Polypyrrole / graphene composite material and preparation method thereof

By synthesizing PPy nanotubes and graphene composites, and using a water bath heating method to prepare polypyrrole/graphene composite materials, the stability and performance problems of polypyrrole/graphene composite materials in sodium-ion batteries have been solved, and a higher ratio has been achieved. Surface area and cycling stability improve the electrochemical performance of sodium-ion batteries.

CN118825221APending Publication Date: 2024-10-22BEIJING TECH & BUSINESS UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410790842.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing polypyrrole/graphene composite materials in sodium-ion batteries have problems such as easy accumulation of single-layer graphene sheets, reduced specific surface area, rapid initial capacity fading, and poor cycle stability and processing performance of polypyrrole.

Method used

PPy nanotubes were synthesized from ferric chloride, methyl orange and pyrrole monomers as raw materials, and compounded with graphene. The polypyrrole/graphene composite material was synthesized using a water bath heating method to improve its conductive properties and cycle stability.

Benefits of technology

It improves the specific surface area and cycle stability of the material, enhances the electrical conductivity, ensures a high reversible capacity under high current density, and overcomes the impact of volume and mass changes of the anode material during the charge and discharge process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825221A_ABST
    Figure CN118825221A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion batteries, and particularly relates to a polypyrrole / graphene composite material and a preparation method thereof. Comprising the following steps: 1, synthesizing polypyrrole nanofibers by taking ferric trichloride and methyl orange as raw materials; and 2, synthesizing the polypyrrole / graphene composite material by taking the polypyrrole nanofiber and graphene as raw materials. According to the polypyrrole / graphene composite material and the preparation method thereof provided by the invention, the polypyrrole / graphene composite material is used as a negative electrode material of an electrode for deep analysis and research, and graphene is subjected to polypyrrole composite modification in a mode of characterizing the conductivity of graphene, so that the polypyrrole / graphene composite material shows the optimal conductivity. In the future, an electrode material with low cost, high efficiency and excellent conductivity is developed, the limitation of the prior art is broken through, and the development of a sodium ion battery negative electrode material meeting various requirements becomes a main development direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries, and particularly relates to a polypyrrole / graphene composite material and a preparation method thereof. Background Art

[0002] Sodium-ion batteries are mainly composed of positive electrode, electrolyte, diaphragm, negative electrode and shell. The electrolyte is composed of organic solution containing sodium ions, and the diaphragm is glass fiber. Common positive electrode materials are metal oxides. There are many types of shells with different shapes. The negative electrode materials should consider factors such as structural stability and irreversible capacity. There are many types at present, such as hard carbon and alloy materials. During the charging and discharging process, the sodium-ion battery realizes the charging and discharging behavior of mutual conversion of chemical energy and electrical energy by the intercalation and deintercalation of sodium ions between the positive and negative electrode materials. During charging, the positive electrode loses electrons, and sodium ions escape from the positive electrode, enter the electrolyte, pass through the diaphragm, and embed into the surface of the negative electrode, and then react with the negative electrode material. The electrons are transmitted to the negative electrode through the external circuit. The discharge process is exactly the opposite of the charging process. Sodium ions escape from the negative electrode and return to the surface of the positive electrode to react with the positive electrode material. During the conventional charging and discharging process, sodium ions move back and forth between the positive and negative electrodes, which is similar to the rocking chair principle of lithium batteries.

[0003] Two-dimensional nanographene has a special honeycomb lattice structure, which gives it good mechanical properties and thermal stability, greatly increases its specific surface area, and also improves its electrical conductivity. After compounding with other conductive polymers, its specific surface area is further expanded, and the surface of the material is also rich in functional groups, which can greatly improve the capacitance performance of the polymer. Such a structure provides more areas for polypyrrole, which enhances the electrochemical reaction activity of polypyrrole, thereby improving the electrochemical performance of the material. The nanostructure of graphene gives it a high electrical conductivity and thermal conductivity. Yang Jun et al.

[21] By adopting the method of chemical vapor deposition, the graphene film is coated with the foam copper with a three-dimensional network structure to form a composite material of the two, so that the graphene is evenly dispersed on the copper base, thereby maximizing the conductive properties of the material.

[0004] As an excellent conductive polymer, polypyrrole (PPy) has the characteristics of high conductivity and specific capacitance. It contains a heterocyclic ring in its chemical structure. As a conductive polymer, it is easy to electrochemically polymerize into a film, making it an ideal choice for preparing electrode materials. However, due to the insoluble and infusible characteristics of polypyrrole itself, in actual production, it is usually combined with other materials to improve its performance.

[0005] Compared with pure PPy, composite materials synthesized from it have advantages in various properties, such as thermal stability. Studies have shown that the comprehensive performance of PPy / rGO composite materials is more satisfactory than that of single polypyrrole or graphene. There are many methods for preparing polypyrrole / graphene composite materials, among which the more commonly used ones are in-situ polymerization, electrochemical polymerization and interfacial polymerization. Based on the good electrical conductivity and thermal stability of the composite material, the research on polypyrrole / graphene composite materials has become one of the mainstream research directions in this field.

[0006] However, the current composite materials still have the following problems:

[0007] Single-layer graphene sheets are very easy to stack, and the reduction in specific surface area causes them to lose some sodium storage space; the first coulombic efficiency is low; the initial capacity decays quickly, etc. Polypyrrole, as a conductive polymer, has the characteristics of large specific surface area and environmental friendliness, but polypyrrole has poor cycle stability and processing performance. Summary of the invention

[0008] In order to comprehensively solve the above problems, the present invention proposes a polypyrrole / graphene composite material and a preparation method thereof, and through in-depth analysis and research of the negative electrode material using the polypyrrole / graphene composite material as an electrode, the graphene is subjected to polypyrrole composite modification by characterizing the conductive properties of graphene, so that it exhibits the best conductive properties. In the future, the development of low-cost, high-efficiency, and excellent conductive electrode materials, breaking through the limitations of the existing technology, and developing negative electrode materials for sodium ion batteries that meet various needs will become the main development direction.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0010] A polypyrrole / graphene composite material is prepared by taking ferric chloride, methyl orange and pyrrole monomer as raw materials to synthesize PPy nanotubes, and then adding graphene to finally synthesize the polypyrrole / graphene composite material.

[0011] A method for preparing a polypyrrole / graphene composite material, comprising:

[0012] Step 1: Using ferric chloride, methyl orange and pyrrole monomer as raw materials, PPy nanotubes are synthesized by room temperature polymerization;

[0013] Step 2: Using PPy nanotubes and graphene as raw materials, synthesize polypyrrole / graphene composite materials by water bath heating method.

[0014] Preferably, step 1 comprises:

[0015] Step 1.1: Add ferric chloride and methyl orange to water and stir for half an hour;

[0016] Step 1.2: Add pyrrole monomer, stir at room temperature for 24 hours, wash the obtained black product with ethanol and deionized water several times, and dry it in an oven at 50°C for 24 hours to obtain PPy nanotubes.

[0017] Preferably, step 2 comprises:

[0018] Step 2.1: Mix the PPy nanotubes from step 1 with the graphene solution, add water, and adjust the graphene concentration to 1 mg ml -1 , stir and mix evenly;

[0019] Step 2.2: Add L-ascorbic acid, stir alternately, sonicate until there is no precipitation at the bottom, heat in a water bath for 2 h to obtain a hydrogel, and freeze-dry to obtain the final product.

[0020] Preferably, in step 1.1, the mass ratio of ferric chloride, methyl orange and pyrrole monomer is 0.41:0.05:0.1.

[0021] Preferably, in step 2.1, the mass ratio of PPy nanotubes to graphene is 14:1.

[0022] Preferably, the water bath heating temperature in step 2.2 is 95°C.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The one-dimensional nano-polypyrrole material prepared by the present invention has the characteristics of high specific surface area, which makes it have a larger reaction surface and higher activity, and can be used in fields such as energy conversion and chemical reaction. Therefore, the problem of poor cycle stability can be improved. At the same time, the introduction of large-sheet graphene can further improve the dispersibility of polypyrrole nanowires, slow down the volume expansion of polypyrrole nanowires during the sodium extraction process, and improve the cycle stability of the composite material.

[0025] 2. When the material prepared by the present invention is cycled at a high current density of 500 mA / g, the PPy / rGO composite material maintains a reversible capacity of 58.1 mAh / g after 500 cycles. The composite of polypyrrole nanotubes and graphene overcomes the influence of the volume and mass changes of the negative electrode material polypyrrole during the electrode charge and discharge process, and obtains better performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.

[0027] In the attached picture:

[0028] Attached Figure 1It is the XRD test of PPy / rGO composite material.

[0029] Attached Figure 2 It is FTIR test of PPy / rGO composite material.

[0030] Attached Figure 3 It is the Raman test of PPy / rGO composite material.

[0031] Attached Figure 4 This is the XPS test of PPy / rGO composite material: (a) N 1s energy spectrum; (b) C 1s energy spectrum.

[0032] Attached Figure 5 It is the SEM test of PPy.

[0033] Attached Figure 6 This is the SEM test of PPy / rGO composite material.

[0034] Attached Figure 7 It is the cycle performance test of PPy / rGO composite material.

[0035] Attached Figure 8 This is the rate performance test of PPy / rGO composite materials.

[0036] Attached Fig. 9 Long cycle performance test of PPy / rGO composite materials.

[0037] Attached Fig.10 AC impedance test of PPy / rGO composite material.

[0038] Attached Fig.11 The figure is a flow chart of the method of the present invention. DETAILED DESCRIPTION

[0039] The following is combined with Figure 1-11 The preferred embodiments of the present invention are described. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0040] A method for preparing a polypyrrole / graphene composite material, comprising:

[0041] Step 1: Using ferric chloride, methyl orange and pyrrole monomer as raw materials, polypyrrole (PPy) nanotubes are synthesized by room temperature polymerization.

[0042] Step 1.1: Add 1.5 mmol of ferric chloride and 0.15 mmol of methyl orange to 30 mL of water and stir for half an hour;

[0043] Step 1.2: Add 100 μl of pyrrole monomer, stir at room temperature for 24 h, wash the resulting black product several times with ethanol and deionized water, and dry it in an oven at 50° C. for 24 h to obtain polypyrrole nanofibers.

[0044] Step 2: Using polypyrrole nanofibers and graphene as raw materials, synthesizing polypyrrole / graphene composite materials.

[0045] Step 2.1: Mix 0.14 g polypyrrole nanotubes with 0.1 g graphene solution, add water to 100 mL, and adjust the graphene concentration to 1 mg ml -1 , stir for 30 minutes to mix evenly;

[0046] Step 2.2: Add 1.44 g of L-ascorbic acid, stir and sonicate alternately until there is no precipitation at the bottom, heat in a 95° C. water bath for 2 h (without stirring) to obtain a hydrogel, and freeze-dry to obtain the final product.

[0047] test:

[0048] 1. Basic characterization of PPy / rGO composites

[0049] 1.1XRD test

[0050] The crystal structure of PPy / rGO composites was studied by XRD. Figure 1 As shown, the XRD curve has two peaks at 2θ=12.8 and 24.98. The peak at 2θ=12.8 indicates that it is a material containing carbon, and the peak at 2θ=24.98 indicates that it is a polypyrrole peak. Both peaks are relatively broad, indicating that the material is amorphous and does not have high crystallinity.

[0051] 1.2 FTIR test

[0052] The composition of PPy / rGO was further detected by FTIR. Figure 2 As shown in the infrared absorption spectrum of polypyrrole / graphene composites, multiple PPy characteristic peaks were observed. Among them, the peaks at 891 and 1037 cm -1 The two bands correspond to the out-of-plane deformation vibration of the CH of the pyrrole ring, located at 1154 cm -1 The band at 1544 cm -1 The peak centered at 3426 cm is attributed to the stretching vibration of C=C. -1 The peak at is the stretching vibration of NH. This proves that the PPy / rGO composite material is successfully synthesized.

[0053] 1.3 Raman spectroscopy test

[0054] like Figure 3As shown, the Raman spectrum of carbon materials is between 1200-1700 cm -1 There are two peaks in between. The higher peak on the left indicates that the material has more defects; the higher peak on the right indicates that the material has a higher degree of graphitization. -1 There is a peak at 1601cm, which means that this material has more defects and more active sites for reacting with sodium ions. -1 There is a peak at , which means the material has a certain degree of graphitization.

[0055] 1.4XPS test

[0056] In order to study the composition and surface state of the composite samples, the XPS spectrum of the PPy / rGO composite was tested. Figure 4 The valence state of the elements in the composite material was tested by XPS. The XPS test spectrum showed that the composite material contained nitrogen, carbon and other elements. For PPy / rGO, the spectra of N and C are as follows Figure 4 As shown in (a) and (b). Figure 4 (a) Corresponding to the N1s spectrum, the N1s broadband is divided into three peaks, centered at 400.88, 399.28, and 398.58 eV, respectively, corresponding to the protonated amine unit (-NH + ), cationic N atom (=NH + ) corresponds to aniline (-NH-). Aniline (-NH-) is located in the skeleton of polypyrrole. =NH + The high peak value indicates that PPy / rGO has good electrical conductivity. Figure 4 The C1s spectrum in (b) is fitted by component peaks centered at 283.98, 284.68, 286.08, and 288.28 eV, corresponding to C=C, CC, CN, and C=O, respectively. In summary, it is proved that the PPy / rGO composite material was successfully synthesized.

[0057] 1.5 Scanning electron microscope test

[0058] Figure 5 The SEM image of PPy shows that the morphology of PPy is a nanowire structure with a diameter of about 200 nm. There is no obvious agglomeration phenomenon in the image, indicating that the PPy sample material is not easy to agglomerate. It can be seen from the image that there are some polypyrrole particles that have not grown into nanowires.

[0059] Figure 6 It can be seen that after compounding with graphene, PPy nanotubes are dispersed between graphene sheets, which is more dispersed than before compounding, which increases the specific surface area of ​​the composite material and improves the sodium storage capacity of the material.

[0060] 2. Characterization of sample electrochemical properties

[0061] Preparation of battery working electrode

[0062] The preparation method of the negative electrode sheet of the sodium ion battery is as follows:

[0063] Step 1: Using deionized water as solvent, the active material PPy / rGO composite material, the reaction conductive agent SuperP and the binder sodium alginate are mixed. In the mixture, the mass of the active material accounts for 60%, the mass of SuperP accounts for 20%, and the mass of sodium alginate accounts for 20%.

[0064] Step 2: Take a piece of glass, wipe its front clean with an alcohol cotton ball, then cut a piece of copper foil of appropriate size, wipe both sides of it clean with an alcohol cotton ball, and place it on the prepared glass to ensure that there are no bubbles between the two.

[0065] Step 3: Take a mortar, weigh 60 mg of the active material PPy / rGO composite material, 20 mg of SuperP, and 20 mg of sodium alginate and put them in the mortar, and grind them vigorously for 30 minutes to mix the materials evenly and refine them into particles.

[0066] Step 4: Add an appropriate amount of deionized water to the mortar and continue grinding until the mixture is evenly mixed. During this period, add appropriate amount of deionized water according to the viscosity of the slurry, and adjust the viscosity to keep it in an appropriate range. After each addition of deionized water, it is also necessary to fully grind to mix the various components in the slurry evenly. Move the mixed slurry to the clean copper foil, and use a medicine spoon to gently scrape the slurry to keep the thickness of the slurry on the copper foil basically consistent, and dry it at room temperature.

[0067] Step 5: Use a slicer to cut the copper foil with electrode material into several discs with a diameter of 10 mm, so as to obtain the negative electrode sheets required for the subsequent assembly of the battery. At the same time, use a slicer to cut several blank copper foil discs that are not coated with slurry as blank comparisons. Place the obtained negative electrode sheets in a vacuum drying oven and dry them at 120 degrees Celsius. Weigh the mass of the obtained negative electrode sheets and blank copper foil discs one by one, and make corresponding records. Subtract the average mass of the blank copper foil discs from the mass of each negative electrode sheet, and then multiply by 0.6 to obtain the mass of the active material coated on the copper foil, and record the mass accordingly, and then evaluate its electrochemical performance through battery electrochemical performance tests.

[0068] 2.1 Cycle performance test

[0069] Figure 7 The cycling performance of the PPy / rGO composite material at a current density of 50 mA / g was tested. After 100 cycles, it was still able to stably maintain a capacity of 144.9 mAh / g. The current cycling performance is relatively stable.

[0070] 2.2x performance test

[0071] The rate performance of the PPy / rGO composite material was tested, and the test results showed that when the current density was 0.05, 0.1, 0.2, 0.5, and 1A / g, the battery capacity could be maintained at 157.1, 113.7, 89.4, 60.6, and 40.2 mAh / g after 10 cycles. When the current density was restored to 0.05A / g, the reversible capacity of 165.4 mAh / g could still be maintained, showing good rate performance.

[0072] 2.3 High current long cycle performance test

[0073] When cycled at a high current density of 500 mA / g, the long-cycle performance of the PPy / rGO composite material is slightly poor, maintaining a reversible capacity of 58.1 mAh / g after 500 cycles. The cycling performance at high current still needs to be improved.

[0074] 2.4 AC impedance test

[0075] like Fig.10 , the AC impedance test was performed on the battery that was cycled 20 times at a current of 200mA / g, and an equivalent circuit was simulated. Re, Rf, and Rct were obtained by fitting the data, which represent the impedance of the battery respectively. Re represents the resistance of the battery itself, Rf represents the resistance generated by the battery during the cycle, and Rct represents the charge transfer impedance. As shown in Table 1, the value of Re is 3.314Ω, the value of Rf is 289.4Ω, and the value of Rct is 55.16Ω. The smaller the Rct number, the faster the charge transfer, which means the better the cycle performance of the battery. The above data show that the prepared battery has a good ability to transfer electrons.

[0076] Table 1 Battery AC impedance test fitting values

[0077] Re R Rct Impedance(Ω) 3.314 289.4 55.16

[0078] Summarize:

[0079] The present invention obtains PPy nanotubes by a room temperature polymerization method, and then synthesizes a PPy / rGO nanocomposite material by a water bath heating method. Scanning electron microscopy shows that the PPy nanotubes are dispersed between graphene sheets, and are more dispersed than before the composite. Electrochemical tests show that the prepared composite material has excellent cycle performance. When the current density is 50 mA / g, the capacity of 144.9 mAh / g can still be stably maintained after 100 cycles; when the composite material is subjected to a rate test, when the current density is 0.05, 0.1, 0.2, 0.5, and 1 A / g, respectively, after 10 cycles, the battery capacity can be maintained at 157.1, 113.7, 89.4, 60.6, and 40.2 mAh / g, respectively. When the current density is restored to 0.05 A / g, the reversible capacity can still be maintained at 165.4 mAh / g, showing good rate performance of the polypyrrole / graphene composite material. When cycling at a high current density of 500 mA / g, the long-cycle performance of the PPy / rGO composite material is slightly worse, maintaining a reversible capacity of 58.1 mAh / g after 500 cycles. The composite of polypyrrole nanotubes and graphene overcomes the impact of the volume and mass changes of the negative electrode material polypyrrole during the electrode charge and discharge process, and achieves better performance.

[0080] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A polypyrrole / graphene composite material, characterized in that: PPy nanotubes were synthesized using ferric chloride, methyl orange and pyrrole monomers as raw materials, and then graphene was added to finally synthesize polypyrrole / graphene composite materials.

2. A method for preparing a polypyrrole / graphene composite material, characterized in that: include: Step 1: Using ferric chloride, methyl orange and pyrrole monomer as raw materials, PPy nanotubes are synthesized by room temperature polymerization; Step 2: Using PPy nanotubes and graphene as raw materials, synthesize polypyrrole / graphene composite materials by water bath heating method.

3. The method for preparing a polypyrrole / graphene composite material according to claim 2, characterized in that: Step 1 includes: Step 1.1: Add ferric chloride and methyl orange to water and stir for half an hour; Step 1.2: Add pyrrole monomer, stir at room temperature for 24 hours, wash the obtained black product with ethanol and deionized water several times, and dry it in an oven at 50°C for 24 hours to obtain PPy nanotubes.

4. The method for preparing a polypyrrole / graphene composite material according to claim 3, characterized in that: Step 2 includes: Step 2.1: Mix the PPy nanotubes from step 1 with the graphene solution, add water, and adjust the graphene concentration to 1 mg ml -1 , stir and mix evenly; Step 2.2: Add L-ascorbic acid, stir alternately, sonicate until there is no precipitation at the bottom, heat in a water bath for 2 h to obtain a hydrogel, and freeze-dry to obtain the final product.

5. The method for preparing a polypyrrole / graphene composite material according to claim 4, characterized in that: The mass ratio of ferric chloride, methyl orange and pyrrole monomer in step 1.1 is 0.41:0.05:0.

1.

6. The method for preparing a polypyrrole / graphene composite material according to claim 5, characterized in that: The mass ratio of PPy nanotubes to graphene in step 2.1 is 14:

1.

7. The method for preparing a polypyrrole / graphene composite material according to claim 6, characterized in that: Step 2.2 The water bath is heated to 95°C.