Ion implanted thick film resist composition, method of manufacturing processed substrate using same, and method of manufacturing device using same
By using polymers and photoacid generators with specific structures in ion implantation resists, combined with optical exposure technology, the problems of insufficient rectangularity, resolution and heat resistance of resist patterns in the existing technology are solved, and high-quality photo-acid generators are achieved. Transparency and high aspect ratio resist pattern suitable for high energy ion implantation processes.
Patent Information
- Application Number
- CN202380024606.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-27
- Publication Date
- 2024-10-22
AI Technical Summary
Existing ion implantation resist compositions have deficiencies in squareness, resolution, heat resistance and transmittance, making it difficult to form resist patterns with high aspect ratio, high squareness and heat resistance.
An ion-implanted thick film resist composition containing a polymer with a specific structure, a photoacid generator and a solvent is used to form high transparency, high rectangularity and heat resistance through the combination of specific repeating units of the polymer and the photoacid generator. resist film, and prepare resist patterns through optical exposure and development techniques.
It achieves a resist pattern with high rectangularity, resolution and heat resistance, improves the transmittance of the resist film and the stability of the pattern, and is suitable for high-energy ion implantation processes.
Smart Images

Figure CN118829945A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an ion implantation thick film resist composition, a method for manufacturing a processed substrate using the same, and a method for manufacturing a device using the same. Background Art
[0002] In the manufacture of semiconductor devices, an ion implantation process is used to introduce impurity ions into a semiconductor substrate using a resist pattern as a mask. The impurity ions are implanted at high energy using an ion implantation device. As designs become more sophisticated and the amount of ion implantation increases, the resist pattern used in the ion implantation process is required to be thicker, more rectangular, and more heat-resistant.
[0003] Thick film resist compositions have been proposed for plating steps, etching steps, and the like (for example, Patent Document 1), but improvements in resolution and rectangularity are still required.
[0004] Thick film resist compositions have been proposed for high energy ion implantation processes, but improvements in resolution and the like are still required (for example, Patent Document 2).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2007-206425
[0008] Patent document 2: International Publication No. 2004 / 104702 Summary of the invention
[0009] Technical Problems to be Solved by the Invention
[0010] The inventors of the present invention believe that there are still one or more problems that need to be improved regarding ion implantation resist compositions and their use. Examples of these problems include: failure to obtain a resist pattern with sufficiently high rectangularity; failure to obtain sufficient resolution; insufficient ion implantation resistance of the resist pattern; low transmittance of the resist film; failure to form a resist pattern with a high aspect ratio; and insufficient heat resistance of the resist pattern.
[0011] The present invention has been accomplished based on the above-mentioned technical background, and provides an ion implantation thick film resist composition and a method for manufacturing a processed substrate using the same.
[0012] Solutions for solving technical problems
[0013] The ion implantation thick film resist composition of the present invention comprises a polymer (A), a photoacid generator (B) and a solvent (C).
[0014] The resist film formed from the above composition has a film thickness of 1.0 to 50 μm.
[0015] The mass average molecular weight of polymer (A) is 5,000 to 19,000, and
[0016] The polymer (A) contains at least one of the repeating units represented by the formulae (A-1), (A-2), (A-3) and (A-4).
[0017]
[0018] in,
[0019] R 11 , R 21 , R 41 and R 45 Each is independent of C 1-5 Alkyl, wherein the methylene group in the alkyl may be replaced by an oxy group;
[0020] R 12 , R 13 , R 14 , R 22 , R 23 , R 24 , R 32 , R 33 , R 34 , R 42 , R 43 , and R 44 are independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH;
[0021] p11 is 0 to 4, p15 is 1 to 2, p11+p15≤5,
[0022] p21 is 0 to 5,
[0023] p41 is 0-4, p45 is 1-2, p41+p45≤5;
[0024] P 31 C 4-20 Alkyl groups, wherein a part or all of the alkyl groups may form a ring, a part or all of the H groups in the alkyl groups may be substituted by halogen, and the methylene groups in the alkyl groups may be replaced by oxy groups or carbonyl groups.
[0025] The method for manufacturing a processed substrate of the present invention comprises the following steps:
[0026] Using the above-mentioned ion implantation thick film resist composition to manufacture a resist pattern; and
[0027] Ion implantation is performed using the resist pattern as a mask, or
[0028] The lower layer of the resist pattern is processed using the resist pattern as a mask to form a lower layer pattern, and ion implantation is performed using the lower layer pattern as a mask.
[0029] The method for manufacturing a device of the present invention includes the method for manufacturing a processed substrate as described above.
[0030] Effects of the Invention
[0031] In the process of reaching the present invention, the idea of the inventors is as follows. Since the resist pattern itself as a mask can also be reduced by the injection of ionized impurities, it is necessary to form a thick resist film. In order to form a thick film, the transparency of the film is required to be high. The thicker the film, the higher the rectangularity required. Furthermore, since the ion implantation resist pattern will generate heat in the process, it is also necessary to have excellent heat resistance. The inventors conducted in-depth research and obtained the composition of the present invention.
[0032] According to the present invention, one or more of the following effects can be expected.
[0033] A resist pattern with high rectangularity can be obtained; a resist film with high resolution can be obtained; the resist pattern has high ion implantation resistance; the resist film has high transmittance; a resist pattern with high aspect ratio can be formed; and the resist pattern has high heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 A schematic diagram showing the cross-sectional shape of a groove pattern.
[0035] Figure 2 A schematic diagram showing the cross-sectional shape of a resist pattern having different Wt / Wb. DETAILED DESCRIPTION
[0036] [definition]
[0037] In this specification, unless otherwise specified or mentioned, the definitions and examples described in this paragraph shall apply.
[0038] The singular includes the plural, and “a” and “the” mean “at least one.” An element of a certain concept may be expressed in plural forms, and when the amount (eg, mass % or mol %) thereof is described, the amount means the total of the plural types.
[0039] "And / or" includes all combinations of elements and also includes individual uses.
[0040] When "to" or "- / to" is used to express a numerical range, both endpoints are included and the units are common. For example, 5 to 25 mol% means 5 mol% or more and 25 mol% or less.
[0041] “Cx-y ”, “C x ~C y ” and “C x " refers to the number of carbon atoms in a molecule or substituent. For example: C 1-6 The alkyl group means an alkyl chain having 1 to 6 carbon atoms (such as methyl, ethyl, propyl, butyl, pentyl, and hexyl).
[0042] In the case where the polymer has a plurality of repeating units, these repeating units are copolymerized. These copolymerizations may be alternating copolymerizations, random copolymerizations, block copolymerizations, graft copolymerizations, or any of these mixed forms. When a polymer or resin is represented by a structural formula, n, m, etc. outside the brackets represent the number of repetitions.
[0043] The unit of temperature is Celsius. For example, 20 degrees means 20 degrees Celsius.
[0044] The additive refers to the compound itself having the function (for example, if it is a base generator, it is the compound itself that generates the base). It can also be a method in which the compound is dissolved or dispersed in a solvent and added to the composition. As one embodiment of the present invention, these solvents are preferably contained in the composition of the present invention as solvent (C) or other components.
[0045] The following is a detailed description of the embodiments of the present invention.
[0046] <Ion implantation thick film resist composition>
[0047] The ion-implanted thick-film resist composition of the present invention (hereinafter sometimes referred to as a composition) comprises a polymer (A) having a specific structure, a photoacid generator (B), and a solvent (C).
[0048] The composition of the present invention is a thick film resist composition. In the present invention, thick film refers to a film with a thickness of 1.0 to 50 μm, preferably a film with a thickness of 1.2 to 30 μm (more preferably 1.5 to 20 μm, and further preferably 2 to 10 μm). The viscosity of the composition of the present invention is preferably 10 to 1,000 mPa·s; more preferably 12 to 500 mPa·s. The viscosity is a value measured at 25°C using a capillary viscometer.
[0049] The composition of the present invention is preferably a KrF chemically amplified resist composition; more preferably a KrF positive chemically amplified resist composition.
[0050] Polymer (A)
[0051] The composition of the present invention comprises a polymer (A). The polymer (A) comprises at least one of the repeating units represented by the following formulae (A-1), (A-2), (A-3) and (A-4). The polymer (A) is a polymer that reacts with an acid and increases its solubility in an alkaline aqueous solution. Such a polymer is, for example, the following: having an acid group protected by a protecting group, when an acid is added from the outside, the protecting group is detached, and the solubility in an alkaline aqueous solution increases.
[0052] Formula (A-1) is as follows.
[0053]
[0054] Among them, R 11 Each is independent of C 1-5 Alkyl (wherein the methylene group in the alkyl group may be replaced by an oxy group); preferably a methyl group or an ethyl group; more preferably a methyl group. In the present invention, the expression "the methylene group in the alkyl group may be replaced by an oxy group" means that an oxy group may exist between carbon atoms in the alkyl group, but it is not intended that the terminal carbon atoms in the alkyl group become oxy groups, that is, it is not intended to have alkoxy groups or hydroxy groups.
[0055] R 12 , R 13 , and R 14 are independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH; preferably hydrogen or methyl; more preferably hydrogen.
[0056] p11 is 0 to 4; preferably 0 or 1; more preferably 0.
[0057] p15 is 1 to 2, preferably 1.
[0058] p11+p15≤5.
[0059] The polymer (A) may contain a plurality of repeating units represented by the formula (A-1). For example, it may contain a structural unit with p15=1 and a structural unit with p15=2 in a ratio of 1:1. In this case, p15=1.5 as a whole. The numerical values representing the polymers in the present invention are the same unless otherwise specified.
[0060] Specific examples of the formula (A-1) include the following.
[0061]
[0062] Formula (A-2) is as follows.
[0063]
[0064] Among them, R 21 Each is independent of C1-5 Alkyl (wherein the methylene group in the alkyl group may be replaced by an oxy group); preferably methyl, ethyl, tert-butyl or tert-butoxy; more preferably methyl or ethyl; more preferably methyl.
[0065] R 22 , R 23 , and R 24 are independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH; preferably hydrogen, or methyl; more preferably hydrogen.
[0066] p21 is 0 to 5; preferably 0, 1, 2, 3, 4 or 5; more preferably 0 or 1; further preferably 0.
[0067] Specific examples of the formula (A-2) include the following.
[0068]
[0069] Formula (A-3) is as follows.
[0070]
[0071] Among them, R 32 , R 33 and R 34 are independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy or -COOH; preferably hydrogen, methyl, ethyl, tert-butyl, methoxy, tert-butoxy or -COOH; more preferably hydrogen or methyl; further preferably hydrogen.
[0072] P 31 C 4-20 Alkyl. Part or all of the alkyl group may form a ring, part or all of the H in the alkyl group may be replaced by halogen, and the methylene group in the alkyl group may be replaced by an oxy group or a carbonyl group. 31 The alkyl portion of is preferably branched or cyclic. 31 C 4-20 When the alkyl group is substituted with halogen, it is preferably completely substituted, and the substituted halogen is preferably F or Cl; more preferably F. 31 C 4-20 It is an ideal embodiment of the present invention that the H of the alkyl group is not substituted by halogen. 31 Preferred is methyl, isopropyl, tert-butyl, cyclopentyl, methylcyclopentyl, ethylcyclopentyl, cyclohexyl, methylcyclohexyl, ethylcyclohexyl, adamantyl, methyladamantyl or ethyladamantyl; more preferably tert-butyl, ethylcyclopentyl, ethylcyclohexyl or ethyladamantyl; further preferably tert-butyl, ethylcyclopentyl or ethyladamantyl; further preferably tert-butyl.
[0073] Specific examples of the formula (A-3) include the following.
[0074]
[0075] Formula (A-4) is as follows.
[0076]
[0077] Among them, R 41 Each is independent of C 1-5 Alkyl (wherein the methylene group in the alkyl group may be replaced by an oxy group); preferably methyl, ethyl or tert-butyl; more preferably methyl.
[0078] R 45 Each is independent of C 1-5 Alkyl (wherein the methylene group in the alkyl group may be replaced by an oxy group); preferably methyl, tert-butyl or -CH(CH3)-O-CH2CH3.
[0079] R 42 , R 43 , and R 44 are independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH; preferably hydrogen or methyl; more preferably hydrogen.
[0080] p41 is 0 to 4; more preferably 0 or 1; further preferably 0.
[0081] p45 is 1 to 2; more preferably 1.
[0082] p41+p45≤5.
[0083] Specific examples of the formula (A-4) include the following.
[0084]
[0085] These structural units can be appropriately blended depending on the purpose, and it is a preferred embodiment to blend them so that the solubility in an alkaline aqueous solution increases in a suitable ratio due to acid.
[0086] The following is the number of repeating units n of the repeating units (A-1), (A-2), (A-3) and (A-4) in the polymer (A): A-1 、n A-2 、n A-3 and n A-4 Provide explanation.
[0087] n A-1 / (n A-1 +n A-2+n A-3 +n A-4 ) is preferably 40 to 80%; more preferably 50 to 80%; further preferably 55 to 75%; further preferably 55 to 65%.
[0088] n A-2 / (n A-1 +n A-2 +n A-3 +n A-4 ) is preferably 0 to 40%; more preferably 0 to 30%; further preferably 5 to 25%; further preferably 15 to 25%.
[0089] n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 ) is preferably 10 to 50%; more preferably 10 to 40%; further preferably 15 to 35%; further preferably 15 to 25%.
[0090] n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 ) is preferably 0 to 40%; more preferably 0 to 30%; further preferably 0 to 10%; further preferably 0 to 5%. n A-4 A preferred embodiment of the present invention is 0. A-1 / (n A-1 +n A-2 +n A-3 +n A-4 )=40~80%、n A-2 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~40%、n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 ) = 10 to 50%, and n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 )=0 to 40% can be mentioned as a preferred embodiment.
[0091] As one embodiment of the present invention, n A-3 >0 and n A-4 =0.
[0092] The polymer (A) may contain further repeating units other than the repeating units represented by (A-1), (A-2), (A-3) and (A-4).
[0093] Still further repeating units are preferably repeating units comprising an arylcarbonyl group.
[0094] The content of the further repeating unit contained in the polymer (A) is preferably 0 to 10 parts by mass, more preferably 0 to 5 parts by mass, and even more preferably 0 to 1 part by mass, relative to 100 parts by mass of the polymer (A). It is also a preferred embodiment of the polymer (A) that the further repeating unit is not contained. In other words, it is also a preferred embodiment that the repeating unit containing an aromatic carbonyl group is not contained.
[0095] Specific examples of the polymer (A) include the following.
[0096]
[0097] The mass average molecular weight (hereinafter sometimes referred to as Mw) of the polymer (A) is 5,000 to 19,000, more preferably 8,000 to 19,000, further preferably 10,000 to 19,000, and further preferably 11,000 to 13,000. Without being bound by theory, it is believed that a polymer (A) having such Mw enables a resist pattern having good rectangularity or resolution to be formed from the composition of the present invention.
[0098] In the present invention, Mw can be measured by gel permeation chromatography (GPC). In this measurement, a GPC column is set at 40 degrees Celsius, an elution solvent of tetrahydrofuran is set at 0.6 mL / min, and monodisperse polystyrene is used as a standard, which is a preferred example.
[0099] The following is for the sake of explanation. In the composition of the present invention, as long as the polymer (A) is represented by the above formula, two or more polymers may be used in combination. For example, a composition containing the following two polymers (A) at the same time is also one embodiment of the present invention.
[0100]
[0101] The composition of the present invention shall apply the same in the following description unless otherwise specified.
[0102] The polymer (A) contained in the composition of the present invention comprises one or two polymers, and preferably comprises one polymer. Deviations in Mw distribution and polymerization are allowed.
[0103] The content of the polymer (A) is preferably 10 to 40% by mass, more preferably 12 to 38% by mass, and further preferably 15 to 36% by mass, based on the composition.
[0104] The composition of the present invention may contain a polymer other than the polymer (A), but an embodiment in which no polymer other than the polymer (A) is contained is a preferred embodiment.
[0105] Photoacid generator (B)
[0106] The composition of the present invention comprises a photoacid generator (B). The photoacid generator (B) releases an acid by irradiation with light. Preferably, the acid derived from the photoacid generator (B) acts on the polymer (A) to increase the solubility of the polymer (A) in alkaline aqueous solution. For example, when the polymer (A) has an acid group protected by a protecting group, the protecting group is detached by the acid. The photoacid generator (B) used in the composition of the present invention can be selected from those known in the past.
[0107] The photoacid generator (B) releases an acid having an acid dissociation constant pKa (H2O) of preferably -20 to 1.4 upon exposure; more preferably -16 to 1.4; further preferably -16 to 1.2; and further preferably -16 to 1.1.
[0108] The photoacid generator (B) is preferably represented by formula (B-1).
[0109] B n+ Cation B n- Anion (B-1)
[0110] Among them, B n+ The cation is a cation represented by formula (BC1), a cation represented by formula (BC2), or a cation represented by formula (BC3); preferably, it is a cation represented by formula (BC1) or a cation represented by (BC2); more preferably, it is a cation represented by (BC1). n+ The cation is generally n-valent, where n is 1-3.
[0111] B n- The anion is a sulfonic acid anion, preferably an anion represented by formula (BA1), an anion represented by formula (BA2), an anion represented by formula (BA3), or an anion represented by formula (BA4); more preferably, an anion represented by formula (BA3). n- Anions are generally n-valent.
[0112] n is preferably 1 or 2; more preferably 1.
[0113] Without being bound by theory, it is believed that by using the above-mentioned photoacid generator (B), it is possible to control the photoacid generator (B) to be present in large quantities near the bottom surface when forming the resist film, and it is possible to control the pattern shape to be rectangular. The positive resist dissolves the exposed part, but since the amount of light reaching decreases as it approaches the bottom surface of the resist film, it is effective to control the pattern shape by the amount of photoacid generator (B) present.
[0114] Formula (BC1) is as follows.
[0115]
[0116] Among them, R b1 Each is independent of C 1-6 Alkyl, C 1-6 Alkoxy, C 6-12 Aryl, C 6-12 Arylthio, or C 6-12 Aryloxy; preferably methyl, ethyl, tert-butyl, methoxy, ethoxy, phenylthio, or phenoxy; more preferably tert-butyl, methoxy, ethoxy, phenylthio, or phenoxy.
[0117] nb1 is independently 0, 1, 2 or 3; preferably 0 or 1, more preferably 0.
[0118] Specific examples of the formula (BC1) include the following.
[0119]
[0120] Formula (BC2) is as follows.
[0121]
[0122] Among them, R b2 Each is independent of C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 Aryl; preferably having C 4-6 The alkyl group of the branched chain structure. b2 They may be the same or different, but the same is more preferred. b2 More preferred is tert-butyl or 1,1-dimethylpropyl; further preferred is tert-butyl.
[0123] nb2 is independently 0, 1, 2 or 3; preferably 1.
[0124] Specific examples of the formula (BC2) include the following.
[0125]
[0126] Formula (BC3) is as follows.
[0127]
[0128] Among them, R b3 are independently hydroxyl, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 Aryl; preferably methyl, ethyl, methoxy, or ethoxy; more preferably methyl or methoxy.
[0129] R b4 Each is independent of C 1-6 Alkyl; preferably methyl, ethyl, propyl, or butyl. 2 R b4 They may be bonded to each other to form a ring structure, and when forming a ring, it is preferably a 5-membered or 6-membered alicyclic ring.
[0130] nb3 is independently 0, 1, 2 or 3; preferably 1, 2 or 3; more preferably 1 or 3.
[0131] Specific examples of the formula (BC3) include the following.
[0132]
[0133] Formula (BA1) is as follows.
[0134]
[0135] Among them, R b5 Each is independent of C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, or C 1-6 Alkyl. For example, -CF3 means that all hydrogen atoms of a methyl group (C1) are replaced by fluorine atoms. In the present invention, fluorine substitution means that part or all of the hydrogen atoms present in the alkyl moiety are replaced by fluorine atoms, and more preferably, all of the hydrogen atoms are replaced by fluorine atoms.
[0136] R b5 The alkyl portion of is preferably methyl, ethyl or tert-butyl, more preferably methyl.
[0137] R b5 Preferred is a fluorine-substituted alkyl group; more preferred is -CF3.
[0138] Specific examples of the formula (BA1) include the following.
[0139]
[0140] Formula (BA2) is as follows.
[0141]
[0142] Among them, R b6 C 1-10 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, C 6-12 Fluorine-substituted aryl, C 2-12 Fluorine-substituted acyl, or C 6-12 Fluorine-substituted alkoxyaryl; preferably C 1-10 Fluorine-substituted alkyl. b6 The alkyl portion of R is preferably linear or cyclic. b6 Preferably C 1-6 Fluorine-substituted alkyl; more preferably C 2-6 Fluorine substituted alkyl group.
[0143] Specific examples of the formula (BA2) include the following.
[0144]
[0145] Formula (BA3) is as follows.
[0146]
[0147] Among them, R b7 Each is independent of C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, C 6-12 Fluorine-substituted aryl, C 2-12 Fluorine-substituted acyl, or C 6-12 Fluorine-substituted alkoxyaryl; preferably C 2-6 Fluorine substituted alkyl. Two R b7 They may also be bonded to each other to form a fluorine-substituted heterocyclic structure. The heterocyclic structure is preferably a saturated ring. The heterocyclic structure contains N and S, and is preferably a monocyclic structure with 5 to 8 members; more preferably a five-membered ring or a six-membered ring; and even more preferably a six-membered ring.
[0148] Specific examples of the formula (BA3) include the following.
[0149]
[0150] Formula (BA4) is as follows.
[0151]
[0152] Among them, R b8 For hydrogen, C 1-6 Alkyl, C 1-6 Alkoxy or hydroxy; preferably hydrogen, methyl, ethyl, methoxy or hydroxy; more preferably hydrogen or hydroxy.
[0153] L bIt is methylene, ethylene, carbonyl, oxy or carbonyloxy; preferably ethylene or carbonyl.
[0154] Y b Each independently represents hydrogen or fluorine; preferably, at least one of them is fluorine.
[0155] nb4 is an integer from 0 to 10; preferably 0, 1 or 2.
[0156] nb5 is an integer from 0 to 21; preferably 4, 5 or 6.
[0157] Specific examples of the formula (BA4) include the following.
[0158]
[0159] The molecular weight of the photoacid generator (B) is preferably 300 to 1,200; more preferably 400 to 900.
[0160] The content of the photoacid generator (B) is preferably 0.3 to 4 parts by mass, more preferably 0.4 to 2 parts by mass, and further preferably 0.5 to 2 parts by mass relative to 100 parts by mass of the polymer (A). Although not limited to theory, it is believed that a resist pattern with better resolution can be formed by the content of the photoacid generator (B) being within the above range.
[0161] The composition of the present invention may contain a photoacid generator other than the photoacid generator (B), for example, a photoacid generator (B') represented by the following formula (B'-1) may be mentioned. In the present invention, the photoacid generator (B') is different from the photoacid generator (B). As a preferred embodiment of the present invention, the acid that directly acts on the polymer (A) is an acid released by the photoacid generator (B), not an acid released by the photoacid generator (B').
[0162] As a preferred embodiment of the present invention, the cation derived from the photoacid generator (B') partially reacts with the anion derived from the photoacid generator (B) to function as a quencher. In this case, the photoacid generator (B') inhibits the diffusion of the acid derived from the photoacid generator (B) generated in the exposed part and functions as a quencher.
[0163] The photoacid generator (B') is represented by the formula (B'-1).
[0164] B ’m+ Cation B ’m- Anion (B-1)
[0165] in,
[0166] B ’m+ The cation is a cation represented by the above formula (BC1) or a cation represented by the formula (BC2). The preferred embodiment is also the same as above.
[0167] B ’m+ The cation is generally m-valent, where m is 1-3.
[0168] B ’m- The anion is an anion represented by formula (B'A1) or an anion represented by formula (B'A2). ’m- Anions are generally m-valent.
[0169] m is preferably 1 or 2; more preferably 1.
[0170] Formula (B'A1) is as follows.
[0171]
[0172] Among them, X 1 C 1-20 of hydrocarbons or single bonds,
[0173] R b’1 are independently hydrogen, hydroxyl, C 1-6 Alkyl, or C 6-10 Aryl,
[0174] nb'1 is 1, 2, or 3, and
[0175] nb'2 is 0, 1, or 2.
[0176] When X 1 When it is a hydrocarbon, it may be any of a straight chain, a branched chain, or a cyclic chain, but is preferably a straight chain or a cyclic chain. When it is a straight chain, it is preferably C 1-4 (More preferably C 1-2 ), preferably has one double bond in the chain, or is saturated. When cyclic, it may be a monocyclic aromatic ring, or a saturated monocyclic or polycyclic ring, when a monocyclic ring, preferably a 6-membered ring, when a polycyclic ring, preferably an adamantane ring.
[0177] X 1 Preferred are methyl, ethyl, propyl, butyl, ethane, phenyl, cyclohexane, adamantane or a single bond; more preferred are methyl, phenyl, cyclohexane or a single bond; further preferred are phenyl or a single bond; further preferred are phenyl.
[0178] nb'1 is preferably 1 or 2; more preferably 1.
[0179] nb'2 is preferably 0 or 1; more preferably 1.
[0180] R b’1 Preferred is hydroxy, methyl, ethyl, 1-propyl, 2-propyl, tert-butyl, or phenyl; more preferred is hydroxy.
[0181] When X 1 When it is a single bond, Rb’1 Preferably, it is hydrogen. 1 is a single bond, R b’1 (B'A1) where nb'1 = nb'2 = 1 represents H-COO - anion.
[0182] Specific examples of the formula (B'A1) include the following.
[0183]
[0184] Formula (B'A2) is as follows.
[0185]
[0186] Among them, R b’2 C 1-20 Alkyl (wherein a part or all of the alkyl group may form a ring, and -CH2- in the alkyl group may be replaced by -C(=O)-) b’2 Preferably C 3-13 Alkyl; more preferably C 5-12 Alkyl; more preferably C 8-12 Alkyl; more preferably C 10 Alkyl. b’2 The alkyl group of is preferably partially or entirely formed into a ring; more preferably partially formed into a ring. b’2 One or more (more preferably one) -CH2- groups in the alkyl group are replaced by -C(=O)-.
[0187] Specific examples of the formula (B'A2) include the following.
[0188]
[0189] The photoacid generator (B') releases an acid having an acid dissociation constant pKa (H2O) of preferably 1.5 to 8, and more preferably 1.5 to 5, upon exposure.
[0190] The molecular weight of the photoacid generator (B') is preferably 300 to 1,400; more preferably 300 to 1,200.
[0191] The content of the photoacid generator (B') is preferably 0.01 to 5% by mass based on the polymer (A), more preferably 0.03 to 1% by mass, further preferably 0.05 to 1% by mass, and further preferably 0.5 to 1% by mass. Not containing the photoacid generator (B') is also a preferred embodiment of the present invention.
[0192] Solvent (C)
[0193] The composition of the present invention contains a solvent (C). The solvent is not particularly limited as long as it can dissolve the components to be blended.
[0194] Specific examples of the solvent include water, n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, 2,2,4-trimethylpentane, n-octane, isooctane, cyclohexane, methylcyclohexane, benzene, toluene, xylene, ethylbenzene, trimethylbenzene, methylethylbenzene, n-propylbenzene, isopropylbenzene, diethylbenzene, isobutylbenzene, triethylbenzene, diisopropylbenzene, n-pentylnaphthalene, trimethylbenzene, methanol, ethylbenzene, alcohol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, sec-pentanol, tert-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, sec-hexanol, 2-ethylbutanol, sec-heptanol, heptanol-3, n-octanol, 2-ethylhexanol, sec-octanol, n-nonanol, 2,6-dimethylheptanol-4, n-decanol, sec-undecyl alcohol, trimethylnonanol, sec-tetradecanol, sec-decyl alcohol Heptane, phenol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, phenylmethylcarbinol, diacetone alcohol, cresol, ethylene glycol, propylene glycol, 1,3-butanediol, pentanediol-2,4, 2-methylpentanediol-2,4, hexanediol-2,5, heptanediol-2,4, 2-ethylhexanediol-1,3, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, acetone, methyl ethyl Ketone, methyl n-propyl ketone, methyl n-butyl ketone, diethyl ketone, methyl isobutyl ketone, methyl n-amyl ketone, ethyl n-butyl ketone, methyl n-hexyl ketone, diisobutyl ketone, trimethyl nonanone, cyclohexanone, cyclopentanone, methyl cyclohexanone, 2,4-pentanedione, acetone acetone, diacetone alcohol, acetophenone, fenchone, ethyl ether, isopropyl ether, n-butyl ether (di-n-butyl ether, DBE), n-hexyl ether, 2-ethylhexyl ether, ethylene oxide, 1,2-propylene oxide, dioxolane, 4-methyldioxolane, dioxane, dimethyldioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-n-hexyl ether, ethylene glycol monophenyl ether, ethylene glycol mono-2-ethyl butyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol di-n-butyl ether, diethylene glycol mono-n-hexyl ether, ethoxytriethylene glycol (ethoxy triglycol), tetraethylene glycol di-n-butyl ether, propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, diethyl carbonate, methyl acetate, ethyl acetate, γ-butyrolactone, γ-valerolactone, n-propyl acetate, isopropyl acetate, n-butyl acetate (nBA), isobutyl acetate, sec-butyl acetate, n-pentyl acetate, sec-pentyl acetate, 3-methoxybutyl acetate, Methyl amyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, benzyl acetate, cyclohexyl acetate, methylcyclohexyl acetate, n-nonyl acetate, methyl acetoacetate, ethyl acetoacetate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl acetate, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, ethylene glycol diacetate, methoxytriethylene glycol acetate (methoxy triglycol acetate), ethyl propionate, n-butyl propionate, isoamyl propionate, diethyl oxalate, di-n-butyl oxalate, methyl lactate, ethyl lactate (EL), γ-butyrolactone, n-butyl lactate, n-amyl lactate, diethyl malonate, dimethyl phthalate, diethyl phthalate, propylene glycol 1-monomethyl ether 2-acetate (PGMEA), propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, N-methylformamide, N,N-dimethylformamide, N,N-diethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropionamide, N-methylamide, N-methylpyrrolidone, dimethyl sulfide, diethyl sulfide, thiophene, tetrahydrothiophene, dimethyl sulfoxide, sulfolane, and 1,3-propane sultone. These solvents can be used alone or in combination of two or more.
[0195] The solvent (C) is preferably propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, n-butyl acetate, n-butyl ether, 2-heptanone, cyclohexanone, or any combination thereof; more preferably PGME, EL, nBA, DBE, or any mixture thereof; further preferably PGME, EL, or a mixture thereof; and further preferably a mixture of PGME and EL. When two solvents are mixed, the mass ratio of the first solvent to the second solvent is preferably 95:5 to 5:95 (more preferably 90:10 to 10:90, and further preferably 80:20 to 20:80).
[0196] Based on the relationship with other layers and films, the solvent (C) does not substantially contain water, which is also a mode. For example, the amount of water in the solvent (C) as a whole is preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and further preferably 0.001% by mass or less. It is also a preferred mode that the solvent (C) does not contain water (0% by mass).
[0197] The content of the solvent (C) is preferably 50 to 90% by mass, more preferably 60 to 88% by mass, and even more preferably 65 to 85% by mass based on the composition. The thickness of the film after film formation can be controlled by increasing or decreasing the amount of the solvent in the entire composition.
[0198] Basic compound (D)
[0199] The composition of the present invention may further contain a basic compound (D). The basic compound has the effect of suppressing the diffusion of acid generated in the exposed area and the effect of suppressing the deactivation of acid on the resist film surface caused by amine components contained in the air.
[0200] Preferred examples of the alkaline compound (D) include ammonia, C 1-16 Aliphatic primary amines, C 2-32 Aliphatic secondary amines, C 3-48 Aliphatic tertiary amines, C 6-30 Aromatic amines, C 5-30 Heterocyclic amines and their derivatives.
[0201] Specific examples of the base compound (D) include ammonia, ethylamine, n-octylamine, n-heptylamine, ethylenediamine, triethylamine, tri-n-octylamine, diethylamine, tri[2-(2-methoxyethoxy)ethyl]amine, 1,8-diazabicyclo[5.4.0]undecene-7, 1,5-diazabicyclo[4.3.0]nonene-5, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
[0202] The base dissociation constant pKb(H2O) of the basic compound (D) is preferably -12 to 5, more preferably 1 to 4.
[0203] The molecular weight of the base compound (D) is preferably 17-500, more preferably 60-400.
[0204] The content of the basic compound (D) is preferably 0.01 to 5 parts by mass, and more preferably 0.05 to 2 parts by mass, based on 100 parts by mass of the polymer (A).
[0205] Surfactant (E)
[0206] The composition of the present invention may further include a surfactant (E). By including a surfactant, the coating property can be improved. As the surfactant that can be used in the present invention, there can be listed: (I) anionic surfactants, (II) cationic surfactants or (III) nonionic surfactants, more specifically: (I) alkyl sulfonates, alkylbenzene sulfonic acid, and alkylbenzene sulfonates, (II) lauryl pyridinium chloride and lauryl methyl ammonium chloride, and (III) polyoxyethylene octyl ether, polyoxyethylene lauryl ether, polyoxyethylene acetylene glycol ether, fluorine-containing surfactants (e.g., Fluorad (3M), Megaface (DIC), Sulfron (AGC), and organosiloxane surfactants (e.g., KF-53, KP341 (Shin-Etsu Chemical Industry)).
[0207] These surfactants may be used alone or in combination of two or more. The content of the surfactant (E) is preferably 0.005 to 1 part by mass, and more preferably 0.01 to 0.2 parts by mass, based on 100 parts by mass of the polymer (A).
[0208] Dye(F)
[0209] The composition of the present invention may further contain a dye (F). By containing the dye (F), the pattern shape can be improved.
[0210] The content of the dye (F) is preferably 0 to 0.5 parts by mass relative to 100 parts by mass of the polymer (A); more preferably 0 to 0.2 parts by mass; and further preferably 0 to 0.1 parts by mass. Since the resist film of the present invention preferably has a high transmittance, it is preferred that the dye is not substantially contained. It is also a more preferred embodiment of the present invention that the composition of the present invention does not contain the dye (F) (0 parts by mass).
[0211] Additives (G)
[0212] The composition of the present invention may further contain an additive (G) other than the above-mentioned components. The additive (G) is preferably a surface smoothing agent, a plasticizer, a contrast enhancer, an acid, a radical generator, a substrate adhesion enhancer, a defoaming agent, or any combination thereof.
[0213] The content of the additive (G) (the sum of the additives in the case of multiple types) is preferably 0 to 5 parts by mass, more preferably 0 to 3 parts by mass, and even more preferably 0 to 1 part by mass relative to 100 parts by mass of the polymer (A). It is also one embodiment of the present invention that the composition of the present invention does not contain the additive (G) (0 parts by mass).
[0214] Acids may be used to adjust the pH of the composition and to improve the solubility of additive components. The acid used is not particularly limited, but examples thereof include formic acid, acetic acid, propionic acid, benzoic acid, phthalic acid, salicylic acid, lactic acid, malic acid, citric acid, oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, aconitic acid, glutaric acid, adipic acid, and combinations thereof.
[0215] In the present invention, the content of salicylic acid is preferably 0 to 0.005 parts by mass, more preferably 0 to 0.001 parts by mass, based on 100 parts by mass of the polymer (A). It is also one embodiment of the present invention that the composition of the present invention does not contain salicylic acid (0 parts by mass).
[0216] <Method for Manufacturing Processed Substrate>
[0217] The method for manufacturing a processed substrate of the present invention includes the following steps.
[0218] Using the composition of the present invention to produce a resist pattern; and
[0219] Ion implantation is performed using the resist pattern as a mask, or
[0220] The lower layer of the resist pattern is processed using the resist pattern as a mask to form a lower layer pattern, and ion implantation is performed using the lower layer pattern as a mask.
[0221] One embodiment of the production method of the present invention is described below.
[0222] The composition of the present invention is applied by an appropriate method on a substrate (e.g., a silicon / silicon dioxide coated substrate, a silicon nitride substrate, a silicon wafer substrate, a glass substrate, and an ITO substrate, etc.). In the present invention, the above includes the case where it is directly formed thereon and the case where it is formed through other layers. For example, a planarization film or a resist underlayer film may also be formed directly on the substrate, and the composition of the present invention may be directly applied thereon. As a resist underlayer film, a BARC layer may be cited. The application method is not particularly limited, but for example, a method of coating using a spin coater or a coater may be cited. After coating, the film of the present invention is formed by heating. The heating may be performed, for example, by a heating plate. The heating temperature is preferably 100 to 250°C; more preferably 100 to 200°C; and further preferably 100 to 160°C. The temperature here is a heating atmosphere, such as the heating surface temperature of a heating plate. The heating time is preferably 30 to 300 seconds; more preferably 30 to 120 seconds; and further preferably 45 to 90 seconds. The heating is preferably performed in the atmosphere or in a nitrogen atmosphere.
[0223] The resist film formed by the present invention has a high transmittance. When the film thickness is set to 5 μm, the transmittance at a wavelength of 248 nm is preferably 15 to 50%; more preferably 17 to 40%. With such a transmittance, even if the film thickness is thick, the exposure light reaches the lower part of the film, and a highly rectangular resist pattern can be formed.
[0224] The resist film can be exposed through a specified mask. The wavelength of the light used for exposure is not particularly limited, but it is preferably exposed with light having a wavelength of 13.5 to 248 nm. Specifically, KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), and extreme ultraviolet light (wavelength 13.5 nm) can be used, preferably KrF excimer laser. These wavelengths allow a range of ±1%. After exposure, post-exposure heating (PEB) can be performed as needed. The temperature of PEB is preferably 80 to 160°C; more preferably 100 to 150°C, and the heating time is 0.3 to 5 minutes; preferably 0.5 to 2 minutes.
[0225] For the resist film after exposure, a developer can be used for development. As a developing method, a method previously used in the development of photoresists such as a spinning immersion developing method, an immersion developing method, and a shaking immersion developing method can be used. In addition, as a developer, an aqueous solution containing inorganic bases such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, organic amines such as ammonia, ethylamine, propylamine, diethylamine, diethylaminoethanol, triethylamine, and quaternary amines such as tetramethylammonium hydroxide (TMAH) is used, preferably a 2.38 mass % TMAH aqueous solution. A surfactant may also be further added to the developer. The temperature of the developer is preferably 5 to 50°C; more preferably 25 to 40°C, and the developing time is preferably 10 to 300 seconds; more preferably 30 to 60 seconds. After display, water washing or rinsing treatment may also be performed as needed. When a positive resist composition is used, the exposed portion is removed by development to form a resist pattern. The resist pattern may also be further refined by using, for example, a shrinking material.
[0226] When the composition of the present invention is used, a resist pattern having a high resolution (ie, a high aspect ratio) despite being a thick film can be formed. When the thickness of the resist film is set to 3 μm, the resolution is preferably 150 to 220 nm, and more preferably 160 to 200 nm.
[0227] When the composition of the present invention is used, a highly rectangular resist pattern can be formed. When the composition of the present invention is a positive resist pattern forming composition, if the width of the top of the resist pattern is set to Wt and the width of the bottom is set to Wb, Wt / Wb (hereinafter sometimes referred to as Pr) is preferably 0.6 to 1.7; more preferably 0.7 to 1.0; and further preferably 0.8 to 1.0.
[0228] The conditions for comparing these values are preferably the same as those in the examples described below. For example, a film with a thickness of 3.0 μm and a groove pattern with a line width of 0.8 μm and a gap width of 0.2 μm are preferably formed for comparison.
[0229] The formed resist pattern has high heat resistance. If the formed groove pattern with a film thickness of 3 μm, a line width of 0.8 μm, and a gap width of 0.2 μm is heated at 50°C for 60 seconds, the line width change at the top of the pattern before and after heating is preferably less than 50 nm, and more preferably less than 35 nm.
[0230] The processed substrate can be formed by using the formed resist pattern as a mask to perform ion implantation, or by using the formed resist pattern as a mask to process the lower layer of the resist pattern to form a lower layer pattern, and then using the lower layer pattern as a mask to perform ion implantation.
[0231] Ion implantation can be performed using a known ion implantation device and a known method. In the manufacture of semiconductor devices, liquid crystal display devices, etc., an impurity diffusion layer is formed on the surface of the substrate. The formation of the impurity diffusion layer is usually carried out in two stages: the introduction and diffusion of impurities. As one of the methods of introduction, there is ion implantation in which impurities such as phosphorus and boron are ionized in a vacuum and accelerated with a high electric field to be injected into the surface of the support. As the ion acceleration energy during ion implantation, there is usually a situation in which an energy load of 10 to 200 keV is applied to the resist pattern, and the resist pattern is destroyed.
[0232] The resist pattern formed by the present invention is a thick film, has high rectangularity and high heat resistance, and therefore can be suitably used for ion implantation applications in which ions are implanted at high energy.
[0233] Examples of the ion source (impurity element) include ions of boron, phosphorus, arsenic, argon, etc. Examples of the thin film on the substrate include silicon, silicon dioxide, silicon nitride, aluminum, and the like.
[0234] After that, further processing such as forming wiring on the processed substrate can be implemented as needed to form a device. These further processing can be applied to known methods. As the device, semiconductor devices, liquid crystal display devices, organic EL display devices, plasma display devices, solar cell devices can be listed. The device is preferably a semiconductor device.
[0235] [Example]
[0236] The present invention is described below by way of various examples. It should be noted that the present invention is not limited to these examples.
[0237] Preparation of Composition 1
[0238] 100 parts by mass of polymer 1, 1.00 parts by mass of photoacid generator 1, 0.15 parts by mass of base compound 1, and 0.06 parts by mass of surfactant 1 were added to a mixed solvent having a mass ratio of PGME:EL=70:30 in such a manner that the solid content ratio was 25.0% by mass. The mixture was stirred at room temperature for 30 minutes. The added material was visually confirmed to be dissolved. The mixture was filtered through a 0.05 μm filter. Composition 1 was thus obtained.
[0239]
[0240] (Polymer 1) Hydroxystyrene: styrene: tert-butyl acrylate copolymer, in a molar ratio of 6:2:2, Mw about 9,0000
[0241] The above ratio represents the ratio of the number of structural units of each repeating unit, and the same shall apply hereinafter.
[0242]
[0243] (Photoacid generator 1)
[0244] Base compound 1: tris[2-(2-methoxyethoxy)ethyl]amine
[0245] Surfactant 1: Megaface R-40, DIC Corporation
[0246] Preparation of Compositions 2 to 11 and Comparative Composition 1
[0247] The components were changed as described in Table 1, and the same solvent and solid content ratio as those of Composition 1 were used to obtain Compositions 2 to 11 and Comparative Composition 1 in the same manner as Composition 1. In the table, the numerical value of each component represents parts by mass.
[0248] [Table 1]
[0249]
[0250] In the table,
[0251] Polymer 2
[0252]
[0253] Hydroxystyrene: styrene: tert-butyl acrylate copolymer, in a molar ratio of 6:2:2, Mw about 12,000
[0254] Polymer 3
[0255]
[0256] Hydroxystyrene: styrene: tert-butyl acrylate copolymer, in a molar ratio of 6:2:2, Mw about 15,000
[0257] Polymer 4
[0258]
[0259] Hydroxystyrene: styrene: tert-butyl acrylate copolymer, in a molar ratio of 6:2:2, Mw about 18,000
[0260] Polymer 5 (Comparative polymer)
[0261]
[0262] Hydroxystyrene: styrene: tert-butyl acrylate copolymer, in a molar ratio of 6:2:2, Mw about 24,000
[0263] Polymer 6
[0264]
[0265] Hydroxystyrene: styrene: ethyl cyclopentyl acrylate copolymer, in a molar ratio of 6:2:2, Mw about 12,000
[0266] Polymer 7
[0267]
[0268] Hydroxystyrene: cyclohexyl acrylate: tert-butyl acrylate copolymer, in a molar ratio of 6:2:2, Mw about 12,000
[0269] Polymer 8
[0270]
[0271] Hydroxystyrene: styrene: tert-butyl acrylate copolymer, in a molar ratio of 6:1:3, Mw about 12,000
[0272] Polymer 9
[0273]
[0274] Anthracene methyl methacrylate: acetoacetoxyethyl methacrylate: 2-hydroxypropyl methacrylate: tert-butyl methacrylate copolymer, in a molar ratio of 1:1:0.3:0.5, Mw about 15,000
[0275] Photoacid generator 2
[0276]
[0277] Example of resist pattern formation
[0278] The composition prepared above was dropped onto an 8-inch Si wafer using a coating developer Mark 8 (Tokyo Electron) and spin-coated. The wafer was heated at 140°C for 90 seconds using a hot plate under atmospheric conditions to form a resist film. The thickness of the resist film at this time point was measured using an optical interference film thickness measuring device M-1210 (SCREEN) and was 3.0 μm.
[0279] The resist film was exposed using a KrF stepper FPA3000-EX5 (Canon). The exposed wafer was heated (PEB) at 120°C for 90 seconds using a hot plate under atmospheric conditions. Thereafter, the resist film was spin-developed with a 2.38 mass % TMAH aqueous solution for 60 seconds, washed with DIW, and spin-dried at 1,000 rpm. Thus, a groove pattern with a line width of 0.8 μm and a gap width of 0.2 μm was formed. The line width and gap width are measured at the bottom of the pattern.
[0280] Figure 1 The vertical cross-sectional shape of the pattern is schematically shown. A groove pattern 2 is formed on a substrate 1. The exposure amount for forming a groove pattern with a line width of 0.8 μm and a gap width of 0.2 μm is defined as an optimal exposure amount, and the resolution described later is evaluated at this optimal exposure amount.
[0281] Evaluation of the rectangularity of the pattern
[0282] A slice of the sample prepared in the above-mentioned "Example of Forming a Resist Pattern" was prepared, and the vertical cross section of the pattern was observed using a scanning electron microscope (SEM). The ratio of the width of the top of the pattern to the width of the bottom of the pattern was evaluated. Figure 2 The vertical cross section is schematically shown, and the groove pattern 2 is formed on the substrate 1. The width of the top of the pattern is Wt, and the width of the bottom of the pattern is Wb. This ratio Pr is defined as Pr=Wt / Wb, which is used as an index for evaluating the rectangularity of the pattern.
[0283] The evaluation criteria are as follows.
[0284] A: Pr is 0.8 to 1.0
[0285] B: Pr is 0.7 to 0.8
[0286] C: Pr is 1.0 or more or 0.7 or less
[0287] The evaluation results are shown in Table 2.
[0288] Resolution Evaluation
[0289] Using a mask pattern with a gap size of 0.25 to 0.16 μm, the above-mentioned pattern forming method was used to expose at the optimal exposure amount. The minimum size (μm) of the resist pattern resolved when exposed at the optimal exposure amount was taken as the resolution. For those where a 0.20 μm pattern could not be formed, the minimum size that could be formed was taken as the resolution.
[0290] The evaluation results are shown in Table 2.
[0291] Transmittance Evaluation
[0292] Each composition was dropped onto a quartz substrate and spin-coated. The wafer was heated at 140°C for 90 seconds using a hot plate under atmospheric conditions to form a resist film with a film thickness of 5.0 μm. The transmission spectrum of the film was measured using an ultraviolet-visible spectrometer (ThermoFisher Scientific). The transmittance at 248 nm was used as the transmittance for evaluation. The control was a quartz substrate without a resist film.
[0293] Evaluation of heat resistance
[0294] The substrate on which the pattern was formed in the above-mentioned "Example of Forming a Resist Pattern" was heated at 150° C. for 60 seconds using a hot plate. Thereafter, changes in the pattern shape were observed from a vertical cross section using a SEM. The evaluation criteria were as follows.
[0295] A: No change in shape has been confirmed
[0296] B: There is a change at the top of the resist pattern, and the amount of deformation is 50 nm or less.
[0297] C: The deformation amount of the top of the resist pattern is larger than 50 nm.
[0298] [Table 2]
[0299]
[0300] Evaluation of Composition 11
[0301] Using composition 11, the following evaluations were performed.
[0302] When the resolution was evaluated in the same manner as above, the resolution was 180 nm, which was evaluated as A. When the heat resistance was evaluated in the same manner as above, the deformation amount was 0 nm, which was evaluated as A.
[0303] Description of Reference Numerals
[0304] 1: Substrate
[0305] 2: Groove pattern.
Claims
1. An ion implantation thick film resist composition comprising a polymer (A), a photoacid generator (B) and a solvent (C), wherein: The film thickness of the resist film formed by the composition is 1.0 to 50 μm; The mass average molecular weight of polymer (A) is 5,000 to 19,000; and The polymer (A) comprises at least one of the repeating units represented by formula (A-1), (A-2), (A-3) and (A-4); in, R 11 , R 21 , R 41 and R 45 Each is independent of C 1-5 Alkyl, wherein the methylene group in the alkyl may be replaced by an oxy group; R 12 , R 13 , R 14 , R 22 , R 23 , R 24 , R 32 , R 33 , R 34 , R 42 , R 43 , and R 44 are independently hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, or -COOH; p11 is 0 to 4, p15 is 1 to 2, p11+p15≤5, p21 is 0 to 5, p41 is 0-4, p45 is 1-2, p41+p45≤5; P 31 C 4-20 Alkyl groups, wherein a part or all of the alkyl groups may form a ring, a part or all of the H groups in the alkyl groups may be substituted by halogen, and the methylene groups in the alkyl groups may be replaced by oxy groups or carbonyl groups.
2. The composition according to claim 1, wherein When the thickness of the resist film is 5 μm, the transmittance at a wavelength of 248 nm is 15 to 50%.
3. The composition according to claim 1 or 2, wherein The number of repeating units (A-1), (A-2), (A-3) and (A-4) in the polymer (A) is n A-1 、n A-2 、n A-3 , and n A-4 satisfy: n A-1 / (n A-1 +n A-2 +n A-3 +n A-4 )=40~80%、 n A-2 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~40%、 n A-3 / (n A-1 +n A-2 +n A-3 +n A-4 ) = 10-50%, or n A-4 / (n A-1 +n A-2 +n A-3 +n A-4 )=0~40%; It is preferred that the total number of all repeating units contained in the polymer (A) be n total When (n A-1 +n A-2 +n A-3 +n A-4 ) / n total =80~100%。 4. A composition according to one or more of claims 1 to 3, wherein When the film thickness of the resist film is set to 3 μm, the resolution is 150 to 220 nm.
5. A composition according to one or more of claims 1 to 4, wherein If a groove pattern with a film thickness of 3 μm, a line width of 0.8 μm, and a gap width of 0.2 μm formed by the resist film is heated at 50°C for 60 seconds, the line width change at the top of the pattern before and after heating is less than 50 nm, and if the width of the top of the groove pattern is Wt and the width of the bottom of the pattern is Wb, then 0.6≤Wt / Wb≤1.7 is satisfied.
6. A composition according to one or more of claims 1 to 5, wherein The photoacid generator (B) is represented by formula (B-1): B n+ Cation B n- Anion (B-1) in, B n+ The cation is a cation represented by formula (BC1), a cation represented by formula (BC2), or a cation represented by formula (BC3), and B n+ The cation is generally n-valent, where n is 1 to 3. B n- The anion is an anion represented by formula (BA1), an anion represented by formula (BA2), an anion represented by formula (BA3), or an anion represented by formula (BA4), and B n- Anions are generally n-valent; in, R b1 Each is independent of C 1-6 Alkyl, C 1-6 Alkoxy, C 6-12 Aryl, C 6-12 Arylthio, or C 6-12 aryloxy, nb1 is independently 0, 1, 2, or 3; in, R b2 Each is independent of C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 Aryl, nb2 is independently 0, 1, 2 or 3; in, R b3 are independently hydroxyl, C 1-6 Alkyl, C 1-6 Alkoxy, or C 6-12 Aryl, R b4 Each is independent of C 1-6 Alkyl, but 2 R b4 They can also bond to each other to form a ring structure. nb3 is independently 0, 1, 2 or 3; Among them, R b5 Each is independent of C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, or C 1-6 alkyl; Among them, R b6 C 1-10 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, C 6-12 Fluorine-substituted aryl, C 2-12 Fluorine-substituted acyl, or C 6-12 Fluorine-substituted alkoxyaryl; in, R b7 Each is independent of C 1-6 Fluorine-substituted alkyl, C 1-6 Fluorine-substituted alkoxy, C 6-12 Fluorine-substituted aryl, C 2-12 Fluorine-substituted acyl, or C 6-12 Fluorine-substituted alkoxyaryl, wherein 2 R b7 They can also bond to each other to form a heterocyclic structure substituted by fluorine; in, R b8 For hydrogen, C 1-6 Alkyl, C 1-6 Alkoxy or hydroxyl, L b is methylene, ethylene, carbonyl, oxy or carbonyloxy, Y b are independently hydrogen or fluorine, nb4 is an integer from 0 to 10, and nb5 is an integer from 0 to 21.
7. A composition according to one or more of claims 1 to 6, wherein The solvent (C) is propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, n-butyl acetate, n-butyl ether, 2-heptanone, cyclohexanone, or any combination thereof.
8. A composition according to one or more of claims 1 to 7, wherein further comprising a base compound (D); Preferably the basic compound (D) is ammonia, C 1-16 Aliphatic primary amine compounds, C 2-32 Aliphatic secondary amine compounds, C 3-48 Aliphatic tertiary amine compounds, C 6-30 Aromatic amine compounds, C 5-30 Heterocyclic amine compounds, or any combination thereof; or The content of the basic compound (D) is preferably 0.01 to 5 parts by mass based on 100 parts by mass of the polymer (A).
9. A composition according to one or more of claims 1 to 8, wherein further comprising a surfactant (E); The content of the surfactant (E) is preferably 0.005 to 1 part by mass based on 100 parts by mass of the polymer (A).
10. The composition according to one or more of claims 1 to 9, wherein further comprising a dye (F); The content of the dye (F) is preferably 0 to 0.5 parts by mass based on 100 parts by mass of the polymer (A).
11. A composition according to one or more of claims 1 to 10, wherein further comprising an additive (G); The additive (G) is preferably a surface smoothing agent, a plasticizer, a contrast enhancer, an acid, a free radical generator, a substrate adhesion enhancer, a defoaming agent, or any combination thereof, or The content of the additive (G) is preferably 0 to 5 parts by mass based on 100 parts by mass of the polymer (A).
12. A composition according to one or more of claims 1 to 11, wherein The polymer (A) contains further repeating units other than the repeating units represented by formulae (A-1) to (A-4); Preferably, the content of the further repeating unit contained in the polymer (A) is 0 to 10 parts by mass based on 100 parts by mass of the polymer (A); or Preferably the further repeating unit comprises an arylcarbonyl group.
13. A composition according to one or more of claims 1 to 12, wherein The content of salicylic acid is 0 to 0.005 parts by mass based on 100 parts by mass of the polymer (A).
14. A composition according to one or more of claims 1 to 13, wherein The content of the polymer (A) is 10 to 40% by mass based on the composition. The content of the photoacid generator (B) is 0.3 to 4 parts by mass, preferably 0.4 to 2 parts by mass, based on 100 parts by mass of the polymer (A). The content of the solvent (C) is 50 to 90% by mass based on the composition.
15. A method for manufacturing a processed substrate, comprising the steps of: Using the composition according to one or more of claims 1 to 14 to produce a resist pattern; and Ion implantation is performed using the resist pattern as a mask, or The lower layer of the resist pattern is processed using the resist pattern as a mask to form a lower layer pattern, and ion implantation is performed using the lower layer pattern as a mask.
16. A method for manufacturing a device, comprising the method according to claim 15; preferably further comprising forming wiring on the processed substrate.