Fiber cloth-based battery diaphragm and processing technology thereof

Through the combination of sea-island fiber, ultra-fine carbon fiber and polyolefin fiber, the battery separator is prepared using polyacrylonitrile and polymethyl methacrylate spinning technology, which solves the problems of thermal shrinkage and insufficient liquid absorption performance of existing separators at high temperatures. A battery separator with high porosity, low pore size and good mechanical properties was achieved.

CN118825554AActive Publication Date: 2024-10-22ANHUI HUITONG NEW ENERGY TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410849645.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-22
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators suffer from serious thermal shrinkage in high-temperature environments, and lack sufficient liquid absorption performance and mechanical strength, making it difficult to meet battery usage requirements. In particular, the single material of polyacrylonitrile nano-separators has defects and cannot meet the multiple requirements of battery separators. Performance requirements.

Method used

A combination of sea-island fiber, ultra-fine carbon fiber and polyolefin fiber is used to prepare the fiber cloth-based battery separator through the spinning technology of polyacrylonitrile and polymethyl methacrylate spinning solution. The sea-island fiber uses polyacrylonitrile as the island phase and poly Methyl methacrylate is a marine phase, ultra-fine carbon fibers are carbonized, and the proportion of fiber components is optimized to improve porosity and mechanical properties.

Benefits of technology

It significantly improves the temperature resistance and electrolyte wettability of the separator, meets the high porosity and small pore size requirements of the battery separator, improves the mechanical properties, avoids high-temperature thermal shrinkage, and ensures battery safety and performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004916484920000101
    Figure BDA0004916484920000101
Patent Text Reader

Abstract

The invention discloses a fiber cloth-based battery diaphragm and a processing technology thereof, and belongs to the technical field of diaphragms.The fiber cloth-based battery diaphragm is prepared by adopting polyacrylonitrile and polymethyl methacrylate to prepare sea-island fibers, carbonizing the sea-island fibers to prepare superfine carbon fibers, blending the sea-island fibers, the superfine carbon fibers and polyolefin fibers, preparing fiber non-woven fabric through dry carding, and preparing the fiber non-woven fabric into the battery diaphragm. And obtaining the fiber cloth-based battery diaphragm. The sea-island fibers take polyacrylonitrile with high temperature resistance and high strength as a framework, polymethyl methacrylate has good hydrophilicity and is blended with the polyolefin fibers to endow the diaphragm with good temperature resistance and hydrophilicity, the superfine carbon fibers are good in temperature resistance and mechanical property and small in size, fiber cloth is prepared by blending the superfine carbon fibers, the sea-island fibers and the polyolefin fibers through a dry carding method, and the diaphragm has good heat resistance and hydrophilicity. The small aperture and high porosity of the fiber cloth-based battery diaphragm can be realized, and the safety of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of diaphragms, and in particular relates to a fiber cloth-based battery diaphragm and a processing technology thereof. Background Art

[0002] In order to promote the rapid development of the lithium-ion battery industry and help the automotive industry achieve its "dual carbon" goals, people have developed many new types of separators based on traditional polyolefin separators and based on the needs of lithium battery application scenarios.

[0003] The nonwoven membrane uses a non-woven method to orient or randomly arrange the fibers to form a fiber mesh structure, and then use chemical or physical methods to reinforce the membrane to have good air permeability and liquid absorption rate. Polyolefin fiber is an ideal substrate for preparing battery separators, but polyolefin fiber has poor hydrophilicity due to the lack of hydrophilic groups in the polyolefin macromolecular structure, and the nonwoven fabric used for battery separators must have excellent liquid absorption performance. Therefore, the hydrophilic treatment technology of polyolefin fiber nonwoven fabric is a key technology for preparing battery separators. In addition, since the thermal deformation temperature of polyolefin fiber is relatively low, the separator will experience severe thermal shrinkage when the temperature is too high, so it is not suitable for use in high temperature environments. Nonwoven fiber cloth separators have the characteristics of large pore size and high porosity. In order to reduce the pore size, the thickness must be increased, but too large a thickness will affect the battery capacity. At present, electrospinning nanofibers are mostly used to prepare fiber cloth separators, but the relative cost of electrospinning is relatively high, which is not conducive to the mass production of battery separators.

[0004] Polyacrylonitrile has gradually become one of the membrane modification materials in recent years due to its excellent chemical stability and temperature resistance. Polyacrylonitrile membranes are mainly prepared by electrospinning. However, nano-membrane materials made from single polyacrylonitrile have defects, poor mechanical strength and hydrophilicity, and need further improvement to meet the requirements for battery membrane use.

[0005] The Chinese invention patent with application number CN201811265901.8 discloses a modified polyacrylonitrile nonwoven fabric / silicon dioxide aerogel composite diaphragm for batteries and its preparation method, which uses polyacrylonitrile nonwoven fabric as the composite diaphragm substrate and uses heat-resistant and lightweight silicon dioxide aerogel as the coating material to improve the heat resistance of the diaphragm. However, due to the in-situ growth of silicon dioxide aerogel on the surface of the modified polyacrylonitrile nonwoven fabric fiber, the pore size and porosity of the composite diaphragm cannot be guaranteed to change, and there is no significant improvement in its mechanical properties. Summary of the invention

[0006] The object of the present invention is to provide a fiber cloth-based battery separator and a processing technology thereof, which can effectively improve the temperature resistance and electrolyte wettability of the battery separator.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] The present invention provides a fiber cloth-based battery diaphragm, wherein the diaphragm fiber components include sea-island fibers, ultrafine carbon fibers and polyolefin fibers; the sea-island fibers have polyacrylonitrile as the island phase and polymethyl methacrylate as the sea phase; the ultrafine carbon fibers are the carbonization products of the sea-island fibers; and the polyolefin fibers are any combination of polypropylene fibers and polyethylene fibers.

[0009] Furthermore, the mass ratio of the island-island component of the sea-island fiber is (5-3):(5-7). The higher the proportion of the "island" component in the sea-island fiber, the more difficult it is to prepare, which is not conducive to the "sea" component forming a continuous phase.

[0010] Furthermore, the ratio of sea island fibers, ultrafine carbon fibers and polyolefin fibers in the diaphragm fiber components is: 10-30wt% of sea island fibers, 10-40wt% of ultrafine carbon fibers, and the remainder is polyolefin fibers. A large proportion of sea island fibers and ultrafine fibers will increase the cost, and ultrafine carbon fibers are beneficial to reducing the pore size of the fiber cloth and ensuring a good porosity.

[0011] Furthermore, the fiber cloth-based battery separator has a pore size of 1-5 μm, a porosity of 38-65%, a thickness of 20-30 μm, and a gram weight of 10-15 g / m 2 .

[0012] The present invention also provides a processing technology for a fiber cloth-based battery separator, and the processing steps are as follows:

[0013] S1. Preparation of spinning solution:

[0014] Dissolving polymethyl methacrylate and polyacrylonitrile in dimethylacetamide (DMAC) to prepare solutions, respectively obtaining polymethyl methacrylate spinning solution and polyacrylonitrile spinning solution;

[0015] S2. Preparation of sea-island fibers and ultrafine carbon fibers:

[0016] The spinning solutions are filtered and vacuum degassed for 12-24 hours respectively, and then enter the No. 1 and No. 2 feed ports of the spinning machine respectively, and are ejected from the island-in-the-sea composite spinneret. The composite fibers from the spinneret are successively subjected to a coagulation bath, water washing, and drawing to obtain island-in-the-sea fibers, in which polyacrylonitrile is the island and polymethyl methacrylate is the sea. The island-in-the-sea fibers, which account for 1 / 3 of the mass, are pre-oxidized and carbonized to obtain ultrafine carbon fibers;

[0017] S3. Preparation of fiber nonwoven fabric:

[0018] The sea-island fibers, ultrafine carbon fibers and polyolefin fibers are blended, and the fiber cloth-based battery separator is obtained through opening, carding, web laying, hot rolling reinforcement and heat setting.

[0019] Furthermore, the concentration of polymethyl methacrylate in the polymethyl methacrylate spinning solution is 25-30wt%, and the concentration of polyacrylonitrile in the polyacrylonitrile spinning solution is 5%-15wt%.

[0020] Furthermore, the flow rate ratio of the polymethyl methacrylate spinning solution to the polyacrylonitrile spinning solution is 1:1-1:5, and the flow rate can be adjusted according to the required sea island component mass ratio.

[0021] Furthermore, the component of the coagulation bath is a dimethylacetamide aqueous solution, the concentration of the dimethylacetamide aqueous solution is 5%-35wt%, the coagulation bath temperature is 40-60°C, and the fiber coagulation time is 10-15min; the water washing time is set to 10-15min, and the water washing temperature is room temperature; the stretching multiple is 5-6 times, and the stretching temperature is 70-80°C. The stretching multiple should not be too large or too small. If it is too large, it will cause fiber breakage, and if it is too small, it will cause the fiber to be too thick and have poor mechanical properties.

[0022] Furthermore, the pre-oxidation temperature of the sea island fiber is 200-300°C, the pre-oxidation time is 1.5-2h, the carbonization temperature is 600-1500°C, the carbonization time is 30-60min, the diameter of the sea island fiber is 0.8-1.2μm, the diameter of the ultrafine carbon fiber is 300-500nm, and the carbonization treatment adopts multi-stage carbonization at different temperatures to achieve stable and uniform carbonization of the fiber.

[0023] Furthermore, the hot rolling reinforcement temperature is 80-105°C, and the heat setting temperature is 95-105°C.

[0024] Beneficial effects of the present invention:

[0025] (1) The sea-island fibers are prepared by combining polyacrylonitrile and polymethyl methacrylate, with polyacrylonitrile as the island and polymethyl methacrylate as the sea. Polyacrylonitrile can improve the temperature resistance and mechanical properties, while polymethyl methacrylate improves the electrolyte wettability of the fiber.

[0026] (2) The carbonization treatment of the sea-island fibers is used to remove the polymethyl methacrylate component to obtain ultrafine carbon fibers. The ultrafine carbon fibers have excellent heat-resistant mechanical properties and can make up for the defect of large pore size of nonwoven fabrics.

[0027] (3) The fiber cloth-based battery separator is prepared by dry-blending sea-island fibers, ultrafine carbon fibers and polyolefin fibers. It has outstanding temperature resistance, hydrophilicity and mechanical strength, and can meet the requirements of small pore size and high porosity of battery separator. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] Polymethyl methacrylate and polyacrylonitrile are dissolved in dimethylacetamide (DMAC) respectively to obtain 25 wt % polymethyl methacrylate spinning solution and 10 wt % polyacrylonitrile spinning solution.

[0031] The prepared spinning solutions were filtered and vacuum degassed for 12-24 hours respectively, and then entered into the No. 1 and No. 2 feed ports of the spinning machine respectively. Polyacrylonitrile was the island and polymethyl methacrylate was the sea. They were sprayed out from the island-in-sea composite spinneret, and the flow rate ratio of polymethyl methacrylate spinning solution to polyacrylonitrile spinning solution was set to 1:2.5.

[0032] The composite fiber from the spinneret enters the coagulation bath with the temperature set at 60°C. After 10 minutes of coagulation, it enters the washing tank and is washed at room temperature for 15 minutes to remove the surface solvent. The fiber is then hot-stretched with the stretching temperature set at 80°C and the stretching multiple set to 5 times to ensure fiber densification. Sea island fibers are obtained with a fiber diameter of 1.0 μm.

[0033] One third of the total mass of the sea island fiber was further processed, pre-oxidized at 220°C for 2 hours, carbonized in nitrogen, carbonized at 600-800°C for 20 minutes, and carbonized at 800-1500°C for 10 minutes. During the carbonization process, polymethyl methacrylate was removed to obtain ultrafine carbon fiber with a fiber diameter of 500nm.

[0034] 10wt% sea island fiber, 10wt% ultrafine carbon fiber and 80wt% polypropylene fiber were blended, and a blended fiber web was formed by opening, combing and laying. The fiber web was hot-rolled and reinforced by a hot roller set at a temperature of 100°C. In order to further improve the dimensional stability and mechanical properties of the fiber cloth, a heat setting treatment was performed, and the heat setting temperature was set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25μm and a gram weight of 15g / m 2 .

[0035] Example 2

[0036] Compared with Example 1, the proportion of sea-island fibers in the fiber component is increased from 10wt% to 20wt%. The specific implementation steps are as follows:

[0037] Polymethyl methacrylate and polyacrylonitrile are dissolved in dimethylacetamide (DMAC) respectively to obtain 25 wt % polymethyl methacrylate spinning solution and 10 wt % polyacrylonitrile spinning solution.

[0038] The prepared spinning solutions were filtered and vacuum degassed for 12-24 hours respectively, and then entered into the No. 1 and No. 2 feed ports of the spinning machine respectively. Polyacrylonitrile was the island and polymethyl methacrylate was the sea. They were sprayed out from the island-in-sea composite spinneret, and the flow rate ratio of polymethyl methacrylate spinning solution to polyacrylonitrile spinning solution was set to 1:2.5.

[0039] The composite fiber from the spinneret enters the coagulation bath with the temperature set at 60°C. After 10 minutes of coagulation, it enters the washing tank and is washed at room temperature for 15 minutes to remove the surface solvent. The fiber is then hot-stretched with the stretching temperature set at 80°C and the stretching multiple set to 5 times to ensure fiber densification. Sea island fibers are obtained with a fiber diameter of 1.0 μm.

[0040] One third of the total mass of the sea island fiber was further processed, pre-oxidized at 220°C for 2 hours, carbonized in nitrogen, carbonized at 600-800°C for 20 minutes, and carbonized at 800-1500°C for 10 minutes. During the carbonization process, polymethyl methacrylate was removed to obtain ultrafine carbon fiber with a fiber diameter of 500nm.

[0041] 20wt% sea island fiber, 10wt% ultrafine carbon fiber and 70wt% polypropylene fiber were blended, and a blended fiber web was formed through opening, combing and laying. The fiber web was hot-rolled and reinforced by a hot roller set at a temperature of 100°C. In order to further improve the dimensional stability and mechanical properties of the fiber cloth, a heat setting treatment was performed, and the heat setting temperature was set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25μm and a gram weight of 15g / m 2 .

[0042] Example 3

[0043] Compared with Example 1, the proportion of sea-island fibers in the fiber component is increased from 10wt% to 30wt%. The specific implementation steps are as follows:

[0044] Polymethyl methacrylate and polyacrylonitrile are dissolved in dimethylacetamide (DMAC) respectively to obtain 25 wt % polymethyl methacrylate spinning solution and 10 wt % polyacrylonitrile spinning solution.

[0045] The prepared spinning solutions were filtered and vacuum degassed for 12-24 hours respectively, and then entered into the No. 1 and No. 2 feed ports of the spinning machine respectively. Polyacrylonitrile was the island and polymethyl methacrylate was the sea. They were sprayed out from the island-in-sea composite spinneret, and the flow rate ratio of polymethyl methacrylate spinning solution to polyacrylonitrile spinning solution was set to 1:2.5.

[0046] The composite fiber from the spinneret enters the coagulation bath with the temperature set at 60°C. After 10 minutes of coagulation, it enters the washing tank and is washed at room temperature for 15 minutes to remove the surface solvent. The fiber is then hot-stretched with the stretching temperature set at 80°C and the stretching multiple set to 5 times to ensure fiber densification. Sea island fibers are obtained with a fiber diameter of 1.0 μm.

[0047] One third of the total mass of the sea island fiber was further processed, pre-oxidized at 220°C for 2 hours, carbonized in nitrogen, carbonized at 600-800°C for 20 minutes, and carbonized at 800-1500°C for 10 minutes. During the carbonization process, polymethyl methacrylate was removed to obtain ultrafine carbon fiber with a fiber diameter of 500nm.

[0048] 30wt% sea island fiber, 10wt% ultrafine carbon fiber and 60wt% polypropylene fiber were blended, and a blended fiber web was formed by opening, combing and laying. The fiber web was hot-rolled and reinforced by a hot roller set at a temperature of 100°C. In order to further improve the dimensional stability and mechanical properties of the fiber cloth, a heat setting treatment was performed, and the heat setting temperature was set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25μm and a gram weight of 15g / m 2 .

[0049] Example 4

[0050] Compared with Example 1, the proportion of ultrafine carbon fibers in the fiber component is increased from 10wt% to 25wt%. The specific implementation steps are as follows:

[0051] Polymethyl methacrylate and polyacrylonitrile are dissolved in dimethylacetamide (DMAC) respectively to obtain 25 wt % polymethyl methacrylate spinning solution and 10 wt % polyacrylonitrile spinning solution.

[0052] The prepared spinning solutions were filtered and vacuum degassed for 12-24 hours respectively, and then entered into the No. 1 and No. 2 feed ports of the spinning machine respectively. Polyacrylonitrile was the island and polymethyl methacrylate was the sea. They were sprayed out from the island-in-sea composite spinneret, and the flow rate ratio of polymethyl methacrylate spinning solution to polyacrylonitrile spinning solution was set to 1:2.5.

[0053] The composite fiber from the spinneret enters the coagulation bath with the temperature set at 60°C. After 10 minutes of coagulation, it enters the washing tank and is washed at room temperature for 15 minutes to remove the surface solvent. The fiber is then hot-stretched with the stretching temperature set at 80°C and the stretching multiple set to 5 times to ensure fiber densification. Sea island fibers are obtained with a fiber diameter of 1.0 μm.

[0054] One third of the total mass of the sea island fiber was further processed, pre-oxidized at 220°C for 2 hours, carbonized in nitrogen, carbonized at 600-800°C for 20 minutes, and carbonized at 800-1500°C for 10 minutes. During the carbonization process, polymethyl methacrylate was removed to obtain ultrafine carbon fiber with a fiber diameter of 500nm.

[0055] 10wt% island fiber, 25wt% ultrafine carbon fiber and 65wt% polypropylene fiber were blended, and a blended fiber web was formed by opening, combing and laying. The fiber web was hot-rolled and reinforced by a hot roller set at a temperature of 100°C. In order to further improve the dimensional stability and mechanical properties of the fiber cloth, a heat setting treatment was performed, and the heat setting temperature was set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25μm and a gram weight of 15g / m 2 .

[0056] Example 5

[0057] Compared with Example 1, the proportion of ultrafine carbon fibers in the fiber component is increased from 10wt% to 40wt%. The specific implementation steps are as follows:

[0058] Polymethyl methacrylate and polyacrylonitrile are dissolved in dimethylacetamide (DMAC) respectively to obtain 25 wt % polymethyl methacrylate spinning solution and 10 wt % polyacrylonitrile spinning solution.

[0059] The prepared spinning solutions were filtered and vacuum degassed for 12-24 hours respectively, and then entered into the No. 1 and No. 2 feed ports of the spinning machine respectively. Polyacrylonitrile was the island and polymethyl methacrylate was the sea. They were sprayed out from the island-in-sea composite spinneret, and the flow rate ratio of polymethyl methacrylate spinning solution to polyacrylonitrile spinning solution was set to 1:2.5.

[0060] The composite fiber from the spinneret enters the coagulation bath with the temperature set at 60°C. After 10 minutes of coagulation, it enters the washing tank and is washed at room temperature for 15 minutes to remove the surface solvent. The fiber is then hot-stretched with the stretching temperature set at 80°C and the stretching multiple set to 5 times to ensure fiber densification. Sea island fibers are obtained with a fiber diameter of 1.0 μm.

[0061] One third of the total mass of the sea island fiber was further processed, pre-oxidized at 220°C for 2 hours, carbonized in nitrogen, carbonized at 600-800°C for 20 minutes, and carbonized at 800-1500°C for 10 minutes. During the carbonization process, polymethyl methacrylate was removed to obtain ultrafine carbon fiber with a fiber diameter of 500nm.

[0062] 10wt% sea island fiber, 40wt% ultrafine carbon fiber and 50wt% polypropylene fiber were blended, and a blended fiber web was formed through opening, combing and laying. The fiber web was hot-rolled and reinforced by a hot roller set at a temperature of 100°C. In order to further improve the dimensional stability and mechanical properties of the fiber cloth, a heat setting treatment was performed, and the heat setting temperature was set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25μm and a gram weight of 15g / m 2 .

[0063] Comparative Example 1

[0064] Compared with Example 5, the difference is that a single polyacrylonitrile fiber is used to prepare the fiber cloth-based battery separator.

[0065] The polypropylene fiber is opened, combed, and laid to form a blended fiber web. The fiber web is hot-rolled and reinforced by a hot roller set at 100°C, and then heat-set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25 μm and a gram weight of 15 g / m 2 .

[0066] Comparative Example 2

[0067] Compared with Example 5, the difference is that polyacrylonitrile fiber is used to replace the sea-island fiber and the ultrafine carbon fiber to prepare the fiber cloth-based battery separator, and the polyacrylonitrile fiber used is prepared by the same wet spinning method as in Example 5.

[0068] 50wt% polyacrylonitrile fiber and 50wt% polypropylene fiber were blended, and the diameter of the polyacrylonitrile fiber was 1μm. The blended fiber web was formed by opening, combing, and laying. The fiber web was hot-rolled and reinforced by a hot roller set at a temperature of 100°C. In order to further improve the dimensional stability and mechanical properties of the fiber cloth, a heat setting treatment was performed, and the heat setting temperature was set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25μm and a gram weight of 15g / m 2 .

[0069] Comparative Example 3

[0070] Compared with Example 5, the difference is that carbon nanofibers are used to replace the sea-island fibers and ultrafine carbon fibers to prepare the fiber cloth-based battery separator, and the carbon nanofibers used are prepared by electrospinning, and the fiber diameter is 500 nm.

[0071] 50wt% electrospun carbon nanofibers and 50wt% polypropylene fibers were blended, and a blended fiber web was formed by opening, combing, and laying. The fiber web was hot-rolled and reinforced by a hot roller set at a temperature of 100°C. In order to further improve the dimensional stability and mechanical properties of the fiber cloth, a heat setting treatment was performed, and the heat setting temperature was set at 105°C to obtain a fiber cloth-based battery separator with a thickness of 25μm and a gram weight of 15g / m2 .

[0072] Performance tests were performed on Examples 1 to 5 and Comparative Examples 1 to 3, and the performance tests were performed with reference to GB / T36363-2018 “Lithium Ion Battery Separator Performance Test”. The results are shown in Table 1.

[0073] The thermal shrinkage test method is: place the sample in a 150°C oven for heat treatment for 60 minutes, and then measure the change in the diaphragm area before and after the heat treatment.

[0074] Table 1

[0075]

[0076] As can be seen from Table 1, the proportion of sea-island fibers in Examples 1-3 gradually increases, and the various properties of the diaphragm are improved. Polymethyl methacrylate can improve hydrophilicity, and polyacrylonitrile can enhance tensile strength and thermal stability. In Example 3, the electrolyte contact angle is only 9.1°, and the wettability of the electrolyte is greatly improved. Compared with Example 1, the content of ultrafine carbon fibers in Examples 4 and 5 is gradually increased, and the thermal stability of the diaphragm is significantly improved accordingly. The thermal shrinkage rate at 150°C is reduced to 0%, which can avoid the risk of high-temperature short circuit of the battery. The tensile strength of the diaphragm is increased to 104MPa, which can ensure the safety of the battery. In addition, the increase of ultrafine carbon fibers increases the porosity of the diaphragm on the one hand, and reduces the pore size of the diaphragm on the other hand, which is conducive to the migration of ions in the battery. Comparative Example 1 is a fiber cloth-based diaphragm prepared from a single polypropylene fiber component, and its various properties are relatively poor. Comparative Example 2 is a heat-resistant modification by adding conventional polyacrylonitrile fiber to polypropylene fiber, and its heat resistance and tensile strength are greatly improved compared with Comparative Example 1, but its hydrophilicity is significantly poorer than that of Example 5. Comparative Example 3 uses electrostatically spun carbon nanofibers and polypropylene fibers to blend and prepare a diaphragm. The diaphragm has a low heat shrinkage rate and a small pore size due to the effect of nanocarbon fibers, but the electrostatically spun fibers have relatively poor mechanical properties. Carbon fibers are hydrophobic fibers with poor affinity for electrolytes and large contact angles. Comprehensive analysis shows that the fiber cloth-based diaphragm prepared in Example 5 has good mechanical properties, thermal stability, and electrolyte wettability, and the diaphragm has a high porosity and a small pore size, with obvious advantages.

[0077] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A fiber cloth-based battery separator, characterized in that: The diaphragm includes sea-island fibers, ultrafine carbon fibers and polyolefin fibers; The sea-island fiber has polyacrylonitrile as the island phase and polymethyl methacrylate as the sea phase; The ultrafine carbon fiber is a carbonized product of sea-island fibers; The polyolefin fibers are any combination of polypropylene fibers and polyethylene fibers.

2. A fiber cloth-based battery separator according to claim 1, characterized in that: The mass ratio of the island-in-sea fiber components is (5-3):(5-7).

3. A fiber cloth-based battery separator according to claim 1, characterized in that: Calculated by weight percentage, the sea island fiber is 10wt%-30wt%, the ultrafine carbon fiber is 10wt%-40wt%, and the rest is polyolefin fiber.

4. The fiber cloth-based battery separator according to claim 1, characterized in that: The fiber cloth-based battery separator has a pore size of 1-3 μm, a porosity of 38-65%, a thickness of 20-30 μm, and a gram weight of 10-15 g / m 2 .

5. A processing technology for a fiber cloth-based battery separator according to any one of claims 1 to 4, characterized in that: The steps include: S1. Preparation of spinning solution: Dissolving polymethyl methacrylate and polyacrylonitrile in dimethylacetamide to prepare solutions, respectively, to obtain polymethyl methacrylate spinning solution and polyacrylonitrile spinning solution; S2. Preparation of sea-island fibers and ultrafine carbon fibers: The spinning solutions are filtered and vacuum degassed for 12-24 hours respectively, and then enter the No. 1 and No. 2 feed ports of the spinning machine respectively, and are ejected from the island-in-the-sea composite spinneret. The composite fibers from the spinneret are successively subjected to a coagulation bath, water washing, and drawing to obtain island-in-the-sea fibers, wherein polyacrylonitrile is the island and polymethyl methacrylate is the sea; the island-in-the-sea fibers, which account for 1 / 3 of the mass, are pre-oxidized and carbonized to obtain ultrafine carbon fibers; S3. Preparation of fiber nonwoven fabric: The sea-island fibers, ultrafine carbon fibers and polyolefin fibers are blended, and the fiber cloth-based battery separator is obtained through opening, carding, web laying, hot rolling reinforcement and heat setting.

6. The processing technology of a fiber cloth-based battery separator according to claim 5, characterized in that: The concentration of polymethyl methacrylate in the polymethyl methacrylate spinning solution is 25wt%-30wt%, and the concentration of polyacrylonitrile in the polyacrylonitrile spinning solution is 5wt%-15wt%.

7. The processing technology of a fiber cloth-based battery separator according to claim 5, characterized in that: The flow rate ratio of the polymethyl methacrylate spinning solution to the polyacrylonitrile spinning solution is 1:1-1:

5.

8. The processing technology of a fiber cloth-based battery separator according to claim 5, characterized in that: The component of the coagulation bath is a dimethylacetamide aqueous solution, the concentration of the dimethylacetamide aqueous solution is 5wt%-35wt%, the coagulation bath temperature is set to 40-60°C, and the fiber coagulation time is 10-15min; the water washing time is 10-15min, and the water washing temperature is room temperature; the stretching multiple is 5-6 times, and the stretching temperature is set to 70-80°C.

9. The processing technology of a fiber cloth-based battery separator according to claim 5, characterized in that: The sea island fiber pre-oxidation temperature is 200-300°C, the pre-oxidation time is 1.5-2h, the carbonization temperature is 600-1500°C, the carbonization time is 30-60min, the sea island fiber diameter is 0.8-1.2μm, and the ultrafine carbon fiber diameter is 300-500nm.

10. The processing technology of a fiber cloth-based battery separator according to claim 5, characterized in that: The hot rolling reinforcement temperature is 80-105°C, and the heat setting temperature is 95-105°C.

Citation Information

Patent Citations

  • Composite sea-island fiber synthetic needle-punched fabric

    CN105479872A

  • Preparation method of PA / PP porous battery separator material

    CN105789528A

  • Island-in-sea bicomponent spinning spinneret assembly and preparation method utilizing island-in-sea bicomponent spinning spinneret assembly for preparing superfine carbon fiber

    CN106192034A

  • Low-diameter high-strength polyacrylonitrile-based carbon fibers and preparation method thereof

    CN109402792A

  • Fiber cloth-based lithium ion battery diaphragm as well as preparation method and application thereof

    CN112038542A