Method for improving creep age forming performance of aluminum-lithium alloy component under assistance of electric pulse
In the aluminum-lithium alloy creep aging forming process, two-stage pulse current assist technology is used, combined with a hot autoclave and an electric pulse generating device, to adjust the angle between the current direction and the rolling direction, thereby solving the problem of low forming efficiency and creep of aluminum-lithium alloys. The problem of insufficient variable variables is eliminated, and efficient aluminum-lithium alloy component forming and good mechanical properties are achieved.
Patent Information
- Application Number
- CN202410978536.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The existing creep aging forming process of aluminum-lithium alloys has the problems of low forming efficiency and insufficient creep variables. Moreover, the laser shock method is costly and complex, and the subsequent forming deformation resistance of the heat treatment method is large, resulting in a decrease in forming accuracy.
Two-stage pulse current is used to assist the creep aging forming of aluminum-lithium alloy sheets. The direction of the pulse current has a certain angle with the rolling direction (30°≤θ≤60°). The creep aging is controlled by a hot autoclave and an electric pulse generating device. Forming is divided into one-stage and three-stage creep aging forming stages, and pulse current is applied to improve creep deformation and mechanical properties.
It significantly improves the creep deformation and forming efficiency of aluminum-lithium alloy components, reduces processing costs, avoids buckling instability caused by deformation resistance, and ensures good elongation and mechanical properties.
Smart Images

Figure CN118832048A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal component forming, and in particular relates to a method for improving the creep aging forming performance of an aluminum-lithium alloy component with the assistance of electric pulses. Background Art
[0002] Complex thin-walled components of aluminum-lithium alloys are widely used in aviation, aerospace, high-speed rail, automobile and other fields. Their precise forming is extremely important for subsequent equipment parts assembly, aerodynamic shape and service performance.
[0003] The existing technology mainly uses aluminum-lithium alloy rolled plates as raw materials to form aluminum-lithium alloy components through creep aging forming process. The creep aging forming process is an advanced sheet metal processing technology that utilizes metal creep, stress relaxation and aging strengthening characteristics, and is suitable for high-performance and precise forming of complex metal components. It mainly includes three stages: component loading bending, creep aging, and unloading springback. Specifically: the sheet is fixed on the mold surface of the forming mold, and the sheet is heated by the heating system of the autoclave, so that the sheet is kept at the creep aging temperature for a certain period of time to complete the creep aging forming. This method mainly has the problems of low forming efficiency and low creep amount.
[0004] To solve this technical problem, CN117025937A: This invention discloses a laser impact method for improving the collaborative manufacturing capability of creep deformation of thin-walled aluminum-lithium alloy, including solid solution of aluminum-lithium alloy plate, water quenching, and aging; with the intersection of the maximum transverse and longitudinal dimensions of the plate as the center of the circle, the area with a radius of 10-20cm is marked as the part with the largest creep amount required by the component; the marked part is cleaned, and then the constraint layer and energy absorption layer are arranged, and then laser impact is performed on it; the plate is cold rolled, and then the non-laser impact side is thinned to obtain an aluminum-lithium alloy plate of target thickness; the aluminum-lithium alloy plate is wire cut according to the unfolded diagram of the forming target profile to obtain the final aluminum-lithium alloy plate to be formed; the aluminum-lithium alloy plate to be formed is arranged on the forming mold, and then creep aging is performed. The present invention effectively improves the local creep amount of thin-walled aluminum-lithium alloy components through local laser impact, and at the same time improves the local toughness, inhibits the appearance and expansion of cracks, and prevents cracking. Due to the high cost of the laser impact equipment itself, the experimental process also requires a high experimental protection cost, and the entire experimental process is relatively complicated.
[0005] CN112981284A: This invention relates to a method for preparing a stress-aged high-strength aluminum-lithium alloy, and belongs to the technical field of aluminum-lithium alloy heat treatment. First, the aluminum-lithium alloy prepared by a conventional method is solution treated at 500℃~530℃ for 0.5h~5h, then subjected to 4%~10% tensile deformation along the rolling direction, and finally aged for 7h~14h at 155℃~225℃ and 160MPa~220MPa, and then air-cooled to obtain a stress-aged high-strength aluminum-lithium alloy. The method of the present invention controls the pre-deformation amount, the stress field and the temperature field distribution during the heat treatment, thereby achieving a comprehensive regulation of the type, quantity and size distribution of the precipitated phase in the aluminum-lithium alloy to achieve the optimal value, thereby greatly improving the yield strength and elongation of the aluminum-lithium alloy, and the method effectively shortens the heat treatment time of the aluminum-lithium alloy, thereby effectively improving the production efficiency and saving energy consumption. This invention only improves the performance. After the forming is first performed, the deformation resistance of the subsequent forming is large, which is not conducive to forming.
[0006] CN106917058B: A room temperature forming method for 2198 aluminum-lithium alloy sheet. The method comprises the following steps: 1) solution treatment, placing the sheet in a heating furnace and controlling the heat preservation time; 2) quenching treatment, quickly transferring the sheet after solution treatment to low-temperature water, strictly controlling the transfer time to ensure that the entire sheet is quenched; 3) room temperature forming, quickly taking the sheet out of the water, and completing the leveling and forming of the sheet in a short time; 4) natural aging, standing for 3 to 9 days; 5) artificial aging, placing the parts in a heating furnace and keeping them warm for a certain period of time; 6) taking out the parts for trimming and surface treatment to obtain 2198 aluminum-lithium alloy sheet parts. The present invention performs room temperature forming on the 2198 aluminum-lithium alloy sheet before aging treatment, combines plastic forming with the necessary pre-deformation before aging, avoids the difficulty of poor plasticity of the 2198 aluminum-lithium alloy, increases the strength of the parts, effectively reduces the processing cost, improves the geometric accuracy of the parts, and has the potential for large-scale industrial production. This method will inevitably produce large residual stress during the room temperature forming process in the third step. The residual stress will be released during the subsequent natural aging and artificial aging processes. The residual stress release process will inevitably lead to a significant decrease in the initial forming accuracy of the material. Summary of the invention
[0007] The purpose of the present invention is to assist the creep aging forming of aluminum-lithium alloy sheets by two-stage pulse current, and the current direction of the pulse current has a certain angle θ (30°≤θ≤60°) with the rolling direction of the aluminum-lithium alloy sheets, so as to increase the creep amount of the aluminum-lithium alloy sheets and ensure better mechanical properties, thereby promoting better shape-property coordinated manufacturing of aluminum-lithium alloy components.
[0008] To achieve the above-mentioned object, the present invention provides a method for improving the creep aging forming performance of an aluminum-lithium alloy component by electric pulse assistance. The method controls a workpiece to be formed to perform creep aging forming according to a preset process through an autoclave and an electric pulse generator. The workpiece to be formed comprises an aluminum-lithium alloy sheet, and a plurality of first electrodes and a plurality of second electrodes respectively installed at opposite ends of the aluminum-lithium alloy sheet. The aluminum-lithium alloy sheet is a rolled sheet, and the plurality of first electrodes and the plurality of second electrodes are evenly distributed, and the plurality of first electrodes and the plurality of second electrodes are respectively connected to the positive electrode and the negative electrode of the electric pulse generator. The angle between the current direction of the pulse current applied by the electric pulse generator and the rolling direction of the aluminum-lithium alloy sheet is θ, and 30°≤θ≤60°, wherein the preset process comprises:
[0009] At room temperature, by evacuating the sealed cavity between the workpiece to be formed and the mold panel of the forming mold, the component to be formed is moved closer to the mold panel and the edge of the component to be formed is in contact with the mold panel;
[0010] Starting the heating system of the autoclave to heat the workpiece to be formed to a preset target temperature and then keeping it warm;
[0011] Starting the pressurizing system of the autoclave to load the component to be formed, so that the workpiece to be formed completely fits the mold panel, and maintaining the pressure;
[0012] While starting the pressurization system of the autoclave, the electric pulse generator is turned on to apply a primary pulse current, and the electric pulse generator is kept powered on for a first preset time, so that the workpiece to be formed undergoes primary creep aging forming, wherein the first preset time is 0.75 to 1.25 hours;
[0013] At the end of the first preset time, the electric pulse generating device is turned off, and the heating system and the pressurizing system of the autoclave are used to keep the workpiece to be formed at a temperature and pressure for a second preset time, so that the workpiece to be formed undergoes secondary creep aging forming;
[0014] At the end of the second preset time, the electric pulse generator is turned on to apply a secondary pulse current, and the electric pulse generator is kept powered on for a third preset time, so that the workpiece to be formed undergoes three-level creep aging forming, wherein the third preset time is 0.75 to 1.25 hours;
[0015] At the end of the third preset time, the autoclave and the electric pulse generator are closed to unload and rebound the workpiece to be formed, thereby obtaining the aluminum-lithium alloy component.
[0016] In a specific embodiment, θ is 45°.
[0017] In a specific implementation manner, the first preset duration is the same as the third preset duration.
[0018] In a specific implementation, the first preset duration and the third preset duration are both 1 hour.
[0019] In a specific implementation manner, the sum of the first preset time length, the second preset time length and the third preset time length is 10 to 20 hours.
[0020] In a specific embodiment, the target temperature is 160-180°C.
[0021] In a specific embodiment, the electric pulse parameters of the primary pulse current include: a pulse frequency of 250-350 Hz, a pulse current density of 8-15 A / mm 2 , the duty cycle is 15-25%; the electric pulse parameters of the secondary pulse current include: pulse frequency is 250-350Hz, pulse current density is 8-15A / mm 2 , with a duty cycle of 15-25%.
[0022] In a specific embodiment, the electric pulse parameters of the primary pulse current are the same as the electric pulse parameters of the secondary pulse current.
[0023] In a specific embodiment, the maximum temperature of the primary creep aging forming and the maximum temperature of the tertiary creep aging forming are both lower than the maximum creep aging temperature corresponding to the aluminum-lithium alloy material.
[0024] In a specific embodiment, the aluminum-lithium alloy component is a melon-shaped component or a thin-walled metal component.
[0025] The beneficial effects of the present invention include at least:
[0026] 1. The method provided by the present invention for improving the creep aging forming performance of aluminum-lithium alloy components with electric pulse assistance, controls the components to be formed to perform creep aging forming according to a preset process through a hot autoclave and an electric pulse generator, wherein the preset process improves the conventional creep aging forming process, and applies a pulse current through the electric pulse generator to assist the creep aging forming of the aluminum-lithium alloy sheet during the first preset time of the initial creep aging and the third preset time of the final creep aging. The creep strain experimental data show that the greater the angle θ between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet, the greater the creep strain. However, the creep amount of the primary / tertiary creep aging deformation corresponding to θ of 90° is relative to the primary / tertiary creep aging deformation corresponding to θ of 45°. The creep amount of θ is not improved much, while the creep amount of the primary / tertiary creep aging deformation corresponding to θ of 45° is improved more than the creep amount of the primary / tertiary creep aging deformation corresponding to θ of 0°, that is, with the increase of the angle θ, the increase of the creep amount decreases; at the same time, the mechanical property data show that the mechanical properties corresponding to θ of 90° are poor, while the mechanical properties corresponding to θ of 45° are slightly worse than those corresponding to θ of 0°, that is, the elongation is slightly worse, but a small loss of elongation can obtain a larger deformation; in this way, the current direction of the pulse current has a certain angle θ (30°≤θ≤60°) with the rolling direction of the aluminum-lithium alloy sheet, and better mechanical properties are obtained while obtaining a larger deformation than θ of 0°.
[0027] 2. The creep aging forming provided by the present invention is divided into three stages, and pulse current is applied in the first stage (the first-level creep aging duration is 0.75h~1.25h) and the third stage (the third-level creep aging duration is 0.75h~1.25h) to assist the autoclave creep aging forming. On the one hand, the electron wind force of the pulse current increases the atomic diffusion capacity, reduces the dislocation movement resistance, and reduces the barrier difference between the deformation activation energy and the precipitation activation energy, so that the aging precipitation process is accelerated and the nucleation rate of the precipitated phase is increased, so that the creep amount and forming efficiency of the aluminum-lithium alloy are greatly improved; on the other hand, two pulse current assisted forming will obtain two opportunities to increase the creep deformation, and because the pulse current is applied for a period of time at the beginning and the end of the creep aging, a good elongation can also be guaranteed.
[0028] 3. The preset process of creep aging forming of aluminum-lithium alloy components provided by the present invention is to pass a pulse current while loading and bending. On the one hand, the non-thermal effect of the electric pulse can reduce the flow stress of the aluminum-lithium alloy, making it easier for the component to be formed to fit the mold panel; on the other hand, the electroplastic effect of the pulse current can effectively avoid the occurrence of buckling instability caused by the large deformation resistance.
[0029] Fourth, the secondary pulse current assists the creep aging forming process, which accelerates the aging precipitation process, increases the nucleation rate of the precipitate phase, improves the forming efficiency, and can reduce the processing cost.
[0030] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of a structure in which a component to be formed is installed on a forming mold according to an embodiment of the present invention;
[0032] Figure 2 A flow chart of the steps of the preset process in the method for improving the creep aging forming performance of aluminum-lithium alloy components with electric pulse assistance provided by the present invention;
[0033] Figure 3 Creep strain diagrams of conventional creep aging process and electric pulse assisted creep aging process provided by Example 1 of the present invention;
[0034] Figure 4 The creep strain diagram corresponding to the angles of 0°, 45° and 90° between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet;
[0035] Figure 5 The temperature curve of the component to be formed in the first hour of power-on when the angles between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet are 0°, 45° and 90°;
[0036] Figure 6 The angles between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet are 0°, 45° and 90°, and the tensile curve corresponding to the conventional creep aging process. DETAILED DESCRIPTION
[0037] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. However, the present invention can be defined and covered by various different implementations according to the claims.
[0038] See also Figure 1 and Figure 2The present invention provides a creep aging forming method for an aluminum-lithium alloy component. The forming method controls a component 200 to be formed to perform creep aging forming according to a preset process through an autoclave and an electric pulse generator. The component 200 to be formed includes an aluminum-lithium alloy sheet 210, and a plurality of first electrodes 220 and a plurality of second electrodes 230 respectively installed at opposite ends of the aluminum-lithium alloy sheet 210. The plurality of first electrodes 220 and the plurality of second electrodes 230 are evenly distributed, and the plurality of first electrodes 220 and the plurality of second electrodes 230 are respectively connected to the positive electrode and the negative electrode of the electric pulse generator.
[0039] When the plurality of first electrodes 220 are positive electrodes, the plurality of second electrodes 230 are negative electrodes; when the plurality of first electrodes 220 are negative electrodes, the plurality of second electrodes 230 are positive electrodes.
[0040] It can be understood that the number of the first electrodes and the number of the second electrodes are the same.
[0041] In the present invention, the plurality of first electrodes 220 and the plurality of second electrodes 230 are copper electrodes.
[0042] In the present invention, the plurality of first electrodes 220 and the plurality of second electrodes 230 are respectively connected to the positive electrode and the negative electrode of the electric pulse generating device through a plurality of wires.
[0043] In the present invention, the aluminum-lithium alloy sheet 210 is a rectangular rolled plate, and a plurality of first electrodes 220 and a plurality of second electrodes 230 are respectively installed at both ends of the width direction of the aluminum-lithium alloy sheet 210. The angle between the current direction of the pulse current applied by the electric pulse generating device and the rolling direction of the aluminum-lithium alloy sheet 210 is θ, and 30°≤θ≤60°.
[0044] The preset process includes:
[0045] Step S10 , at room temperature, by evacuating the sealed cavity between the component to be formed 200 and the mold panel 110 of the forming mold 100 , the component to be formed 200 is moved closer to the mold panel 110 and the edge of the component to be formed 200 is attached to the mold panel 110 .
[0046] The forming mold 100 includes a support mechanism 120 and a mold-shaped panel 110 fixedly mounted on the top of the support mechanism 120. In the present invention, the forming mold 100 is a forming mold provided by the prior art, and the present invention does not make any improvements.
[0047] In the present invention, the technology of forming a sealed cavity between the component to be formed 200 and the mold panel 110 of the forming mold 100 is all prior art, and the present invention does not make any improvements. Specifically, it can be: the component to be formed 200 is completely covered with a breathable felt, at least one circle of sealant is pasted on the edge of the forming mold 100, and a vacuum bag is pasted on the sealant so that the vacuum bag and the mold panel form a sealed cavity together.
[0048] It can be understood that when the sealed cavity is formed, the plurality of first electrodes and the second electrodes all extend out of the vacuum bag to facilitate connection with the electric pulse generating device.
[0049] In step S10 , a vacuum of 0.1 MPa is drawn into the sealed cavity, and the component to be molded 200 and the mold-type panel 110 are connected.
[0050] Step S20, starting the heating system of the autoclave to heat the component to be formed to a preset target temperature and then keeping it warm.
[0051] The target temperature is associated with the creep aging forming temperature of the aluminum-lithium alloy and the pulse current generated by the electric pulse generator.
[0052] In this step, the preset target temperature is 160°C to 180°C.
[0053] Step S30, starting the pressurizing system of the autoclave to load the component to be formed, so that the component to be formed completely fits the mold panel, and maintaining the pressure.
[0054] In this step, the loading pressure is 160 MPa to 220 MPa.
[0055] Step S40, while starting the pressurization system of the autoclave, turn on the electric pulse generating device to apply a primary pulse current, and keep the electric pulse generating device powered on for a first preset time, so that the component to be formed undergoes primary creep aging forming, wherein the first preset time is 0.75 to 1.25 hours.
[0056] When loading is performed, a pulse current is passed through. On the one hand, the non-thermal effect of the electric pulse can reduce the flow stress of the aluminum-lithium alloy, making it easier for the component to be formed to fit the mold panel. On the other hand, the electroplastic effect brought about by the pulse current can effectively avoid the buckling instability caused by the large deformation resistance.
[0057] When the first preset time is less than 0.75 h, the pulse current does not significantly increase the creep strain. When the first preset time is greater than 1.25 h, such as 1.5 h, it may have an adverse effect on the formability of the component.
[0058] Preferably, the first preset duration is 1 hour.
[0059] Preferably, the maximum temperature of the primary creep aging forming is less than the corresponding maximum creep aging temperature of the aluminum-lithium alloy material.
[0060] In the present invention, the maximum creep aging temperature corresponding to the aluminum-lithium alloy material is 200°C, that is, the maximum temperature of the primary creep aging forming is less than 200°C.
[0061] Preferably, the electric pulse parameters of the primary pulse current are as follows: the pulse frequency is 250 Hz to 350 Hz, the pulse current density is 8 to 15 A / mm 2 , the duty cycle is 15~25%.
[0062] More preferably, the electric pulse parameters of the primary pulse current are as follows: the pulse frequency is 300 Hz, the pulse current density is 10 / mm 2 , the duty cycle is 20%.
[0063] The above electric pulse parameters are used to assist heating of the component to be formed, so that the maximum temperature of creep aging forming will not exceed 200° C., thereby avoiding degradation of material performance.
[0064] Step S50, turning off the electric pulse generating device at the end of the first preset time, and keeping the heating system and the pressurizing system of the autoclave working for a second preset time, so that the component to be formed undergoes secondary creep aging forming.
[0065] In the present invention, the second preset time is associated with the creep aging time corresponding to the aluminum-lithium alloy material.
[0066] Step S60, turning on the electric pulse generating device to apply a secondary pulse current at the end time of the second preset time, and keeping the electric pulse generating device powered on for a third preset time, so that the component to be formed undergoes three-level creep aging forming, wherein the third preset time is 0.75 to 1.25 hours.
[0067] Preferably, the maximum temperature of the three-stage creep aging forming is less than the maximum creep aging temperature corresponding to the aluminum-lithium alloy material.
[0068] In the present invention, the maximum creep aging temperature corresponding to the aluminum-lithium alloy material is 200°C.
[0069] Preferably, the third preset duration is the same as the first preset duration.
[0070] Passing a pulse current during the initial first preset time for primary creep aging forming can greatly increase the creep amount, but it has a certain impact on the elongation of the formed component. Passing a pulse current during the final third preset time for tertiary creep aging forming, although it has little effect on deformation (the "little effect" here refers to the amount of deformation increased by passing the pulse current during the initial first preset time), it is very helpful to improve the elongation of the formed component. Therefore, passing a pulse current during both the initial first preset time and the final third preset time can improve the defect of the deterioration of the elongation of the primary creep aging forming through the tertiary creep aging forming, so that the damage to the elongation of the final aluminum-lithium alloy component is reduced. At the same time, two opportunities to increase creep deformation are obtained, thereby increasing the total creep amount.
[0071] Preferably, the third preset duration is 1 hour.
[0072] Preferably, the sum of the first preset time length, the second preset time length and the third preset time length is 10 to 20 hours.
[0073] In the present invention, 10 to 20 hours can be understood as the total creep aging deformation time of the creep aging forming of the aluminum-lithium alloy component provided by the present invention, and this time is associated with the preset target temperature, that is, the creep aging forming temperature.
[0074] Preferably, the electric pulse parameters of the secondary pulse current are as follows: the pulse frequency is 250 Hz to 350 Hz, the pulse current density is 8 to 15 A / mm 2 , the duty cycle is 15~25%.
[0075] More preferably, the electric pulse parameters of the secondary pulse current are as follows: the pulse frequency is 300 Hz, the pulse current density is 10 A / mm 2 , the duty cycle is 20%.
[0076] By using the above electric pulse parameters to assist in heating the component to be formed, the maximum temperature of creep aging forming will not exceed 200° C., thus avoiding degradation of material performance.
[0077] In the present invention, during the entire creep aging deformation process, the heating system of the autoclave is always in a heat preservation state and the pressurizing system is in a pressure-maintaining state, and the pulse current is used to assist the creep aging deformation of the autoclave during the creep aging forming process. Specifically, the first-stage creep aging forming is when the autoclave and the electric pulse generator are turned on at the same time, the second-stage creep aging forming is when only the autoclave is turned on, and the third-stage creep aging forming is when the autoclave and the electric pulse generator are turned on at the same time.
[0078] In the present invention, the total creep aging forming is divided into three stages. Pulse current is used to assist the forming in the first and third stages, which provides two opportunities to improve creep deformation without affecting the mechanical properties of the aluminum-lithium alloy component. If the entire creep aging forming is performed with pulse current to assist the creep aging forming, although the creep amount can be increased, the mechanical properties of the aluminum-lithium alloy component formed in the end are quite poor. Therefore, the present invention needs to control the application time of the pulse current in the first and third stages to ensure the mechanical properties while increasing the creep amount.
[0079] Step S70, closing the autoclave and the electric pulse generating device at the end of the third preset time period, so that the component to be formed is unloaded and rebounded to obtain the aluminum-lithium alloy component.
[0080] Preferably, the aluminum-lithium alloy component is a thin-walled metal component.
[0081] Example 1
[0082] Please refer to Figures 1 to 6 , the aluminum-lithium alloy component creep aging forming method provided by the present invention is used to form thin-walled metal components.
[0083] The specific steps include:
[0084] Step 1: Provide an aluminum-lithium alloy sheet 210, and install a plurality of first electrodes 220 and a plurality of second electrodes 230 at both ends of the aluminum-lithium alloy sheet 210 to form a component 200 to be formed, wherein the aluminum-lithium alloy sheet 210 is a rectangular rolled sheet with a rolling direction of Figure 1 In the length direction of the aluminum-lithium alloy sheet 210 shown, multiple first electrodes 220 and multiple second electrodes 230 are evenly arranged along the width direction of the aluminum-lithium alloy sheet, so that the angle θ between the current direction when current is passed through the first electrode 220 and the multiple second electrodes 230 and the rolling direction of the aluminum-lithium alloy sheet 210 is 45°.
[0085] In this embodiment, the aluminum-lithium alloy sheet is 2195 aluminum-lithium alloy.
[0086] In this embodiment, the first electrode and the second electrode are both copper electrodes.
[0087] Step 2: Provide a hot press tank, an electric pulse generating device and a plurality of wires, wherein the plurality of wires are used to connect the first electrode, the second electrode and the electric pulse generating device.
[0088] Step 3: Provide a forming mold 100, a breathable felt, a vacuum bag, a vacuum tube, and high-temperature glue, etc., wherein the forming mold includes a supporting mechanism and a mold panel fixed on the top of the supporting mechanism.
[0089] It should be noted that, in this embodiment, there is no sequential order among step one, step two and step three.
[0090] Step 4: Install the component to be formed on the mold-type panel 110, and seal the gap between the component to be formed 200 and the mold-type panel 110 to form a sealed cavity between the component to be formed and the mold-type panel.
[0091] It should be noted that sealing the component to be formed and the mold panel to form a sealed cavity is an existing technology. Breathable felt, vacuum bags, vacuum tubes and high-temperature glue are sealing materials, and the present invention has not made any improvements. It can be understood that since the first electrode and the second electrode need to be connected to the electric pulse generating device, the first electrode and the second electrode both extend out of the vacuum bag.
[0092] Step 5: Place the forming mold and the component to be formed as a whole in an autoclave, and connect the plurality of first electrodes and the plurality of second electrodes to the positive electrode and the negative electrode of the electric pulse generating device respectively through wires.
[0093] Step 6: Control the component to be formed to undergo creep aging forming according to a preset process by using the autoclave and the electric pulse generator. The preset process includes:
[0094] Step (1), at room temperature, by evacuating the sealed cavity between the component to be formed and the mold panel of the forming mold, the component to be formed is moved closer to the mold panel and the edge of the component to be formed is in contact with the mold panel.
[0095] In this step, a vacuum of 0.1 MPa is drawn into the sealed cavity to connect the component to be formed and the mold panel.
[0096] Step (2), starting the heating system of the autoclave to heat the component to be formed to a preset target temperature and then keeping it warm.
[0097] In this step, the preset target temperature is 160°C.
[0098] Step (3), starting the pressurizing system of the autoclave to load the component to be formed, so that the component to be formed completely fits the mold panel, and maintaining the pressure.
[0099] In this step, the loading pressure was 160 MPa.
[0100] Step (4), while starting the pressurization system of the autoclave, turn on the electric pulse generator to apply a primary pulse current, and keep the electric pulse generator powered on for a first preset time, so that the component to be formed undergoes primary creep aging forming, wherein the first preset time is 1 hour.
[0101] In this step, the electric pulse parameters of the primary pulse current are as follows: the pulse frequency is 300 Hz, the pulse current density is 10 A / mm 2 , the duty cycle is 20%.
[0102] By using the above electric pulse parameters to assist in heating the component to be formed, the maximum temperature of the primary creep aging forming will not exceed 200° C., thus avoiding degradation of the material's performance.
[0103] Step (5), turning off the electric pulse generating device at the end of the first preset time, and keeping the heating system and the pressurizing system of the autoclave working for a second preset time, so that the component to be formed undergoes secondary creep aging forming.
[0104] In this step, the second preset time length is 18 hours.
[0105] Step (6), turning on the electric pulse generating device to apply a secondary pulse current at the end of the second preset time, and keeping the electric pulse generating device powered on for a third preset time, so that the component to be formed undergoes three-level creep aging forming, wherein the third preset time is 1 hour.
[0106] In this step, the electric pulse parameters of the secondary pulse current are as follows: the pulse frequency is 300 Hz, the pulse current density is 10 A / mm 2 , the duty cycle is 20%.
[0107] By using the above electric pulse parameters to assist in heating the component to be formed, the maximum temperature of the three-stage creep aging forming will not exceed 200° C., thereby avoiding degradation of the material performance.
[0108] Step (7), closing the autoclave and the electric pulse generator at the end of the third preset time, allowing the component to be unloaded and rebound to obtain an aluminum-lithium alloy component.
[0109] See also Figure 3 , Figure 3 The creep strain diagrams of conventional creep aging forming and the electric pulse assisted creep aging forming provided in Example 1 of the present invention are shown in FIG. Figure 3 It can be seen that after the electric pulse is applied, the creep strain is significantly increased after the first 1 hour and the last 1 hour, respectively. Among them, the promoting effect on the creep strain in the first 1 hour is particularly obvious; and the total creep strain is also significantly greater than the total creep strain of conventional creep aging.
[0110] See also Figure 4 , Figure 4 The creep strain diagram corresponding to the angles of 0°, 45° and 90° between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet is shown in Figure 2. Figure 4It can be seen that the greater the angle θ between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet, the greater the creep strain. However, the creep amount of the primary / tertiary creep aging deformation corresponding to θ of 90° is not much higher than that of the primary / tertiary creep aging deformation corresponding to θ of 45°, while the creep amount of the primary / tertiary creep aging deformation corresponding to θ of 45° is much higher than that of the primary / tertiary creep aging deformation corresponding to θ of 0°, that is, as the angle increases, the increase in the creep amount decreases.
[0111] See also Figure 5 , Figure 5 The temperature curve of the component to be formed in the first hour of power-on when the angles of the pulse current direction and the rolling direction of the aluminum-lithium alloy sheet are 0°, 45° and 90°. Figure 5 It can be seen that the temperatures of θ 0° and θ 45° are similar, but the temperature of θ 90° increases more, which means that under the same pulse current parameters, the more crystal defects are encountered when flowing through the 90-degree direction, the more obvious the local Joule heating effect is. Figure 4 It is known that although the temperature change when θ is 45° is not obvious compared with the temperature change when θ is 0°, the creep amount of the corresponding primary / tertiary creep aging deformation increases significantly.
[0112] See also Figure 6 , Figure 6 The angles between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet are 0°, 45° and 90°, and the tensile curve corresponding to the conventional creep aging process. Figure 6 It can be seen that the mechanical properties corresponding to θ of 0° are basically the same as those corresponding to the conventional creep aging process, the mechanical properties corresponding to θ of 90° are poor, and the mechanical properties corresponding to θ of 45° are slightly worse than those corresponding to θ of 0°, that is, the elongation is slightly worse. It should be noted that in the present invention, the mechanical properties of different angles are judged to be good or bad based on the mechanical properties of the conventional creep aging process.
[0113] Combination Figures 4 to 6It is known that although the creep amount of the primary / tertiary creep aging deformation corresponding to θ of 90° is the largest, its mechanical properties are very poor, while the creep amount of the primary / tertiary creep aging deformation corresponding to θ of 45° is much higher than that of the primary / tertiary creep aging deformation corresponding to θ of 0°, and the mechanical properties corresponding to θ of 45° are only slightly worse than those corresponding to θ of 0°, with a small loss of elongation, and a larger deformation can be obtained. The present invention sets the angle between the current direction of the pulse current and the rolling direction of the aluminum-lithium alloy sheet to 30° to 60°, and the increase in the creep amount of the secondary pulse current assisted aging forming relative to the creep amount of the conventional creep aging deformation is much greater than the increase in the creep amount of the secondary pulse current aging deformation relative to the creep amount of the conventional creep aging deformation when θ is 0°, and the mechanical properties are better.
[0114] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance. It is characterized in that The method controls the workpiece to be formed to perform creep aging forming according to a preset process through an autoclave and an electric pulse generator. The workpiece to be formed includes an aluminum-lithium alloy sheet, and a plurality of first electrodes and a plurality of second electrodes respectively installed at opposite ends of the aluminum-lithium alloy sheet. The aluminum-lithium alloy sheet is a rolled sheet. The plurality of first electrodes and the plurality of second electrodes are evenly distributed, and the plurality of first electrodes and the plurality of second electrodes are respectively connected to the positive electrode and the negative electrode of the electric pulse generator. The angle between the current direction of the pulse current applied by the electric pulse generator and the rolling direction of the aluminum-lithium alloy sheet is θ, and 30°≤θ≤60°. The preset process includes: At room temperature, by evacuating the sealed cavity between the workpiece to be formed and the mold panel of the forming mold, the component to be formed is moved closer to the mold panel and the edge of the component to be formed is in contact with the mold panel; Starting the heating system of the autoclave to heat the workpiece to be formed to a preset target temperature and then keeping it warm; Starting the pressurizing system of the autoclave to load the component to be formed, so that the workpiece to be formed completely fits the mold panel, and maintaining the pressure; While starting the pressurization system of the autoclave, the electric pulse generator is turned on to apply a primary pulse current, and the electric pulse generator is kept powered on for a first preset time, so that the workpiece to be formed undergoes primary creep aging forming, wherein the first preset time is 0.75 to 1.25 hours; At the end of the first preset time, the electric pulse generating device is turned off, and the heating system and the pressurizing system of the autoclave are used to keep the workpiece to be formed at a temperature and pressure for a second preset time, so that the workpiece to be formed undergoes secondary creep aging forming; At the end of the second preset time, the electric pulse generator is turned on to apply a secondary pulse current, and the electric pulse generator is kept powered on for a third preset time, so that the workpiece to be formed undergoes three-level creep aging forming, wherein the third preset time is 0.75 to 1.25 hours; At the end of the third preset time, the autoclave and the electric pulse generator are closed to unload and rebound the workpiece to be formed, thereby obtaining the aluminum-lithium alloy component.
2. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 1, It is characterized in that θ is 45°.
3. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 1, It is characterized in that The first preset time length is the same as the third preset time length.
4. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 3, It is characterized in that The first preset time length and the third preset time length are both 1 hour.
5. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 3 or 4, It is characterized in that The sum of the first preset time length, the second preset time length and the third preset time length is 10 to 20 hours.
6. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 1, It is characterized in that The target temperature is 160-180°C.
7. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 6, It is characterized in that The electric pulse parameters of the primary pulse current include: pulse frequency of 250-350 Hz, pulse current density of 8-15 A / mm 2 , the duty cycle is 15-25%; the electric pulse parameters of the secondary pulse current include: pulse frequency is 250-350Hz, pulse current density is 8-15A / mm 2 , with a duty cycle of 15-25%.
8. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 7, It is characterized in that The electric pulse parameters of the primary pulse current are the same as the electric pulse parameters of the secondary pulse current.
9. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 8, It is characterized in that The maximum temperature of the primary creep aging forming and the maximum temperature of the tertiary creep aging forming are both lower than the corresponding maximum creep aging temperature of the aluminum-lithium alloy material.
10. The method for improving creep aging forming performance of aluminum-lithium alloy components by electric pulse assistance according to claim 1, It is characterized in that The aluminum-lithium alloy component is a thin-walled metal component.
Citation Information
Patent Citations
In SITU thermal processing of a hydrocarbon containing formation via backproducing through a heater well
CA2463112A1
Method for promoting creep forming
CN109570321A
Creep age forming method adopting pulse current regression and used for alloy plate
CN112267082A
Full-process manufacturing method applied to power-assisted superplastic forming and aging treatment on aluminum-lithium alloy thin-wall components
CN113000667A
Method and device for forming thin-wall metal component through pulse current regulation and control
CN117772914A