Laminate, printed substrate, and printed substrate manufacturing method
By using an intermolecular interaction layer between the copper layer and the resist layer, combined with a nitrogen-containing heterocyclic compound, the problem of insufficient adhesion between the copper layer and the resist layer is solved, and low residue stripping and high-precision copper wiring are achieved Manufacturing, suitable for 5G and 6G communication technologies.
Patent Information
- Application Number
- CN202410447230.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-22
AI Technical Summary
In the manufacturing of printed circuit boards in the prior art, the adhesion between the copper layer and the etching resist layer is insufficient, resulting in cracks and high void frequency during high-temperature processes, and there is a lot of residue after the resist layer is peeled off, affecting the smoothness and smoothness of the copper wiring. Accuracy.
An intermolecular interaction layer is provided between the copper layer and the resist layer, containing a nitrogen-containing heterocyclic compound, and the surface roughness of the copper layer is below 0.3 μm. The adhesion is improved through the intermolecular interaction layer, and at the same time, during the process Optimize the stripping conditions of the resist layer.
It achieves high adhesion and low residue peeling between the copper layer and the resist layer, improves the smoothness and pattern accuracy of copper wiring, and reduces the frequency of cracks and voids in high-temperature processes.
Smart Images

Figure CN118829072A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminate, a printed circuit board, and a method for producing the printed circuit board.
[0002] More specifically, the present invention relates to a laminated body for producing a printed circuit board, wherein the copper layer has high smoothness, the copper layer and the resist layer have sufficient adhesion to form a desired copper wiring, and the residue after the resist layer is peeled off is small. Background Art
[0003] In recent years, with the development of digital society, copper wiring is required to be printed circuit boards with high density and high precision. In the manufacturing process of printed circuit boards, before the copper wiring is patterned by etching, an etching resist layer is bonded to the surface of the copper layer. In order to form high-density and high-precision copper wiring, high adhesion is required between the copper layer and the etching resist layer.
[0004] In the past, in order to improve the adhesion between the copper layer and the etching resist layer, the surface of the copper layer was roughened and bonded using the anchoring effect. However, the roughened surface of the copper layer may cause transmission loss to the short-wavelength radio waves used in communication technologies such as 5G and 6G. Therefore, it is necessary to improve the adhesion between the smooth copper layer and the etching resist layer without roughening.
[0005] As a method for improving the adhesion between a smooth copper layer and an etching resist layer, it is considered to provide an adhesive layer using an organic material between the copper layer and the etching resist layer. For example, in Patent Document 1, a surface treatment agent containing a triazole compound is disclosed as a material capable of improving the adhesion between a smooth metal layer and a resin layer.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2019-135295 Summary of the invention
[0009] However, it is known that when the surface treatment agent described in Patent Document 1 is used for the adhesive layer, the frequency of cracks and voids occurring in the high-temperature process during the production of the printed circuit board increases, or the insulating resin layer becomes easily peeled off.
[0010] As a result of intensive studies on the causes of the above-mentioned problems in the prior art, it was found that the cause of any of the problems is that a part of the peeled etching resist layer becomes a residue on the copper layer via the adhesive layer.
[0011] The present invention has been made in view of the above problems and circumstances, and the problem to be solved is to provide a laminated body for manufacturing a printed circuit board, in which the copper layer has high smoothness, the copper layer and the anti-etching layer have sufficient adhesion to form a desired copper wiring, and there is little residue after the anti-etching layer is peeled off. In addition, another problem to be solved by the present invention is to provide a printed circuit board with high smoothness on the surface of the copper wiring, high accuracy of the pattern of the copper wiring, and little residue of the anti-etching layer, and a method for manufacturing the printed circuit board.
[0012] The present inventors have studied the causes of the above problems to solve the above problems, and have found that the above problems can be solved by providing an intermolecular interaction layer between a copper layer having a surface roughness Ra of 0.3 μm or less and an anti-etching layer, thereby completing the present invention.
[0013] That is, the above-mentioned problems according to the present invention are solved by the following means.
[0014] 1. A laminated body, characterized in that it is a laminated body for manufacturing a printed circuit board, comprising: a copper layer, an anti-etching layer, and an intermolecular interaction layer for bonding the copper layer and the anti-etching layer,
[0015] The surface roughness Ra of the copper layer on the molecular interaction layer side is 0.3 μm or less.
[0016] 2. The laminate according to item 1, wherein the intermolecular interaction layer contains a nitrogen-containing heterocyclic compound.
[0017] 3. The laminate according to item 2, characterized in that the nitrogen-containing heterocyclic compound is a compound having both a nitrogen-containing heterocyclic ring and a functional group containing a nitrogen atom or an oxygen atom,
[0018] The number of nitrogen atoms in the nitrogen-containing heterocyclic ring is 2 to 4, and at least one of the nitrogen atoms is bonded to a hydrogen atom.
[0019] 4. The laminate according to item 3, characterized in that the functional group is -COOH, -NH2, -OH, -NHR or -NR2, and R represents an alkyl group.
[0020] 5. The laminate according to item 2, wherein the nitrogen-containing heterocyclic compound has a structure represented by the following general formula 1 or 2.
[0021]
[0022] [In the formula, W1 to W7 represent carbon atoms or nitrogen atoms. 2 to 4 of W1 to W7 represent nitrogen atoms, and at least one represents NH.
[0023] Y1 to Y5 represent a carbon atom or a nitrogen atom. Two to four of Y1 to Y5 represent nitrogen atoms, and at least one of them represents NH.
[0024] Z1 represents -COOH, -NH2, -OH, -NHR or -NR2. Z2 represents -COOH, -OH, -NHR or -NR2. R represents an alkyl group.
[0025] L represents a single bond or a linking group.]
[0026] 6. The laminate according to item 1, wherein the total amount of Zn, Cr, Ni and Sn present in the surface layer of the copper layer on the molecular interaction layer side is within a range of 0.001 to 1.000 at %.
[0027] 7. The laminate according to item 1, wherein the copper layer contains at least Zn.
[0028] 8. The laminate according to item 1, wherein the resist layer contains a photosensitive resin.
[0029] 9. A printed circuit board, characterized in that it has copper wiring,
[0030] The surface roughness Ra of the copper wiring is less than 0.3 μm,
[0031] There was no residue of the resist on the copper wiring.
[0032] 10. A method for manufacturing a printed circuit board, characterized in that a resist layer is used, and the method comprises the following steps:
[0033] Step (A): Cleaning the surface of the copper layer having a surface roughness Ra of 0.3 μm or less with a chemical solution,
[0034] Step (B): forming an intermolecular interaction layer directly above the cleaned copper layer,
[0035] Step (C): forming a resist layer containing a photosensitive resin directly above the intermolecular interaction layer,
[0036] Step (D): patterning the resist layer by exposure and development,
[0037] Step (E): patterning the copper layer by etching, and
[0038] Step (F): peeling off the resist layer and the intermolecular interaction layer.
[0039] 11. The method for producing a printed circuit board according to item 10, wherein the total amount of Zn, Cr, Ni and Sn present in the surface layer on the molecular interaction layer side of the copper layer in the step (B) is in the range of 0.001 to 1.000 at %.
[0040] 12. The method for producing a printed circuit board according to item 10, wherein the pH of the chemical solution used in the step (A) is 2 or less at 25°C.
[0041] 13. The method for producing a printed circuit board according to item 10, wherein the chemical solution used in the step (A) is an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid and nitric acid.
[0042] The above means of the present invention can provide a laminate for printed circuit board production, wherein the copper layer has high smoothness, the copper layer and the resist layer have sufficient adhesion to form a desired copper wiring, and there is little residue after the resist layer is peeled off.
[0043] Furthermore, the above-mentioned means of the present invention can provide a printed circuit board having high surface smoothness of copper wiring, high pattern accuracy of copper wiring and little residue of the resist layer, and a method for producing the printed circuit board.
[0044] The expression mechanism and action mechanism of the effect of the present invention are not yet clear, but are presumed as follows.
[0045] The residue of the etching resist layer causes cracks and voids. In addition, the residue of the etching resist layer prevents the insulating resin layer, which is often designed to ensure adhesion with copper, from contacting with copper, and thus makes the insulating resin layer easy to peel off.
[0046] The cause of the residue was studied, and it was found that the cause was in the adhesive layer. The surface treatment agent described in Patent Document 1 exerts a strong adhesive force by covalently bonding the copper layer and the etching resist layer through a triazole compound. In this technology, the adhesion between the copper layer and the etching resist layer can be ensured, and the desired copper wiring can be formed. However, the strong adhesive force obtained by such covalent bonding is too strong, which prevents the etching resist layer from being cleanly peeled off, and becomes the cause of the residue of the etching resist layer.
[0047] In contrast, the laminate of the present invention has an intermolecular interaction layer between the copper layer and the anti-etching layer to bond them. The intermolecular interaction layer can produce a level of adhesion sufficient to form a desired copper wiring between the copper layer and the anti-etching layer even when a copper layer with a surface roughness Ra of less than 0.3 μm and high smoothness is used. In addition, the intermolecular interaction is appropriately weaker than the covalent bond in terms of adhesion. Therefore, the intermolecular interaction layer is not easy to hinder the stripping of the etching resist layer, and the residue after the etching resist layer is stripped can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 is a schematic diagram showing the coordination state of the nitrogen-containing heterocyclic compound.
[0049] Figure 2 A diagram showing the steps of forming a copper wiring pattern (copper-clad laminate)
[0050] Figure 3 A diagram showing the steps of forming a copper wiring pattern (forming an intermolecular interaction layer)
[0051] Figure 4 A diagram showing a copper wiring pattern forming process (forming a resist layer)
[0052] Figure 5 A diagram showing the steps of forming a copper wiring pattern (patterning of a resist layer)
[0053] Figure 6 A diagram showing the steps of forming a copper wiring pattern (etching of a copper layer)
[0054] Figure 7 A diagram showing the steps of forming a copper wiring pattern (stripping of the resist layer and the molecular interaction layer)
[0055] Explanation of symbols
[0056] 1 Insulation layer
[0057] 2 copper layers
[0058] 3 Intermolecular Interaction Layer
[0059] 4. Anti-corrosion layer
[0060] 5 Copper Clad Laminated Board
[0061] 6-Layered
[0062] 7Copper wiring pattern DETAILED DESCRIPTION
[0063] The surface modifier of the present invention is characterized in that it is a laminate for producing a printed circuit board, comprising a copper layer, an anti-etching layer, and an intermolecular interaction layer bonding the copper layer and the anti-etching layer, wherein the surface roughness Ra of the copper layer on the intermolecular interaction layer side is 0.3 μm or less.
[0064] This feature is the same or corresponding technical feature in the following embodiments.
[0065] As an embodiment of the laminate of the present invention, it is preferable that the intermolecular interaction layer contains a nitrogen-containing heterocyclic compound. The nitrogen-containing heterocyclic compound has high adhesion-improving properties because nitrogen atoms thereof are likely to strongly interact with components of the copper layer.
[0066] As an embodiment of the laminate of the present invention, the nitrogen-containing heterocyclic compound is preferably a compound having both a nitrogen-containing heterocyclic ring and a functional group containing a nitrogen atom or an oxygen atom, the number of nitrogen atoms in the nitrogen-containing heterocyclic ring is 2 to 4, and at least one of the nitrogen atoms is bonded to a hydrogen atom. Thus, the nitrogen atom bonded to the hydrogen atom interacts with the metal to form a coordination bond, thereby improving the adhesion with the copper layer.
[0067] As an embodiment of the laminate of the present invention, the functional group is preferably -COOH, -NH2, -OH, -NHR or -NR2, and R represents an alkyl group. As a result, the functional group can form a hydrogen bond or an ionic bond with the polar group of the resin contained in the anti-corrosion layer. As a result, the nitrogen-containing heterocyclic compound can be closely bonded to the anti-corrosion layer with a stronger interaction force than π-π interaction and van der Waals force. In terms of improving the adhesion between the copper layer and the anti-corrosion layer, it is particularly preferred that the nitrogen-containing heterocyclic compound has a structure represented by the general formula 1 or the general formula 2.
[0068] As an embodiment of the laminate of the present invention, the total amount of Zn, Cr, Ni and Sn present in the surface layer on the molecular interaction layer side of the copper layer is preferably within the range of 0.001 to 1.000 at%. When the total amount is 0.001 at% or more, it becomes easy to appropriately peel off the anti-corrosion layer with these atoms as an opportunity. When the total amount is 1.000 at% or less, it is not easy to damage the adhesion between the copper layer and the anti-corrosion layer, and the adhesion between the copper layer and the insulating resin layer.
[0069] As an embodiment of the laminated body of the present invention, it is preferable that the copper layer contains at least Zn. This facilitates the peeling of the resist layer more appropriately due to Zn.
[0070] As an embodiment of the laminated body of the present invention, it is preferable that the resist layer contains a photosensitive resin. Thereby, the resist layer can be patterned by photolithography.
[0071] The printed circuit board of the present invention is characterized by having copper wiring, the surface roughness Ra of the copper wiring being 0.3 μm or less, and no residue of the etching resist layer being left on the copper wiring.
[0072] The method for producing a printed circuit board of the present invention is characterized by comprising the above steps (A) to (F) using a resist layer.
[0073] As an embodiment of the method for manufacturing a printed circuit board of the present invention, it is preferred that the total amount of Zn, Cr, Ni and Sn present in the surface layer on the molecular interaction layer side of the copper layer in the step (B) is within the range of 0.001 to 1.000 at%. By making the total amount 0.001 at% or more, it becomes easy to appropriately peel off the anti-corrosion layer with these atoms as an opportunity. By making the total amount 1.000 at% or less, it is not easy to damage the adhesion between the copper layer and the anti-corrosion layer, and the adhesion between the copper layer and the insulating resin layer.
[0074] As an embodiment of the method for producing a printed circuit board of the present invention, from the viewpoint of cleaning properties, the pH of the chemical solution used in the step (A) is preferably 2 or less at 25°C.
[0075] As an embodiment of the method for producing a printed circuit board of the present invention, from the viewpoint of cleaning properties, the chemical solution used in the step (A) is preferably an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid and nitric acid.
[0076] Hereinafter, the present invention and its constituent elements and modes and embodiments for carrying out the present invention will be described in detail. In the present application, "to" is used to include the numerical values described before and after it as the lower limit and the upper limit.
[0077] [Overview of the Laminated Body of the Present Invention]
[0078] The laminate of the present invention is a laminate for producing a printed circuit board, comprising a copper layer, a resist layer, and an intermolecular interaction layer bonding the copper layer and the resist layer. The surface roughness Ra of the copper layer on the intermolecular interaction layer side is 0.3 μm or less.
[0079] Figure 4 It is a schematic cross-sectional view of the stacked body 6 . Figure 4 The laminated body 6 illustrated in FIG. 4 includes an insulating layer 1 , a copper layer 2 , an intermolecular interaction layer 3 , and a resist layer 4 .
[0080] [Intermolecular interaction layer]
[0081] The "intermolecular interaction layer" according to the present invention refers to a layer that is bonded to at least one of the copper layer and the resist layer by a means other than forming a covalent bond as a main bonding means.
[0082] "Means other than forming a covalent bond" mainly refers to intermolecular interactions, but may also be a combination of intermolecular interactions and adsorption due to an anchoring effect, etc. Intermolecular interactions include electrostatic interactions, van der Waals forces, hydrogen bonds, charge transfer interactions, hydrophobic interactions, and the like.
[0083] The copper layer and the anti-etching layer of the laminate are bonded via the intermolecular interaction layer, which can be confirmed by the absence of silicon atoms (Si) between the bonded copper layer and the anti-etching layer. The absence of silicon atoms (Si) can be confirmed by secondary ion mass spectrometry (SIMS). In the case of the presence of silicon atoms (Si), it is believed that the copper layer and the anti-etching layer are bonded via a covalent bond of a compound containing silicon atoms (Si).
[0084] The intermolecular interaction layer contains at least a compound capable of intermolecular interaction with the components of the copper layer described later (hereinafter also referred to as "compound A"). The compound A contained in the intermolecular interaction layer may be one kind or two or more kinds. The intermolecular interaction layer may contain compounds other than compound A within a range that does not hinder the effect of the present invention.
[0085] Compound A is preferably non-photosensitive. “Non-photosensitive” means a property that light is not absorbed to break intramolecular bonds or polymerize molecules under normal conditions in the process of forming the intermolecular interaction layer.
[0086] Compound A is preferably a nitrogen-containing compound, and more preferably a nitrogen-containing heterocyclic compound. These compounds have high adhesion-improving properties because nitrogen atoms of these compounds are likely to strongly interact with the components of the copper layer.
[0087] The nitrogen-containing heterocyclic compound is preferably a compound having both a nitrogen-containing heterocyclic ring and a functional group containing a nitrogen atom or an oxygen atom.
[0088] The number of nitrogen atoms in the nitrogen-containing heterocyclic ring is preferably 2 to 4 and at least one of the nitrogen atoms is bonded to a hydrogen atom. Thus, the nitrogen atom bonded to the hydrogen atom interacts with the metal to form a coordinate bond, thereby further improving adhesion to the copper layer.
[0089] As the functional group containing nitrogen atoms or oxygen atoms, -COOH, -NH2, -OH, -NHR or -NR2 is preferred. The functional group is particularly preferably -COOH, -NH2 or -NR2. It should be noted that R represents an alkyl group. Thus, the functional group can form a hydrogen bond or an ionic bond with the polar group of the resin contained in the anti-etching layer. As a result, the nitrogen-containing heterocyclic compound can be closely attached to the anti-etching layer with a stronger interaction force than π-π interaction and van der Waals force.
[0090] The nitrogen-containing heterocyclic compound preferably has a structure represented by the following general formula 1 or 2 in terms of improving the adhesion between the copper layer and the resist layer.
[0091]
[0092] [In the formula, W1 to W7 represent carbon atoms or nitrogen atoms. 2 to 4 of W1 to W7 represent nitrogen atoms, and at least one represents NH.
[0093] Y1 to Y5 represent a carbon atom or a nitrogen atom. Two to four of Y1 to Y5 represent nitrogen atoms, and at least one of them represents NH.
[0094] Z1 represents -COOH, -NH2, -OH, -NHR or -NR2. Z2 represents -COOH, -OH, -NHR or -NR2. R represents an alkyl group.
[0095] L represents a single bond or a linking group.]
[0096] W1 to W7 form a condensed ring.
[0097] Y1 to Y7 form a condensed ring.
[0098] The connecting group represented by L is, for example, an atom or an atomic group containing a carbon atom, a nitrogen atom, a sulfur atom, or an oxygen atom. Specific examples of the connecting group represented by L include -O-, -S-, -N(R)-, -CO-, -SO2-, an alkylene group, an arylene group, and combinations thereof. R represents a hydrogen atom, an alkyl group, or a cycloalkyl group. Examples of alkylene groups include methylene, ethylene, propylene, 1,4-cyclohexylene, dodecylene, hexadecylene, 2-ethylhexylene, 2-hexyldecylene, and the like. Examples of arylene groups include phenylene, naphthylene, and the like.
[0099] like Figure 1 As shown, the molecular skeleton of the nitrogen-containing heterocyclic compound having the structure represented by Formula 1 or Formula 2 is easily coordinated in the vertical direction (thickness direction of the intermolecular interaction layer 3) in the intermolecular interaction layer 3. Figure 1 In the figure, the orientation of the nitrogen-containing heterocyclic compound is shown by taking the exemplary compound (1) described later as an example. The nitrogen atom in the ring skeleton of the nitrogen-containing heterocyclic compound interacts with the metal of the copper layer 2 by coordinating the molecular skeleton of the nitrogen-containing heterocyclic compound in the vertical direction. As a result, the alkylamino group, which is a functional group of the nitrogen-containing heterocyclic compound, can be brought close to the anti-corrosion layer 4. As a result, the nitrogen-containing heterocyclic compound also interacts with the anti-corrosion layer 4. The nitrogen-containing heterocyclic compound improves their adhesion by interacting with both the copper layer 2 and the anti-corrosion layer 3 in this way.
[0100] The following are examples of nitrogen-containing heterocyclic compounds having a structure represented by Formula 1 or Formula 2. The nitrogen-containing heterocyclic compound according to the present invention is not limited thereto.
[0101]
[0102]
[0103] [Copper layer]
[0104] The copper layer is a layer containing copper or a copper alloy as a main component. The "main component" refers to a component containing 50% by mass or more.
[0105] The copper alloy may contain gold, silver, platinum, zinc, palladium, rhodium, osmium, ruthenium, iridium, copper, nickel, cobalt, iron, tin, chromium, titanium, tantalum, tungsten, indium, aluminum, lead, molybdenum, etc. The proportion of copper in the copper alloy is preferably 50 at % or more.
[0106] The copper layer of the laminate of the present invention is characterized in that the surface roughness Ra of the molecular interaction layer side is less than 0.3 μm. As a result, the copper wiring formed by the copper layer is less likely to cause cracks and voids in the high-temperature process during manufacturing, and less likely to cause transmission loss of short-wavelength radio waves used in 5G or 6G communication technologies.
[0107] The surface roughness Ra is the arithmetic mean roughness defined in JIS B 0601: 2013. The surface roughness Ra can be measured using, for example, a laser microscope (LASERMICROSCOPE VK-X100 manufactured by KEYENCE CORPORATION).
[0108] The total amount of Zn, Cr, Ni and Sn present in the surface layer on the molecular interaction layer side of the copper layer is preferably in the range of 0.001 to 1.000 at% when the total amount of elements present in the surface layer is set to 100 at%. By making the total amount 0.001 at% or more, it becomes easy to appropriately peel off the anti-corrosion layer with these atoms as an opportunity. By making the total amount 1.000 at% or less, it is not easy to damage the adhesion between the copper layer and the anti-corrosion layer, and the adhesion between the copper layer and the insulating resin layer.
[0109] The copper layer preferably contains at least Zn. The amount of Zn present in the surface layer on the molecular interaction layer side of the copper layer is preferably in the range of 0.001 to 0.100 at% when the total amount of elements present in the surface layer is set to 100 at%. By making the amount of Zn more than 0.100 at%, it becomes easy to appropriately peel off the anti-corrosion layer with Zn as an opportunity. By making the amount of Zn less than 0.100 at%, it is not easy to damage the adhesion between the copper layer and the anti-corrosion layer, and the adhesion between the copper layer and the insulating resin layer.
[0110] The element composition of the surface of the copper layer was measured by the following procedure.
[0111] First, a sample with a known elemental composition on the surface is used to create a standard curve for the elemental content. The standard curve for the range above 0.1 at% is created using data from X-ray photoelectron spectroscopy (XPS). The standard curve for the range less than 0.1 at% is created using data from secondary ion mass spectrometry (SIMS). Next, the elemental composition of the surface of the copper layer of the object to be measured is analyzed by XPS and SIMS. The elemental composition of the surface of the copper layer is determined based on the analysis value and the standard curve.
[0112] XPS was performed under the following conditions.
[0113] XPS measurement device: Quantera SXM (manufactured by ULVAC-PHI)
[0114] X-ray source: monochromatic Al-Kα ray, 100μm, 25W, 15kV
[0115] Signal extraction angle: 45 degrees
[0116] Analysis area: 500μm×500μm
[0117] In XPS, first, a wide scan is performed with a pass energy of 224 eV over a binding energy range of -20 to 1270 eV to find out which elements are detected. Next, a narrow scan is performed with a pass energy of 140 eV for all detected elements. The wide scan and narrow scan are measured at different locations on the same sample. The elemental composition of the surface of the copper layer is quantified using MultiPak, an analysis software made by ULVAC-PHI. For the spectrum of each element, the background is calculated using the Shirley method for elements other than copper, and the background is calculated using the linear method for copper. The elemental composition of the surface of the copper layer is obtained using the relative sensitivity factor method based on the peak area obtained.
[0118] In SIMS, the strength of various metal ions was measured under the following conditions.
[0119]
[0120] The copper layer may be a metal foil, a plated layer, or the like, or may be a film formed by a vacuum film forming method or the like.
[0121] The thickness of the copper layer is not particularly limited. The thickness of the copper layer may be, for example, a thickness corresponding to the thickness of the copper wiring pattern to be formed.
[0122] The copper layer may be a copper layer of a copper-clad laminate in which a copper layer is formed on an insulating layer. In this case, the insulating layer of the copper-clad laminate is, for example, a resin sheet or a prepreg.
[0123] [Resist layer]
[0124] The resist layer is a layer that has an etching resistance function against etching of the copper layer. For example, a UV-curable epoxy resin containing an alkali-soluble resin, a UV-curable acrylic resin, a polyimide, or the like is preferably used for the resist layer.
[0125] The resist preferably contains a photosensitive resin. Thus, the resist can be patterned by photolithography. The resist containing the photosensitive resin can be a negative type in which the photosensitive portion is changed into a pattern by exposure, or a positive type in which the non-photosensitive portion is changed into a pattern by exposure.
[0126] [Manufacturing method of printed circuit board]
[0127] The laminate of the present invention can be used to produce a printed circuit board. The printed circuit board includes a printed wiring board (PWB) before electronic components are mounted and a printed circuit board (PCB) after electronic components are mounted.
[0128] In the production of a printed circuit board using the laminate of the present invention, for example, formation of a copper wiring pattern is performed through the following steps.
[0129] Step (A): A step of cleaning the surface of a copper layer having a surface roughness Ra of 0.3 μm or less using a chemical solution
[0130] Step (B): a step of forming an intermolecular interaction layer directly above the cleaned copper layer
[0131] Step (C): a step of forming a resist layer containing a photosensitive resin directly above the intermolecular interaction layer
[0132] Step (D): a step of patterning the resist layer by exposure and development
[0133] Step (E): a step of patterning the copper layer by etching
[0134] Step (F): a step of peeling off the resist layer and the intermolecular interaction layer
[0135] use Figures 2 to 7 Examples of each of the above steps will be described.
[0136] In step (A), the surface of the copper layer having a surface roughness Ra of 0.3 μm or less is cleaned with a chemical solution, thereby removing dirt, antioxidants, oxide films, etc. attached to the surface of the copper layer 2 that hinder the interaction between the molecular interaction layer 3 and the copper layer 2. Figure 2 An example using a copper-clad laminate 5 in which a copper layer 2 is formed on an insulating layer 1 is shown.
[0137] The pH of the chemical solution used in step (A) at 25° C. is preferably 2 or less from the viewpoint of cleaning properties.
[0138] From the viewpoint of cleaning properties, the chemical solution used in step (A) is preferably an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid, and nitric acid.
[0139] After step (A), the surface of the copper layer 2 may be washed with water.
[0140] The insulating layer 1 is an insulating layer serving as a base material of a printed circuit board. The insulating layer 1 is made of an insulating material such as a resin, and may be a prepreg in which a base material such as paper or glass is impregnated with a resin.
[0141] In step (B), the molecular interaction layer 3 is formed directly on the cleaned copper layer 2 (see Figure 3 ). Specifically, the intermolecular interaction layer forming composition is applied directly on the copper layer 2 to form the intermolecular interaction layer 3 .
[0142] The composition for forming an intermolecular interaction layer contains a compound (compound A) capable of intermolecular interaction with components of the copper layer.
[0143] In terms of solubility, the composition preferably contains at least water or alcohol as a solvent. Examples of the alcohol include methanol, ethanol, and 2-propanol.
[0144] The solvent may be water or two or more alcohols. Specifically, the mass ratio of water to alcohol is preferably within the range of 100:0 to 50:50, more preferably within the range of 100:0 to 75:25.
[0145] The content of the compound A in the composition for forming an intermolecular interaction layer used in the step (B) is, for example, 0.001 to 0.1% by mass.
[0146] The composition for forming an intermolecular interaction layer may contain other components other than those mentioned above within a range that does not inhibit the effects of the present invention. Examples of other components include surfactants, preservatives, stabilizers, acids, bases, pH adjusters, and the like.
[0147] Preferably, the copper-clad laminate 5 having the intermolecular interaction layer 3 formed thereon is washed with water between step (B) and the subsequent step (C). This can remove excess components of the composition for forming the intermolecular interaction layer that do not interact sufficiently with the copper layer 2.
[0148] In step (C), a resist layer 4 containing a photosensitive resin is formed directly on the intermolecular interaction layer 3 (see Figure 4 ). The laminate 6 in this state includes: an insulating layer 1, a copper layer 2, an intermolecular interaction layer 3, and an anti-corrosion layer 4.
[0149] The resist layer 4 can be formed by laminating a resist dry film or applying a liquid resist material.
[0150] In step (D), the resist layer 4 is patterned by exposure and development (see Figure 5 Specifically, first, the resist layer 4 is exposed using a photomask capable of exposing the resist layer 4 in an arbitrary pattern. Then, the resist layer 4 is patterned by dissolving and removing unnecessary portions in the resist layer 4 using a developer.
[0151] The resist layer 4 is preferably washed with water after development.
[0152] The exposure conditions and the development conditions are not particularly limited, and conventionally known exposure conditions and development conditions can be applied.
[0153] In step (E), the copper layer 2 is patterned by etching through the resist layer 4 (see Figure 6 Specifically, by wet etching using an etching solution, the molecular interaction layer 3 and the copper layer 2 are dissolved in the portion where the resist layer 4 is removed. Thus, the copper layer 2 is patterned. At this time, the molecular interaction layer 3 can also be patterned together with the copper layer 2.
[0154] The etching conditions are not particularly limited, and conventionally known etching conditions can be applied.
[0155] In step (F), the resist layer 4 and the molecular interaction layer 3 are peeled off from the copper-clad laminate 5 (see Figure 7 ).
[0156] The method for stripping the resist layer 4 and the intermolecular interaction layer 3 is not particularly limited, but it is preferred to use a stripping solution for stripping. The stripping solution is not particularly limited, and a conventionally known stripping solution can be used.
[0157] Through the above steps, the copper wiring pattern 7 can be formed.
[0158] The use of the molecular interaction layer 3 in the method for forming the copper wiring pattern 7 increases the adhesion between the copper layer 2 and the resist layer 4 in step (E). This prevents the etching solution from penetrating between the copper layer 2 and the resist layer 4, and enables the formation of a high-density and high-definition copper wiring pattern 7.
[0159] [Printed substrate]
[0160] By using the laminated body of the present invention, it is possible to produce a printed circuit board having copper wirings with a surface roughness Ra of 0.3 μm or less and having no resist residue on the copper wirings.
[0161] Such a printed circuit board is not likely to cause transmission loss of short-wavelength radio waves by making the surface roughness Ra of the copper wiring less than 0.3 μm, so it can be appropriately used in 5G and 6G communication technologies. In addition, since such a printed circuit board has no residue of the anti-etching layer on the copper wiring, the frequency of cracks and gaps generated in the high-temperature process during manufacturing is low. In addition, since such a printed circuit board has no residue of the anti-etching layer on the copper wiring, the insulating resin layer formed on the copper wiring is not easy to peel off.
[0162] Example
[0163] The present invention is specifically described below with reference to the examples, but the present invention is not limited thereto. It should be noted that in the following examples, unless otherwise specified, the operation is performed at room temperature (25° C.). In addition, unless otherwise specified, “%” and “parts” represent “mass %” and “mass parts”, respectively.
[0164] [Preparation of treatment solution and copper-clad laminate]
[0165] <Preparation of treatment solution>
[0166] The compounds listed in Table I were added to a solvent consisting of 20 mass % of ethanol and 80 mass % of ion-exchanged water to give 20 mass ppm to prepare treatment liquids 1 to 26. Treatment liquids 1 to 24 are compositions for forming an intermolecular interaction layer.
[0167] [Table 1]
[0168] Table I
[0169] Treatment fluid No. Compound 1 Exemplary compounds (1) 2 Exemplary compounds (2) 3 Example compounds (3) 4 Exemplary compounds (4) 5 Exemplary compounds (5) 6 Exemplary compounds (6) 7 Exemplary compounds (7) 8 Exemplary compounds (8) 9 Exemplary compounds (9) 10 Exemplary compounds (10) 11 Exemplary compounds (11) 12 Exemplary compounds (12) 13 Exemplary compounds (13) 14 Exemplary compounds (14) 15 Exemplary compounds (15) 16 Exemplary compounds (16) 17 Exemplary compounds (17) 18 Exemplary compounds (18) 19 Exemplary compounds (19) 20 Exemplary compounds (20) 21 Exemplary compounds (21) 22 Exemplary compounds (22) 23 Exemplary compounds (23) 24 Exemplary compounds (24) 25 Comparative Compound A 26 Comparative Compound B
[0170] Comparative compounds A and B are compounds having the following structures, respectively. Comparative compounds A and B are compounds that form covalent bonds with components contained in the copper layer and components contained in the resist layer.
[0171] Comparative Compound A
[0172]
[0173] Comparative Compound B
[0174]
[0175] <Adjustment of Surface Roughness Ra of Copper Layer of Copper-Clad Laminate>
[0176] A copper-clad laminate (R-1766 manufactured by Panasonic Corporation) having a metal layer formed on an insulating layer was half-etched with a sulfuric acid-hydrogen peroxide system (sulfuric acid peroxide system) etching solution. The etching time was adjusted to produce copper-clad laminates A to C having the following surface roughness Ra of the copper layer.
[0177] Copper clad laminate A: surface roughness Ra = 0.25 μm
[0178] Copper clad laminate B: surface roughness Ra = 0.10 μm
[0179] Copper clad laminate C: surface roughness Ra = 0.35 μm
[0180] [Example 1]
[0181] <Production of laminates and printed wiring boards>
[0182] The steps (A) to (C) are performed as follows to produce the laminate 1 .
[0183] [Process (A)]
[0184] The copper-clad laminate A prepared as described above was cleaned with a hydrochloric acid cleaning solution (manufactured by Sanwa Chemical Industry Co., Ltd., CP-30). Next, the copper-clad laminate A was cleaned using a chemical solution (hydrochloric acid, pH 1.1) and a spray-type cleaning device. Next, the copper layer was washed with water.
[0185] [Process (B)]
[0186] The treatment solution 1 prepared above was applied to the copper layer using a spray coating device. The surface coated with the treatment solution was then washed with water. The processed product was then dehydrated with a PVA roller and dried with an air knife at 80° C. to form a 5 nm thick intermolecular interaction layer.
[0187] 〔Process (C)〕
[0188] The anti-etching dry film (AK-4034 manufactured by Asahi Kasei Corporation) was laminated on the intermolecular interaction layer using a hot roll laminator. The lamination conditions were a roll temperature of 105°C, an air pressure of 0.35 MPa, and a lamination speed of 1.5 m / min. The anti-etching dry film (AK-4034 manufactured by Asahi Kasei Corporation) used had a support composed of a polyethylene terephthalate film on one side and a protective layer composed of a polyethylene film on the other side. The lamination was performed in such a way that the surface with the protective layer was bonded to the copper layer via an adhesive layer while peeling off the protective layer. Thus, an anti-etching layer was formed.
[0189] Through the above steps (A) to (C), a laminate 1 including a copper layer, an intermolecular interaction layer, and a resist layer is produced.
[0190] <Production of Laminated Bodies 2 to 7>
[0191] In the preparation of laminate 1, the copper-clad laminate and the treatment liquid were changed as shown in Table II, and laminates 2 to 7 were prepared in the same manner. It should be noted that laminates 5 and 6 have a covalent bond layer instead of an intermolecular interaction layer. Since step (B) is not performed in the preparation of laminate 7, laminate 7 does not have an intermolecular interaction layer.
[0192] <Manufacturing of printed wiring boards>
[0193] Using each of the produced laminated bodies, steps (D) to (F) were carried out as described below to produce a printed wiring board.
[0194] [Process (D)]
[0195] The resist layer of the laminate was exposed using a chrome glass mask and a parallel light exposure machine (HMW-801 manufactured by OAK). The exposure conditions were the recommended conditions for the resist dry film, i.e., 60 mj / cm 2 .
[0196] The support is peeled off from the exposed resist layer. Then, a developer consisting of a 1 mass % aqueous solution of sodium carbonate (Na2CO3) and an alkali developer are used to dissolve and remove the unexposed portion of the resist layer, thereby developing. The developing conditions are a temperature of 30°C and a developing time of 3 minutes. Next, the processed product is washed with water.
[0197] By the above operation, the resist layer was patterned so that the circuit width of the copper wiring pattern after etching would be 140 μm and the circuit length would be 760 mm.
[0198] [Process (E)]
[0199] The intermolecular interaction layer (or covalent bond layer) and the copper layer were etched by immersion using an etching solution consisting of an aqueous solution of 2 mass % hydrogen chloride (HCl) and 2 mass % ferric chloride (FeCl3). The etching conditions were a temperature of 30°C and an immersion time of 1 minute.
[0200] Through the above operations, the intermolecular interaction layer (or covalent bond layer) and the copper layer are patterned.
[0201] [Process (F)]
[0202] The resist layer and the intermolecular interaction layer (or the covalent bond layer) were peeled off from the copper-clad laminate at a temperature of 50° C. using a stripping solution consisting of a 3 mass % aqueous solution of sodium hydroxide (NaOH).
[0203] Through the above operations, a printed wiring board is manufactured.
[0204] <Evaluation of Adhesion of Resist Layer>
[0205] The copper wiring pattern on the printed wiring board was observed under a microscope, and the adhesion of the resist layer was evaluated according to the following criteria. The evaluation results are shown in Table II. "AA" and "A" were evaluated as having no practical problems.
[0206] AA: The residual rate of copper wiring is 97% or more.
[0207] A: The residual rate of copper wiring is 95% or more and less than 97%.
[0208] B: The residual rate of copper wiring is less than 95%.
[0209] <Evaluation of peelability of resist layer>
[0210] The copper wiring pattern on the printed wiring board was observed using a microscope. Based on the results of the observation and the time required for step (F), the peelability of the anti-etching layer was evaluated according to the following criteria. The evaluation results are shown in Table II. "AA" and "A" were evaluated as having no practical problems.
[0211] AA: There is no residue of the resist layer, and the time until the resist layer is completely peeled off is shortened.
[0212] A: Although there was no residue of the resist layer, the time until the resist layer was completely peeled off was not shortened.
[0213] B: Residue of the resist layer exists.
[0214] <Evaluation of transmission loss>
[0215] A low dielectric polyphenylene ether resin film (manufactured by Panasonic, multilayer substrate material MEGTRON7, thickness 60 μm) was used to form a stripline. The circuit formed on the copper foil of the printed wiring board was transmitted using a network analyzer N5291A manufactured by Keysight Technologies to transmit high-frequency signals and measure transmission loss. The characteristic impedance was 50Ω. According to the transmission loss at a frequency of 30 GHz, the transmission loss was evaluated according to the following benchmarks. The evaluation results are shown in Table II. "AA" and "A" were evaluated as having no practical problems.
[0216] AA: Transmission loss exceeds -25dB / 760mm.
[0217] A: The transmission loss exceeds -28dB / 760mm and is less than -25dB / 760mm.
[0218] B: Transmission loss is less than -28dB / 760mm.
[0219] [Table 2]
[0220] Table II
[0221]
[0222] According to the results of Example 1, it can be seen that the copper layer of the laminate of the present invention has high smoothness, the copper layer and the anti-etching layer have sufficient adhesion to form the desired copper wiring, and the residue after the anti-etching layer is peeled off is small. In addition, it can be seen that the surface of the copper wiring of the printed circuit board produced using the laminate of the present invention has high smoothness, the pattern accuracy of the copper wiring is high, and the residue of the anti-etching layer is small.
[0223] [Example 2]
[0224] Laminated bodies 8 to 31 were prepared and evaluated using the treatment liquids shown in Table III in the same manner as in Example 1. The evaluation results are shown in Table III.
[0225] [Table 3]
[0226] Table III
[0227]
[0228] From the results of Example 2, it was confirmed that by making the intermolecular interaction layer contain any one of the exemplary compounds (1) to (24), a laminated body can be produced in which the copper layer has high smoothness, the copper layer and the anti-etching layer have sufficient adhesion to form the desired copper wiring, and the residue after the anti-etching layer is peeled off is small.
[0229] [Example 3]
[0230] Laminated bodies 32 to 42 were produced and evaluated using the treatment liquids shown in Table IV in the same manner as in Example 1. The evaluation results are shown in Table IV.
[0231] It should be noted that in Example 3, the chemical solution shown in Table V was used instead of the chemical solution (hydrochloric acid, pH 1.1) in the chemical solution cleaning of the copper-clad laminate in step (A). The pH of the chemical solution shown in Table V is the value at 25° C. In addition, the time for chemical solution cleaning with the chemical solution shown in Table V was adjusted as shown in Table V.
[0232] Chemical solution A is a 0.4 mass % aqueous solution of hydrogen chloride (hydrochloric acid).
[0233] Chemical solution B is a 5 mass % aqueous solution of hydrogen chloride (hydrochloric acid).
[0234] Chemical solution C is a 5 mass % aqueous solution of sodium carbonate.
[0235] Chemical solution D is a 0.01 mass % aqueous solution of formic acid.
[0236] Chemical solution E is a 0.05 mass % aqueous solution of sulfuric acid.
[0237] Chemical solution F is a 0.04 mass % aqueous solution of nitric acid.
[0238] The element amounts [at %] of Zn, Cr, Ni and Sn present in the surface layer on the molecular interaction layer side of the copper layer used in the stacked bodies 32 to 42 when the total amount of elements present in the surface layer is set to 100 at % are measured between steps (A) and (B) by the following method.
[0239] First, a sample with a known surface elemental composition is used to create a calibration curve for elemental content. The calibration curve for the range above 0.1 at% is created using data from X-ray photoelectron spectroscopy (XPS). The calibration curve for the range below 0.1 at% is created using data from secondary ion mass spectrometry (SIMS).
[0240] Next, the elemental composition of the surface of the copper layer to be measured is analyzed by XPS and SIMS, and the elemental composition of the surface of the copper layer is obtained based on the analysis value and the calibration curve.
[0241] XPS was performed under the following conditions.
[0242] XPS measurement device: Quantera SXM (manufactured by ULVAC-PHI)
[0243] X-ray source: monochromatic Al-Kα ray, 100μm, 25W, 15kV
[0244] Signal extraction angle: 45 degrees
[0245] Analysis area: 500μm×500μm
[0246] In XPS, first, a wide scan is performed with a pass energy of 224 eV over a binding energy range of -20 to 1270 eV to find out which elements are detected. Next, a narrow scan is performed with a pass energy of 140 eV for all detected elements. The wide scan and narrow scan are measured at different locations on the same sample. The elemental composition of the surface of the copper layer is quantified using MultiPak, an analysis software made by ULVAC-PHI. For the spectrum of each element, the background is calculated using the Shirley method for elements other than copper, and the background is calculated using the linear method for copper. The elemental composition of the surface of the copper layer is obtained using the relative sensitivity factor method based on the peak area obtained.
[0247] In SIMS, the strength of various metal ions was measured under the following conditions.
[0248] Device: TRIFT5 nanoTOF (manufactured by ULVAC-PHI)
[0249] Primary ion: Bi3 ++
[0250] Primary ion current: 2.0pA
[0251] Data collection time: 60 seconds
[0252] Repetition frequency: 8.2kHz
[0253] Charge neutralization: ON
[0254] Secondary ion polarity: Positive
[0255] Mass scanning range: m / z = 0.5 ~ 2000
[0256] The measurement results are shown in Table V. "-" in Table V indicates that the amount of the element is less than the detection limit (0.001 at %) of the above measurement method.
[0257] [Table 4]
[0258] Table IV
[0259]
[0260] [Table 5]
[0261] Table V
[0262]
[0263] From the results of Example 3, the following can be confirmed.
[0264] By changing the type of chemical solution and the cleaning time in step (A), the amount of different types of metals (metals other than Cu) on the surface of the copper layer can be adjusted.
[0265] There is a tendency that the adhesion between the copper layer and the resist layer becomes better as the number of different types of metals on the surface of the copper layer decreases.
[0266] There is a tendency that the more different types of metal there are on the surface of the copper layer, the better the peeling property of the resist layer will be.
[0267] Furthermore, from the above, it was confirmed that the adhesion and peelability of the resist layer can be controlled by the conditions of the step (A).
Claims
1. A laminate, characterized in that: The invention relates to a laminate for manufacturing a printed circuit board, comprising a copper layer, an anti-etching layer, and an intermolecular interaction layer for bonding the copper layer and the anti-etching layer. The surface roughness Ra of the copper layer on the molecular interaction layer side is 0.3 μm or less.
2. The laminate according to claim 1, characterized in that The intermolecular interaction layer contains a nitrogen-containing heterocyclic compound.
3. The laminate according to claim 2, characterized in that The nitrogen-containing heterocyclic compound is a compound having both a nitrogen-containing heterocyclic ring and a functional group containing a nitrogen atom or an oxygen atom. The number of nitrogen atoms in the nitrogen-containing heterocyclic ring is 2 to 4, and at least one of the nitrogen atoms is bonded to a hydrogen atom.
4. The laminate according to claim 3, characterized in that The functional group is -COOH, -NH2, -OH, -NHR or -NR2, and R represents an alkyl group.
5. The laminate according to claim 2, characterized in that The nitrogen-containing heterocyclic compound has a structure represented by the following general formula 1 or general formula 2: In the formula, W1 to W7 represent carbon atoms or nitrogen atoms, 2 to 4 of W1 to W7 represent nitrogen atoms, and at least 1 represents NH. Y1 to Y5 represent a carbon atom or a nitrogen atom, 2 to 4 of Y1 to Y5 represent nitrogen atoms, and at least one of them represents NH, Z1 represents -COOH, -NH2, -OH, -NHR or -NR2, Z2 represents -COOH, -OH, -NHR or -NR2, R represents an alkyl group, L represents a single bond or a linking group.
6. The laminate according to claim 1, characterized in that The total amount of Zn, Cr, Ni and Sn present in the surface layer of the copper layer on the molecular interaction layer side is in the range of 0.001 to 1.000 at %.
7. The laminate according to claim 1, wherein: The copper layer contains at least Zn.
8. The laminate according to claim 1, wherein: The resist layer contains a photosensitive resin.
9. A printed circuit board, characterized in that: With copper wiring, The surface roughness Ra of the copper wiring is less than 0.3 μm, There was no residue of the resist on the copper wiring.
10. A method for manufacturing a printed circuit board, characterized in that: Using a resist layer, The process is as follows: Step (A): Cleaning the surface of the copper layer having a surface roughness Ra of 0.3 μm or less with a chemical solution, Step (B): forming an intermolecular interaction layer directly above the cleaned copper layer, Step (C): forming a resist layer containing a photosensitive resin directly above the intermolecular interaction layer, Step (D): patterning the resist layer by exposure and development, Step (E): patterning the copper layer by etching, and Step (F): peeling off the resist layer and the intermolecular interaction layer.
11. The method for manufacturing a printed circuit board according to claim 10, characterized in that: The total amount of Zn, Cr, Ni and Sn present in the surface layer on the molecular interaction layer side of the copper layer in the step (B) is within the range of 0.001 to 1.000 at %.
12. The method for manufacturing a printed circuit board according to claim 10, wherein: The pH of the chemical solution used in the step (A) is 2 or less at 25°C.
13. The method for manufacturing a printed circuit board according to claim 10, characterized in that: The chemical solution used in the step (A) is an aqueous solution containing at least one of formic acid, hydrogen chloride, sulfuric acid and nitric acid.