tear, resulting in waste of the substrate. In addition, the grinding wheel thinning process requires spin coating and grinding of a protective film on the front side of the n-type silicon carbide, which increases the process steps.
[0005] Ion implantation thinning of n-type silicon carbide single crystal substrate requires ion implantation and high-temperature annealing processes, which causes significant lattice damage and complex processes.
[0006] The laser thinning process of n-type silicon carbide single crystal substrate requires bonding of glass sheets on the front and back sides of the silicon carbide device, and then using laser to separate the n-type silicon carbide single crystal substrate. After separation, the surface of the silicon carbide separation is rough and needs surface treatment, and the process is complicated;
[0007] After thinning, the thickness of the n-type silicon carbide substrate is still around 100 μm to 150 μm, and the stress is very large;
[0008] Therefore, it is necessary to propose a method for preparing a silicon carbide power device that reduces the manufacturing cost of the silicon carbide power device and improves the forward current conduction capability of the silicon carbide power device. Summary of the invention
[0009] In view of the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a silicon carbide power device and a preparation method and application thereof. The present invention selects a semi-insulating silicon carbide single crystal as a substrate, carries out homoepitaxial growth, device preparation, substrate stripping and other processes, so as to achieve the purpose of reusing the semi-insulating silicon carbide single crystal substrate, reduce the wafer warping and stress of the silicon carbide homoepitaxial layer, reduce the on-resistance and manufacturing cost of the device, and promote the large-scale application of silicon carbide power electronic devices.
[0010] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0011] A method for preparing a silicon carbide power device comprises the following steps:
[0012] A semi-insulating silicon carbide single crystal substrate is used as a substrate, an n-type silicon carbide single crystal epitaxial layer is grown on the silicon surface of the semi-insulating silicon carbide single crystal substrate, a silicon carbide device structure is prepared on the silicon surface of the n-type silicon carbide single crystal epitaxial layer, and then a photoresist is spin-coated on the silicon carbide device structure to protect the device structure on the front side;
[0013] By means of laser scanning, a modified layer is formed at the interface between the n-type silicon carbide single crystal epitaxial layer and the semi-insulating silicon carbide single crystal substrate, and the semi-insulating silicon carbide single crystal substrate is peeled off;
[0014] Ohmic contact metal is deposited on the carbon surface of the n-type silicon carbide single crystal epitaxial layer, and laser annealing is performed to prepare the ohmic contact of the device. Then, thick metallic silver is deposited on the ohmic contact metal. The purpose of depositing metallic silver is to thicken the metal and to combine the device with the packaging material.
[0015] With the help of laser scanning, the ohmic contact metal and the silver metal are laser ablated and sublimated to form grooves, separating the ohmic contact metal and the silver metal on the back side of the silicon carbide device structure;
[0016] The photoresist on the silicon carbide device structure is removed, and the conductive silicon carbide is laser-modified by means of laser scanning to form a void layer in the conductive silicon carbide and separate the silicon carbide device.
[0017] The present invention adopts a semi-insulating silicon carbide single crystal substrate as a substrate, grows an n-type silicon carbide single crystal epitaxial layer on the silicon surface of the semi-insulating single crystal substrate, and then prepares a silicon carbide device structure on the silicon surface of the n-type silicon carbide single crystal epitaxial layer. The semi-insulating silicon carbide substrate is colorless and transparent, and the n-type silicon carbide single crystal is green, and there is an obvious interface between the two. Then, the semi-insulating silicon carbide single crystal substrate is peeled off with the help of laser scanning. The n-type silicon carbide single crystal epitaxial layer after peeling is less damaged, and the semi-insulating silicon carbide single crystal substrate can be reused. Ohmic contact metal is deposited on the carbon surface of the n-type silicon carbide single crystal epitaxial layer, and laser annealing is performed to prepare the ohmic contact of the device. Then, conductive metal is deposited on the ohmic contact metal. Finally, laser scanning is used to separate the metal and photoresist on the back of the silicon carbide device structure, and the silicon carbide device is separated, thereby reducing the wafer warpage and stress of the silicon carbide homoepitaxial layer, completely eliminating the on-resistance and on-loss of the conductive silicon carbide single crystal substrate, and reducing the manufacturing cost.
[0018] In a preferred embodiment of the present invention, the ohmic contact metal is nickel or nickel-titanium alloy.
[0019] In a preferred embodiment of the present invention, the thickness of the nickel or nickel-titanium alloy deposition is 50 nm to 100 nm.
[0020] In a preferred embodiment of the present invention, the thickness of the semi-insulating silicon carbide single crystal substrate is 350 μm to 500 μm, and the thickness of the n-type silicon carbide single crystal epitaxial layer is 10 μm to 100 μm.
[0021] In a preferred embodiment of the present invention, the laser annealing temperature is 900° C. to 1000° C., and the annealing time is 1 min to 10 min.
[0022] In a preferred embodiment of the present invention, when peeling off the semi-insulating silicon carbide single crystal substrate and separating the silicon carbide device, the laser scanning parameters are: laser wavelength 1064 nm, frequency 100 kHz~500 kHz, pulse width 100 fs~5000 fs, scanning speed 100 mm / s~1000 mm / s.
[0023] In a preferred embodiment of the present invention, when separating the metal on the back side of the silicon carbide device, the laser scanning parameters are: laser wavelength 355 nm, frequency 1 kHz~500 kHz, pulse width 100 fs~5000 fs, and scanning speed 100 mm / s~1000 mm / s.
[0024] Another object of the present invention is to provide a silicon carbide power device produced by any of the above-mentioned preparation methods.
[0025] In a preferred embodiment of the present invention, the silicon carbide power device includes an n-type silicon carbide single crystal epitaxial layer, the n-type silicon carbide single crystal epitaxial layer includes a carbon surface and a silicon surface, a silicon carbide device structure is arranged on the silicon surface of the n-type silicon carbide single crystal epitaxial layer, an ohmic contact metal is deposited on the silicon surface of the n-type silicon carbide single crystal epitaxial layer, and metallic silver is deposited on the ohmic contact metal.
[0026] The third object of the present invention is to provide an application of the above-mentioned silicon carbide power device in the manufacture of silicon carbide power electronic devices.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. The main factor limiting the large-scale application of silicon carbide power electronic devices is the high manufacturing cost. The present invention proposes a low-cost silicon carbide power electronic device preparation process, which selects semi-insulating silicon carbide single crystal as a substrate, carries out homoepitaxial growth, device preparation, substrate stripping and other processes, so as to achieve the purpose of reusing the semi-insulating silicon carbide single crystal substrate, reduce the wafer warpage and stress of the silicon carbide homoepitaxial layer, reduce the on-resistance and manufacturing cost of the device, and promote the large-scale application of silicon carbide power electronic devices.
[0029] 2. The present invention adopts a semi-insulating silicon carbide substrate to prepare silicon carbide power devices. Since semi-insulating silicon carbide is colorless and transparent, and conductive silicon carbide is green, there is an obvious interface between the semi-insulating silicon carbide and the conductive silicon carbide. The laser lift-off technology makes it easier to separate the semi-insulating silicon carbide from the epitaxially grown conductive silicon carbide. The conductive silicon carbide is less damaged after lift-off, and the semi-insulating silicon carbide single crystal substrate can be reused. The silicon carbide power device prepared by the method of the present invention completely eliminates the on-resistance and conduction loss of the conductive silicon carbide single crystal substrate.
[0030] 3. In the process of preparing the silicon carbide power device of the present invention, the semi-insulating silicon carbide single crystal substrate can be reused, thereby reducing the preparation cost of the silicon carbide power device. The technical process of the present invention improves the current density of the silicon carbide power device, reduces the on-resistance of the device, and reduces the conduction loss of the device by eliminating the n-type silicon carbide single crystal substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The figure shows an n-type silicon carbide single crystal epitaxial layer grown on a semi-insulating silicon carbide single crystal substrate of the present invention.
[0032] Figure 2 This is a diagram of a device prepared on a silicon carbide wafer of the present invention.
[0033] Figure 3 A diagram of a device in which a photoresist is coated on the front side of the silicon carbide device of the present invention to protect the device.
[0034] Figure 4 This is a diagram of peeling off the epitaxial layer of the semi-insulating silicon carbide single crystal and the n-type silicon carbide single crystal of the present invention.
[0035] Figure 5 This is a diagram of a silicon carbide device after the substrate is peeled off according to the present invention.
[0036] Figure 6 This is the ohmic contact diagram on the back of the silicon carbide device of the present invention.
[0037] Figure 7 This is a diagram of the metal thickening on the back of the silicon carbide device of the present invention.
[0038] Figure 8 This is a diagram of the back metal separation of the silicon carbide device of the present invention.
[0039] Fig. 9 This is a diagram of removing the photoresist and separating the devices according to the present invention.
[0040] Description of the drawings: 1-semi-insulating silicon carbide single crystal substrate; 2-n-type silicon carbide single crystal epitaxial layer; 3-silicon carbide device structure; 4-photoresist; 5-first laser; 6-first optical element; 7-ohmic contact metal; 8-metal silver; 9-second laser; 10-second optical element; 11-third laser; 12-third optical element. DETAILED DESCRIPTION
[0041] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0043] Example 1
[0044] A method for preparing a silicon carbide power device comprises the following steps:
[0045] A 350 μm thick semi-insulating silicon carbide single crystal substrate 1 is used as a substrate, and its resistivity is 1E12 Ω·cm. On the silicon surface of the semi-insulating silicon carbide single crystal substrate 1, an n-type silicon carbide single crystal epitaxial layer 2 is grown by chemical vapor deposition. The epitaxial layer has a thickness of 12 μm and a doping concentration of 1E16 cm-3 ,like Figure 1 FIG. 2 shows a diagram of growing an n-type silicon carbide single crystal epitaxial layer on a semi-insulating silicon carbide single crystal substrate; a silicon carbide device structure 3 is prepared on the silicon surface of the n-type silicon carbide single crystal epitaxial layer 2, as shown in FIG. Figure 2 The figure shows a device fabricated on a silicon carbide wafer; a photoresist 4 is spin-coated on the silicon carbide device structure 3, and the thickness of the photoresist 4 is 10 μm, which is used to protect the device structure on the front side. Figure 3 Shown is a photo of a silicon carbide device with photoresist coated on the front to protect the device.
[0046] like Figure 4 FIG. 1 is a diagram showing the peeling of a semi-insulating silicon carbide single crystal and an n-type silicon carbide single crystal epitaxial layer. By means of laser scanning, the laser scanning includes a first laser 5 and a first optical element 6. A modified layer is formed at the interface between the n-type silicon carbide single crystal epitaxial layer 2 and the semi-insulating silicon carbide single crystal substrate 1, and the semi-insulating silicon carbide single crystal substrate 1 is peeled off. Figure 5 The figure shows the silicon carbide device after substrate peeling; the laser scanning parameters are: laser wavelength 1064 nm, frequency 100 kHz, pulse width 1000 fs, scanning speed 500 mm / s.
[0047] Ohmic contact metal Ni is deposited on the carbon surface of the n-type silicon carbide single crystal epitaxial layer 2 with a thickness of 50 nm. The ohmic contact diagram of the back of the silicon carbide device is shown in the figure below. Figure 6 As shown, local laser annealing is performed in an Ar atmosphere at a temperature of 1000°C for 3 min to prepare the ohmic contact of the silicon carbide device. Thick metal silver 8 is deposited on the ohmic contact metal 7 with a thickness of 4000 nm. The metal thickening diagram of the back of the silicon carbide device is shown in FIG. Figure 7 shown.
[0048] By means of laser scanning, the laser scanning includes a second laser 9 and a second optical element 10, according to the cutting pattern designed for the device, the laser ablates the metal to sublimate to form a groove, and separates the metal on the back of the silicon carbide device. The metal powder on the back of the silicon carbide device is shown in the figure. Figure 8 As shown; the parameters of laser scanning are: laser wavelength 355 nm, frequency 200 kHz, pulse width 2000 fs, and scanning speed 600 mm / s.
[0049] Remove the photoresist on the front side of the device.
[0050] like Fig. 9The figure shows the removal of photoresist and device separation. With the help of laser scanning, the laser scanning includes a third laser 11 and a third optical element 12. According to the cutting pattern designed for the device, the conductive silicon carbide is laser modified. The parameters of the laser scanning are: laser wavelength 1064 nm, frequency 100 kHz, pulse width 1000 fs, scanning speed 500 mm / s, a void layer is formed in the conductive silicon carbide, and the silicon carbide device is separated.
[0051] Example 2
[0052] A method for preparing a silicon carbide power device comprises the following steps:
[0053] A 500 μm thick semi-insulating silicon carbide single crystal substrate 1 is used as a substrate, and its resistivity is 1E12 Ω·cm. On the silicon surface of the semi-insulating silicon carbide single crystal substrate 1, an n-type silicon carbide single crystal epitaxial layer 2 is grown by chemical vapor deposition. The epitaxial layer has a thickness of 10 μm and a doping concentration of 1E16 cm -3 A silicon carbide device structure 3 is prepared on the silicon surface of the n-type silicon carbide single crystal epitaxial layer 2, and a photoresist 4 is spin-coated on the silicon carbide device structure 3. The thickness of the photoresist 4 is 10 μm, which is used to protect the device structure on the front side.
[0054] By means of laser scanning, which includes a first laser 5 and a first optical element 6, a modified layer is formed at the interface between the n-type silicon carbide single crystal epitaxial layer 2 and the semi-insulating silicon carbide single crystal substrate 1, and the semi-insulating silicon carbide single crystal substrate 1 is peeled off; the parameters of the laser scanning are: laser wavelength 1064 nm, frequency 200 kHz, pulse width 100 fs, and scanning speed 100 mm / s.
[0055] Ohmic contact metal Ni is deposited on the carbon surface of the n-type silicon carbide single crystal epitaxial layer 2 with a thickness of 100 nm, and local laser annealing is performed in an Ar atmosphere at a temperature of 900°C for 1 min to prepare the ohmic contact of the silicon carbide device. Thick metal silver 8 is then deposited on the ohmic contact metal 7 with a thickness of 4000 nm.
[0056] With the aid of laser scanning, which includes a second laser 9 and a second optical element 10, the laser ablates the metal to sublimate and form grooves according to the cutting pattern designed for the device, thereby separating the metal on the back of the silicon carbide device; the parameters of the laser scanning are: laser wavelength 355 nm, frequency 1 kHz, pulse width 100 fs, and scanning speed 100 mm / s.
[0057] Remove the photoresist on the front side of the device.
[0058] (6) With the aid of laser scanning, the laser scanning includes a third laser 11 and a third optical element 12, and the conductive silicon carbide is laser modified according to the cutting pattern designed for the device. The parameters of the laser scanning are: laser wavelength 1064 nm, frequency 200 kHz, pulse width 100 fs, scanning speed 100 mm / s, a cavity layer is formed in the conductive silicon carbide, and the silicon carbide device is separated.
[0059] Example 3
[0060] A method for preparing a silicon carbide power device comprises the following steps:
[0061] A 400 μm thick semi-insulating silicon carbide single crystal substrate 1 is used as a substrate, and its resistivity is 1E12 Ω·cm. On the silicon surface of the semi-insulating silicon carbide single crystal substrate 1, an n-type silicon carbide single crystal epitaxial layer 2 is grown by chemical vapor deposition. The epitaxial layer has a thickness of 100 μm and a doping concentration of 1E16 cm -3 A silicon carbide device structure 3 is prepared on the silicon surface of the n-type silicon carbide single crystal epitaxial layer 2, and a photoresist 4 is spin-coated on the silicon carbide device structure 3. The thickness of the photoresist 4 is 10 μm, which is used to protect the device structure on the front side.
[0062] By means of laser scanning, which includes a first laser 5 and a first optical element 6, a modified layer is formed at the interface between the n-type silicon carbide single crystal epitaxial layer 2 and the semi-insulating silicon carbide single crystal substrate 1, and the semi-insulating silicon carbide single crystal substrate 1 is peeled off; the parameters of the laser scanning are: laser wavelength 1064 nm, frequency 500 kHz, pulse width 5000 fs, and scanning speed 1000 mm / s.
[0063] Ohmic contact metal Ni is deposited on the carbon surface of the n-type silicon carbide single crystal epitaxial layer 2 with a thickness of 80 nm, and local laser annealing is performed in an Ar atmosphere at a temperature of 950°C for 10 min to prepare the ohmic contact of the silicon carbide device. Thick metal silver 8 is further deposited on the ohmic contact metal 7 with a thickness of 4000 nm.
[0064] With the aid of laser scanning, which includes a second laser 9 and a second optical element 10, the laser ablates the metal to sublimate and form grooves according to the cutting pattern designed for the device, thereby separating the metal on the back of the silicon carbide device; the parameters of the laser scanning are: laser wavelength 355 nm, frequency 500 kHz, pulse width 5000 fs, and scanning speed 1000 mm / s.
[0065] Remove the photoresist on the front side of the device.
[0066] (6) With the aid of laser scanning, the laser scanning includes a third laser 11 and a third optical element 12, and the conductive silicon carbide is laser modified according to the cutting pattern designed for the device. The parameters of the laser scanning are: laser wavelength 1064 nm, frequency 500 kHz, pulse width 5000 fs, scanning speed 1000 mm / s, to form a void layer in the conductive silicon carbide and separate the silicon carbide device.
[0067] The on-resistance of the existing 1200 V SiC metal oxide field effect transistor (SiC MOSFET) is 80 mΩ. Generally, the thickness of the n-type SiC substrate is 350 μm and the doping concentration is 5E18 cm -3 , the resistivity is 20 mΩ·cm. By using the method for preparing a silicon carbide power device of the present invention, the on-resistance can be reduced to 66 mΩ without changing the device structure and other processes, and the manufacturing cost is reduced, thereby promoting the large-scale application of silicon carbide power electronic devices.
[0068] The present invention uses a semi-insulating silicon carbide substrate to prepare a silicon carbide power device. Since the semi-insulating silicon carbide is colorless and transparent, and the conductive silicon carbide is green, there is an obvious interface between the semi-insulating silicon carbide and the conductive silicon carbide. The laser stripping technology makes it easier to separate the semi-insulating silicon carbide from the epitaxially grown conductive silicon carbide. The conductive silicon carbide after stripping is less damaged. The semi-insulating silicon carbide single crystal substrate can be reused. The silicon carbide power device prepared by the method of the present invention completely eliminates the on-resistance and conduction loss of the conductive silicon carbide single crystal substrate. In the process of preparing the silicon carbide power device, the semi-insulating silicon carbide single crystal substrate can be reused, reducing the preparation cost of the silicon carbide power device. The technical process of the present invention improves the current density of the silicon carbide power device, reduces the on-resistance of the device, and reduces the conduction loss of the device by eliminating the n-type silicon carbide single crystal substrate.
[0069] It should be noted that when the present invention relates to a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundant description, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, once those skilled in the art know the basic creative concept, they can make other changes and modifications to these embodiments. Therefore, the attached protection scope is intended to be interpreted as including the preferred embodiment and all changes and modifications that fall within the scope of the present invention.
[0070] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the protection scope of the present invention and its equivalent technology, the present invention is also intended to include these changes and variations.
Claims
1. A method for preparing a silicon carbide power device, characterized in that: The following steps are involved: A semi-insulating silicon carbide single crystal substrate (1) is used as a substrate, an n-type silicon carbide single crystal epitaxial layer (2) is grown on the silicon surface of the semi-insulating silicon carbide single crystal substrate (1), a silicon carbide device structure (3) is prepared on the silicon surface of the n-type silicon carbide single crystal epitaxial layer (2), and a photoresist (4) is spin-coated on the silicon carbide device structure (3); By means of laser scanning, a modified layer is formed at the interface between the n-type silicon carbide single crystal epitaxial layer (2) and the semi-insulating silicon carbide single crystal substrate (1), and the semi-insulating silicon carbide single crystal substrate (1) is peeled off; Depositing an ohmic contact metal (7) on the carbon surface of the n-type silicon carbide single crystal epitaxial layer (2), and performing laser annealing to prepare an ohmic contact of the device, and then continuing to deposit metal silver (8) on the ohmic contact metal (7); By means of laser scanning, the ohmic contact metal (7) and the metal silver (8) are laser ablated to form grooves by sublimation, thereby separating the ohmic contact metal (7) and the metal silver (8) on the back side of the silicon carbide device structure (3); The photoresist (4) on the silicon carbide device structure (3) is removed, and the conductive silicon carbide is laser-modified by means of laser scanning to form a cavity layer in the conductive silicon carbide, thereby separating the silicon carbide device.
2. The method for preparing a silicon carbide power device according to claim 1, characterized in that: The thickness of the semi-insulating silicon carbide single crystal substrate (1) is 350 μm to 500 μm, and the thickness of the n-type silicon carbide single crystal epitaxial layer (2) is 10 μm to 100 μm.
3. The method for preparing a silicon carbide power device according to claim 1, characterized in that: When peeling off the semi-insulating silicon carbide single crystal substrate and separating the silicon carbide device, the laser scanning parameters are: laser wavelength 1064 nm, frequency 100 kHz~500kHz, pulse width 100 fs~5000 fs, and scanning speed 100 mm / s~1000 mm / s.
4. The method for preparing a silicon carbide power device according to claim 1, characterized in that: When separating the metal on the back of the silicon carbide device, the laser scanning parameters are: laser wavelength 355 nm, frequency 1 kHz~500 kHz, pulse width 100 fs~5000fs, and scanning speed 100 mm / s~1000 mm / s.
5. The method for preparing a silicon carbide power device according to claim 1, characterized in that: The laser annealing temperature is 900°C to 1000°C, and the annealing time is 1 min to 10 min.
6. The method for preparing a silicon carbide power device according to claim 1, characterized in that: The ohmic contact metal (7) is nickel or nickel-titanium alloy.
7. The method for preparing a silicon carbide power device according to claim 6, characterized in that: The thickness of nickel or nickel-titanium alloy deposition is 50 nm~100 nm.
8. A silicon carbide power device prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the silicon carbide power device according to claim 8 in manufacturing silicon carbide power electronic devices.